Method for preparing nano nickel powder by using mixed solvent
By using deionized water and mixed solvent of ethylene glycol and NaOH, sodium borohydride and polyvinylpyrrolidone, the problems of uneven particle size distribution and high cost of nano nickel powder are solved, and more efficient preparation of nano nickel powder and Environmentally friendly production.
Patent Information
- Application Number
- CN202411159887.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-01
AI Technical Summary
The existing nano nickel powder preparation methods have problems of uneven particle size distribution, high cost and environmental pollution. Especially in large-scale production, the use of ethylene glycol increases the preparation cost and may produce toxic by-products.
The method of preparing nano nickel powder by mixing deionized water with ethylene glycol as a solvent, combining NaOH, sodium borohydride and polyvinylpyrrolidone, magnetic stirring and heating reactions are carried out to control the reaction conditions to achieve a more uniform particle Diameter distribution and energy consumption reduction.
Through the synergistic action of mixed solvents, the productivity and particle size distribution of nano nickel powder are improved, energy consumption and production costs are reduced, and environmental pollution risks and difficulty in handling by-products are reduced.
Smart Images

Figure CN118875273A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing nano nickel powder, belonging to the technical field of nanometers. Background Art
[0002] Nano nickel powder has good corrosion resistance, wear resistance and magnetic properties, and is widely used in steel, nickel-based alloys, electroplating and batteries. There are many methods for preparing nickel powder. According to the different preparation processes, it can be roughly divided into several categories such as electrolysis, carbonylation, solution reduction, and atomization. Among them, the solution reduction method has a wide source of raw materials, simple equipment, and easy operation. It can prepare high-purity, small-size, and uniformly distributed nickel powder. Compared with other methods, it has obvious advantages. However, the reaction of a single solvent has some shortcomings;
[0003] According to the existing preparation methods of nano nickel powder, ethylene glycol is mainly used as a solvent, a small part of which is deionized water as a solvent, and generally nickel sulfate or nickel chloride is used as a nickel source. The preparation principle is a reduction method. Ethylene glycol is not only a solvent, but also has a certain reducing property. The general steps include dissolving the nickel salt in the solvent, adding a suitable reducing agent, such as sodium borohydride or ammonia water, and then reacting at 70°C-90°C for 3h-4h. Finally, the nano nickel powder is obtained by separation, washing and drying. Although the nano nickel powder is prepared, there are still several problems:
[0004] Patent No. CN105268984A: relates to a method for preparing nano nickel powder by a liquid phase fluidized reduction method, wherein nickel nitrate or nickel sulfate is dissolved in deionized water, and a coordination agent and a surfactant polyvinyl pyrrolidone are added to generate nano nickel powder. The prepared nano nickel powder usually has a wide particle size distribution and is difficult to accurately control the particle size at the nanometer level. This is because in the aqueous phase reaction, due to the diffusion rate of ions in the solution and the complexity of the reaction kinetics, the growth rate of nano particles is difficult to accurately control, resulting in a problem of wide particle size distribution;
[0005] Patent No. CN115087506A: By dissolving nickel sulfate and citric acid in ethylene glycol, mixing the organic sol containing nickel with a water-soluble salt, a sol-gel transition occurs, and then a calcination process is adopted to calcine the calcined product nickel oxide at 400°C-600°C in a reducing atmosphere to convert the nickel oxide nanoparticles into nickel nanoparticles, and the reduced product is washed with water and dried to obtain highly crystalline nano nickel powder. The cost of ethylene glycol as a solvent is relatively high, especially in large-scale production, which will increase the overall preparation cost. At the same time, ethylene glycol may produce toxic by-products and require additional processing steps. Summary of the invention
[0006] The main purpose of the present invention is to provide a method for preparing nano nickel powder with a mixed solvent, which solves the problems of too large particle size, uneven particle size distribution, high cost and environmental pollution in the existing preparation method.
