Flaky iron powder lightweight wave-absorbing material and preparation method thereof

The preparation of lightweight sheet iron powder through direct reduction and unique ball milling processes has solved the problems of high ball milling and high specific gravity in the prior art, and achieved the preparation of lightweight sheet iron powder with excellent performance and low cost, broadening the application scenarios.

CN118875274APending Publication Date: 2024-11-01ZHENGZHOU QISHAN ANTI CORROSION PROTECTION NEW MATERIAL TECH RES INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410883199.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-03
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The existing process of preparing flaky carbonyl iron powder radar wave absorbers has the problem of high ball hardship, long time and high cost, and its proportion is relatively large, which violates the four elements of "light, wide, thin, and strong" of wave absorbing materials.

Method used

By directly reducing ultrafine iron oxide powder and then performing high-speed ball milling in a planetary mill, combining high-temperature one-step reduction and surface passivation treatment, a sheet iron powder lightweight absorbing material with an average particle size of 8μm was prepared, and repeated washing and Unique ball milling process adjusts the microscopic morphology and reduces production costs.

Benefits of technology

The lightweight sheet iron powder with a specific gravity of only 1/3 of the common iron-based radar wave absorber was successfully prepared, which broadened the application scenarios, improved the wave absorption performance, and reduced production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118875274A_ABST
    Figure CN118875274A_ABST
Patent Text Reader

Abstract

The invention relates to the field of wave-absorbing materials, in particular to a flaky iron powder lightweight wave-absorbing material and a preparation method thereof. The average particle size of the flaky iron powder is 8 microns, the iron grade is 98.5%, the apparent density and the tap density are 1 / 3 of those of carbonyl iron powder, the lamellar morphology is good, the radius-thickness ratio is 15: 1, and the flaky iron powder is prepared through the steps of sanding, water washing, filter pressing, drying, crushing, reduction, planetary ball milling, drying, crushing, sieving and the like. The wave-absorbing performance is excellent, and the production cost is lower.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of wave-absorbing materials, and in particular to a flaky iron powder lightweight wave-absorbing material and a preparation method thereof. Background Art

[0002] At present, the existing processes for preparing reduced iron powder all adopt a two-step reduction method, and the particle size of the reduced iron powder is relatively large; the existing flaky carbonyl iron powder radar wave absorber has a large specific gravity, which restricts its application in certain scenarios; the ball milling time of spherical carbonyl iron powder is long and difficult when it is flaked.

[0003] Existing flaky iron powder radar wave absorbers are all spherical carbonyl iron powders that are prepared by mechanical ball milling. This process has the problems of high difficulty and long ball milling time, and high production cost of spherical carbonyl iron powders. The specific gravity of flaky carbonyl iron powder absorbers is relatively large, which is contrary to the lightness of the four elements of "light, wide, thin, and strong" emphasized by absorbing materials. Summary of the invention

[0004] To solve the problems of the prior art, the present invention provides a flaky iron powder lightweight absorbing material and a preparation method thereof. The flaky iron powder prepared by direct reduction of ultrafine iron oxide powder and then ball milling is lighter, has excellent absorbing performance, and has lower production cost.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] A flaky iron powder lightweight absorbing material, with an average particle size of 8 μm, an iron grade of 98.5%, a bulk density and a tap density of 1 / 3 of carbonyl iron powder, a good lamellar morphology, and a diameter-to-thickness ratio of 15:1.

[0007] A method for preparing a flaky iron powder lightweight absorbing material comprises the following steps:

[0008] S1: Wet-grind 325-mesh iron oxide powder with a sand mill to obtain an iron oxide red slurry with an average particle size of 5 μm;

[0009] S2: repeatedly washing the ground red iron oxide slurry with water to obtain a red iron oxide slurry with a relatively uniform particle size;

[0010] S3: The washed red iron oxide slurry is filtered and dehydrated by a filter press to obtain a filter cake, and then the filter cake is placed in a drum dryer for high-temperature drying, and the dried filter cake is crushed by a pulverizer to obtain red iron oxide powder with an average particle size of 5 μm;

[0011] S4: placing the ultrafine iron oxide red powder into an atmosphere rotary furnace for high-temperature one-step direct reduction, and then performing surface passivation treatment on the reduced iron powder to obtain ultrafine iron powder;

[0012] S5: The surface passivated iron powder is placed in a planetary ball mill for high-speed ball milling. During the ball milling process, the ball mill needs to be ventilated with nitrogen for inert protection. The ball milling dispersant is anhydrous ethanol and the addition amount is 9wt%, the ball-to-material ratio is 10:1, the rotation speed is 300r / min, and the ball milling time is 20h;

[0013] S6: The flaky iron powder slurry after ball milling is placed in a vacuum drying oven and dried at 50° C. for 48 hours. The dried powder is then crushed by a crusher and passed through a 325-mesh vibrating sieve to obtain flaky iron powder with an average particle size of 8 μm.

[0014] In the method for preparing the flaky iron powder lightweight absorbing material, the grinding dispersant in step S1 is deionized water, the grinding solid-liquid ratio is 40%, and the grinding time is 20 minutes.