[0007] To achieve the above object, the technical solution adopted by the present invention is:
[0008] A method for preparing nano nickel powder using a mixed solvent comprises the following steps:
[0009] Step 1: prepare a mixed solvent and perform magnetic stirring to obtain a mixed solution A;
[0010] Step 2: Weigh a nickel salt, add the nickel salt to the mixed solution A, stir and dissolve evenly, to obtain a nickel salt solution B;
[0011] Step 3: Weigh NaOH, a reducing agent and a dispersing agent respectively, and add them to the nickel salt solution B in the order of addition, stirring and dissolving, to obtain a solution C;
[0012] Step 4: Place solution C in a water bath for heating reaction;
[0013] Step 5: After the reaction of solution C is completed, continue stirring to ensure uniform distribution of the nano-nickel powder.
[0014] Step 6: vacuum filtering, washing and vacuum drying the solid-liquid mixture to obtain nano nickel powder;
[0015] The mixed solution is a mixture of deionized water and ethylene glycol;
[0016] Further, the nickel salt is nickel chloride;
[0017] The reducing agent is sodium borohydride;
[0018] The dispersant is polyvinyl pyrrolidone.
[0019] Furthermore, the mixed solution is 360 g, and the mass ratio of ethylene glycol to deionized water in the mixed solution is 1:1-1.6.
[0020] Further, the nickel salt concentration is 0.33 mol / L-0.41 mol / L;
[0021] The amount of NaOH is 7.5g-8.5g;
[0022] The amount of polyvinyl pyrrolidone is 1.5g-4.3g;
[0023] The amount of sodium borohydride used is 11g-13g.
[0024] Furthermore, in step three, the order of addition is to first add NaOH to the nickel salt solution B, then continue to add polyvinyl pyrrolidone and stir until it is completely dissolved, and finally add sodium borohydride and stir until it is completely dissolved.
[0025] Furthermore, the temperature of the heating reaction is 70°C-75°C, the pH value is controlled at about 10, and the reaction time is 2h-3h;
[0026] In step 5, the stirring time is 2h-3h.
[0027] Furthermore, in step six, the washing solvent is deionized water;
[0028] The vacuum drying temperature is 80°C-120°C, and the time is 6h-8h.
[0029] Compared with the prior art, the present invention has the following beneficial effects:
[0030] 1. The present invention combines the good solubility, low surface tension and nucleation barrier, high boiling point, reducibility and stability of ethylene glycol with the wide solubility, moderate viscosity and high fluidity of deionized water by mixing deionized water and ethylene glycol as solvents. The synergistic effect of deionized water and ethylene glycol is utilized to facilitate the reduction reaction at a lower temperature, thereby reducing energy consumption. The mixed solvent can provide a more uniform reaction environment, promote the full dissolution of nickel salt, thereby improving the efficiency of the reduction reaction and the productivity of nano nickel powder, and controlling the size distribution of nano particles and the particle growth rate during the reaction.
[0031] 2. The present invention uses a mixture of deionized water and ethylene glycol as a solvent, which can simultaneously exert the advantages of water and ethylene glycol, reduce the complexity of switching between different solvents, and thus simplify the experimental steps. The mixed solvent improves the reaction efficiency and the productivity of nano nickel powder, reduces energy consumption and the cost of processing by-products, reduces production costs, and reduces the large-scale use of a single solvent, thereby reducing the difficulty of waste liquid treatment and the risk of environmental pollution. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 This is the SEM image of the nano nickel powder prepared in Example 1;
[0033] Figure 2 This is the SEM image of the nano nickel powder prepared in Comparative Example 1. DETAILED DESCRIPTION
[0034] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0035] A method for preparing nano nickel powder using a mixed solvent comprises the following steps:
[0036] Step 1: prepare a mixed solvent and perform magnetic stirring to obtain a mixed solution A;
[0037] Step 2: Weigh a nickel salt, add the nickel salt to the mixed solution A, stir and dissolve evenly, to obtain a nickel salt solution B;
[0038] Step 3: Weigh NaOH, a reducing agent and a dispersing agent respectively, and add them to the nickel salt solution B in the order of addition, stirring and dissolving, to obtain a solution C;
[0039] Step 4: Place solution C in a water bath for heating reaction;
[0040] Step 5: After the reaction of solution C is completed, continue stirring to ensure uniform distribution of the nano-nickel powder.
[0041] Step 6: vacuum filtering, washing and vacuum drying the solid-liquid mixture to obtain nano nickel powder;
[0042] The mixed solution is a mixture of deionized water and ethylene glycol;
[0043] Further, the nickel salt is nickel chloride;
[0044] The reducing agent is sodium borohydride;
[0045] The dispersant is polyvinyl pyrrolidone.
[0046] The invention provides a method for preparing nano nickel powder by using a mixed solvent. The method comprises the following steps: deionized water and ethylene glycol are mixed as solvents, the good solubility, low surface tension and nucleation barrier, high boiling point, reducibility and stability of ethylene glycol are combined with the wide solubility, moderate viscosity and high fluidity of deionized water, and the synergistic effect of deionized water and ethylene glycol is utilized to facilitate reduction reaction at a lower temperature, thereby reducing energy consumption; the mixed solvent can provide a more uniform reaction environment, promote the full dissolution of nickel salt, thereby improving the efficiency of reduction reaction and the productivity of nano nickel powder, controlling the size distribution of nano particles and the particle growth rate during the reaction; and at the same time, reducing the complexity of switching between different solvents, thereby simplifying the experimental steps; the mixed solvent improves the reaction efficiency and the productivity of nano nickel powder, reduces energy consumption and the cost of processing by-products, reduces production costs, reduces the large-scale use of a single solvent, and reduces the difficulty of waste liquid treatment and the risk of environmental pollution.
[0047] Furthermore, the mixed solution is 360 g, and the mass ratio of ethylene glycol to deionized water in the mixed solution is 1:1-1.6.
[0048] Further, the nickel salt concentration is 0.33 mol / L-0.41 mol / L;
[0049] The amount of NaOH is 7.5g-8.5g;
[0050] The amount of polyvinyl pyrrolidone is 1.5g-4.3g;
[0051] The amount of sodium borohydride used is 11g-13g.
[0052] Furthermore, in step three, the order of addition is to first add NaOH to the nickel salt solution B, then continue to add polyvinyl pyrrolidone and stir until it is completely dissolved, and finally add sodium borohydride and stir until it is completely dissolved.
[0053] The main purpose of adding NaOH first is to adjust the pH value of the reaction so that it is in an alkaline environment suitable for nickel ion reduction. Under alkaline conditions, nickel ions (such as Ni2+) are more likely to combine with OH- to form nickel hydroxide (Ni(OH)2) or other intermediates, which are more likely to be reduced to metallic nickel by the reducing agent in the subsequent reduction step;
[0054] Adding polyvinyl pyrrolidone after adding NaOH can control the directional growth and deposition of nickel particles in the reaction system. It can change the surface properties of nickel particles by adsorbing on the surface of nickel particles, thereby affecting the growth rate and aggregation mode of the particles, and ultimately affecting the morphology and particle size distribution of the product.
[0055] Sodium borohydride is added last after NaOH and polyvinyl pyrrolidone are completely dissolved. This is because sodium borohydride, as a strong reducing agent, will quickly initiate a reduction reaction after being added. Therefore, it needs to be added after other raw materials are fully mixed and reach a stable state.
[0056] Furthermore, the temperature of the heating reaction is 70°C-75°C, the pH value is controlled at about 10, and the reaction time is 2h-3h;
[0057] In step 5, the stirring time is 2h-3h.
[0058] Furthermore, in step six, the washing solvent is deionized water;
[0059] The vacuum drying is carried out at a temperature of 80°C-120°C and for a time of 6h-8h.
[0060] The temperature and time of vacuum drying are 80℃-120℃ and 6h-8h respectively. This temperature range helps to effectively remove moisture from nickel powder while avoiding excessively high temperature that may cause changes in the properties of nickel powder or other adverse effects. During this period of time, most of the moisture can be effectively removed. The specific drying time should be adjusted according to actual conditions. If the moisture content in the nickel powder is high, or a higher drying standard needs to be met, the drying time can be appropriately extended. Conversely, if the nickel powder is already relatively dry, or in order to save time and energy, the drying time can be appropriately shortened.
[0061] Some implementation modes of the present invention are described in detail below in conjunction with examples.
[0062] Example 1
[0063] This embodiment provides a method for preparing nano nickel powder with a mixed solvent, and the preparation process is as follows:
[0064] Step 1: first weigh 180 g of deionized water in a beaker, then add 180 g of ethylene glycol, and stir for 1 h to 2 h to obtain a mixed solvent A;
[0065] Step 2: Weigh 16 g of nickel chloride in a beaker, add 360 g of a mixed solvent, and stir to obtain a uniform nickel salt solution B;
[0066] Step 3: Weigh 8 g of NaOH, 11 g of sodium borohydride and 2 g of polyvinylpyrrolidone (PVP) in a beaker, add the weighed NaOH and polyvinylpyrrolidone to nickel salt solution B under stirring, stir until completely dissolved, then add sodium borohydride to nickel salt solution B and stir to obtain solution C;
[0067] Step 4: Place solution C in a water bath for heating reaction at a temperature of 70°C-75°C and a pH value of about 10. To ensure the complete reduction reaction, the reaction time is 2h-3h.
[0068] Step 5: After the reaction is completed, continue stirring for 2h-3h to ensure uniform distribution of the nano-nickel powder.
[0069] Step 6: Separation and Drying
[0070] 1. Separation: Use vacuum filtration equipment to separate the nano nickel powder generated by the reaction from the solution;
[0071] 2. Washing: Wash the nano nickel powder with deionized water to remove residual reactants and by-products;
[0072] 3. Drying: Place the washed nano-nickel powder in a vacuum drying oven for drying at a temperature of 80°C-120°C for 6h-8h to obtain the final nano-nickel powder product with a particle size of about 128nm-295nm.
[0073] The prepared nano nickel powder reference Figure 1
[0074] Example 2
[0075] This embodiment provides a method for preparing nano nickel powder with a mixed solvent, and the preparation process is as follows:
[0076] Step 1: first weigh 218 g of deionized water in a beaker, then add 142 g of ethylene glycol, and stir for 1 h-2 h to obtain a mixed solvent A;
[0077] Step 2: Weigh 16 g of nickel chloride in a beaker, add 360 g of a mixed solvent, and stir to obtain a uniform nickel salt solution B;
[0078] Step 3: Weigh 8 g of NaOH, 12 g of sodium borohydride and 4 g of polyvinylpyrrolidone (PVP) in a beaker, add the weighed NaOH and polyvinylpyrrolidone to nickel salt solution B under stirring, stir until completely dissolved, then add sodium borohydride to nickel salt solution B and stir to obtain solution C;
[0079] Step 4: Place solution C in a water bath for heating reaction at a temperature of 70°C-75°C and a pH value of about 10. To ensure the complete reduction reaction, the reaction time is 2h-3h.
[0080] Step 5: After the reaction is completed, continue stirring for 2h-3h to ensure uniform distribution of the nano-nickel powder.
[0081] Step 6: Separation and Drying
[0082] 1. Separation: Use vacuum filtration equipment to separate the nano nickel powder generated by the reaction from the solution;
[0083] 2. Washing: Wash the nano nickel powder with deionized water to remove residual reactants and by-products;
[0084] 3. Drying: Place the washed nano-nickel powder in a vacuum drying oven for drying at a temperature of 80°C-120°C for a drying time of 6h-8h to obtain the final nano-nickel powder product.
[0085] Comparative Example 1
[0086] This comparative example provides a method for preparing nano nickel powder with a mixed solvent, and the preparation process is as follows:
[0087] Step 1: Weigh 15 g of nickel chloride in a beaker, add 320 g of deionized water, and stir to obtain a uniform nickel salt solution B;
[0088] Step 2: weigh 7 g of NaOH, 15 g of sodium borohydride and 4.2 g of polyvinylpyrrolidone (PVP) in a beaker, add the weighed NaOH and polyvinylpyrrolidone to nickel salt solution B under stirring, stir until completely dissolved, then add sodium borohydride to the nickel salt solution and stir to obtain solution C;
[0089] Step 3: Place solution C in a water bath for heating reaction at a temperature of 70°C-75°C and a pH value of about 10. To ensure the complete reduction reaction, the reaction time is 2h-3h.
[0090] Step 4: After the reaction is completed, continue stirring for 2h-3h to ensure uniform distribution of the nano-nickel powder.
[0091] Step 5: Separation and drying
[0092] 1. Separation: Use vacuum filtration equipment to separate the nano nickel powder generated by the reaction from the solution;
[0093] 2. Washing: Wash the nano nickel powder with deionized water to remove residual reactants and by-products;
[0094] 3. Drying: Place the washed nano-nickel powder in a vacuum drying oven for drying at a temperature of 80°C-120°C for a drying time of 6h-8h to obtain the final nano-nickel powder product.
[0095] Prepared nano nickel powder reference Figure 2 .
[0096] It should be understood that the preferred specific embodiments of the present invention can be modified and varied by ordinary technicians in the field without creative work. Therefore, any technical solution that can be obtained by technicians in the field of technology through logical analysis, reasoning or limited experiments based on the concept of the present invention on the basis of the prior art should be within the scope of protection determined by the claims.
Claims
1. A method for preparing nano nickel powder using a mixed solvent, characterized in that: The following steps are involved: Step 1: prepare a mixed solvent and perform magnetic stirring to obtain a mixed solution A; Step 2: Weigh a nickel salt, add the nickel salt to the mixed solution A, stir and dissolve evenly, to obtain a nickel salt solution B; Step 3: Weigh NaOH, dispersant and reducing agent respectively, and add them into nickel salt solution B in the order of addition, stirring and dissolving to obtain solution C; Step 4: Place solution C in a water bath for heating reaction; Step 5: After the reaction of solution C is completed, continue stirring to ensure uniform distribution of nano-nickel powder; Step 6: vacuum filtering, washing and vacuum drying the solid-liquid mixture to obtain nano nickel powder; The mixed solution is a mixture of deionized water and ethylene glycol.
2. The method for preparing nano nickel powder using a mixed solvent according to claim 1, wherein: The nickel salt is nickel chloride; The reducing agent is sodium borohydride; The dispersant is polyvinyl pyrrolidone.
3. The method for preparing nano nickel powder using a mixed solvent according to claim 1, wherein: The mixed solution is 360 g, and the mass ratio of ethylene glycol to deionized water in the mixed solution is 1:1-1.
6.
4. A method for preparing nano nickel powder using a mixed solvent according to any one of claims 1-2, It is characterized in that The nickel salt concentration is 0.33 mol / L-0.41 mol / L; The amount of NaOH is 7.5g-8.5g; The amount of polyvinyl pyrrolidone is 1.5g-4.3g; The amount of sodium borohydride used is 11g-13g.
5. The method for preparing nano nickel powder using a mixed solvent according to claim 1, wherein: In step three, the order of addition is to first add NaOH to the nickel salt solution B, then continue to add polyvinyl pyrrolidone and stir until it is completely dissolved, and finally add sodium borohydride and stir until it is completely dissolved.
6. The method for preparing nano nickel powder using a mixed solvent according to claim 1, wherein: The heating reaction temperature is 70°C-75°C, the pH value is controlled at about 10, and the reaction time is 2-3h; In step 5, the stirring time is 2h-3h.
7. The method for preparing nano nickel powder using a mixed solvent according to claim 1, wherein: In step six, the washing solvent is deionized water; The vacuum drying is carried out at a temperature of 80°C-120°C and for a time of 6h-8h.