[0015] In the method for preparing the flaky iron powder lightweight absorbing material, the chemical reaction formula involved in step S4 is as follows:

[0016] 3Fe2O3(s)+H2=2Fe3O4(s)+H2O(g) (1)

[0017] Fe3O4(s)+H2=3FeO(s)+H2O(g) (2)

[0018] FeO(s)+H2=Fe(s)+H2O(g) (3)

[0019]

[0020] Fe2O3(s)+3H2=2Fe(s)+3H2O(g) (5)

[0021] In the actual reduction reaction process, Fe2O3 is gradually reduced to Fe, so the Gibbs free energy of the above reaction equation is calculated in a distributed manner. For reaction equation (1):

[0022]

[0023] For reaction formula (4):

[0024]

[0025] From the above calculation results, it can be seen that reaction (1) can react at room temperature, but reaction (4) cannot react. This reaction becomes a limiting factor for the reduction of Fe2O3 to Fe at room temperature. If the temperature condition is changed to 300℃, the Gibbs free energy of reaction (5) is calculated as follows:

[0026]

[0027] From the above calculations, we can see that the Gibbs free energy of reaction (5) at 300°C is less than 0, so the reaction can proceed at this temperature. Subsequent experiments also confirmed this judgment.

[0028] Compared with the prior art, the beneficial effects of the invention are: 1. Innovation of raw materials. The raw materials selected by the present invention are quite different from the raw material carbonyl iron powder used in the past for preparing flaky iron powder radar wave absorbers. The raw materials selected by the present invention are 325 mesh iron concentrate obtained by processing specularite through a variety of mineral processing techniques. The iron concentrate itself does not have wave absorbing properties, but a lightweight flaky iron powder radar wave absorber with excellent performance is successfully prepared through an original one-step direct reduction process and a unique planetary ball milling process.

[0029] 2. In view of the fact that some nano red iron oxide particles are over-ground during the sand grinding process, the present invention proposes to remove them by repeated water washing, thereby solving the problem that the microwave absorption performance of the final product is affected by the uneven particle size distribution of nano ultrafine particles.

[0030] 3. A one-step direct reduction process (reduction temperature 700°C, reduction time 10h, hydrogen volume 21L / min, nitrogen volume 7L / min) is used to directly reduce red iron oxide powder with an average particle size of 5μm into high-purity ultrafine iron powder. The particle size of the iron powder after reduction does not change much compared with red iron oxide, and the average particle size is still only a few microns. The product purity can also reach more than 98.5%. The present invention adopts a unique one-step direct reduction process to successfully solve the problem that it is difficult to directly reduce micro-nano-level ultrafine iron oxide powder into ultrafine iron powder.

[0031] 4. By adopting a unique planetary ball milling process (dispersant addition amount is 9wt%, ball-to-material ratio is 10:1, ball milling speed is 300r / min, ball milling time is 20h), the microstructure of the reduced iron powder is adjusted to a flaky structure, and the obtained flaky iron powder radar wave absorber is lighter, with a specific gravity of only about 1 / 3 of the common iron-based radar wave absorber, which solves the problem that the iron-based radar wave absorber is not light enough and broadens the application scenarios of the iron-based radar wave absorber. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Other features, objectives and advantages of the present invention will become more apparent from a reading of the detailed description of non-limiting embodiments made with reference to the following accompanying drawings.

[0033] Figure 1 It is a curve diagram showing the influence of reduction temperature on the reduction rate of iron powder in the present invention.

[0034] Figure 2 It is a curve diagram showing the effect of reduction time on the reduction rate of iron powder in the present invention.

[0035] Figure 3 It is the laser particle size distribution diagram of the flaky iron powder in the present invention.

[0036] Figure 4 It is a simulation diagram of the detection results of the vector network (coaxial method) in the present invention.

[0037] Figure 5 It is a curve diagram of the vector network (bow method) detection results in the present invention.

[0038] Figure 6 It is a process flow chart of the present invention. DETAILED DESCRIPTION

[0039] The present invention is further described in detail below by examples, which are only used to illustrate the present invention and are not intended to limit the scope of the present invention.

[0040] A flaky iron powder lightweight absorbing material, characterized in that it has an average particle size of 8 μm, an iron grade of 98.5%, a loose density and a tap density of 1 / 3 of carbonyl iron powder, a good lamellar morphology, and a diameter-to-thickness ratio of 15:1. Vector network analyzer simulation and actual measurement show that the absorbing performance is excellent in the X-band.

[0041] The invention provides a method for preparing a flaky iron powder lightweight radar absorbing material from an iron oxide powder, comprising the following steps: S1, high-speed sand milling the 325-mesh iron oxide powder to obtain an iron oxide red slurry with an average particle size of 5 μm; S2, repeatedly washing the iron oxide red slurry with water for multiple times to remove nano-ultrafine particles in the slurry to obtain an iron oxide red slurry with a relatively uniform particle size; S3, filtering and dehydrating the washed iron oxide red slurry, and then putting it into a dryer for drying, and then crushing the dried filter cake to obtain a 5-μm iron oxide red powder; S4, putting the iron oxide red powder into an atmosphere rotary furnace for high-temperature one-step direct reduction, and then performing surface passivation treatment on the reduced iron powder to obtain ultrafine iron powder; S5, putting the ultrafine iron powder into a planetary ball mill, adding a small amount of dispersant, and high-speed ball milling under the protection of an inert atmosphere, and then vacuum drying the ball-milled slurry, crushing it, and sieving it to obtain a flaky iron powder lightweight radar wave absorber.

[0042] A specific method for preparing a flaky iron powder lightweight absorbing material is characterized by comprising the following steps:

[0043] S1: Wet-grind 325-mesh iron oxide powder with a sand mill to obtain an iron oxide red slurry with an average particle size of 5 μm. The grinding dispersant in this step is deionized water, the grinding solid-liquid ratio is 40%, and the grinding time is 20 min.

[0044] S2: repeatedly washing the ground red iron oxide slurry with water to obtain a red iron oxide slurry with a relatively uniform particle size;

[0045] The main purpose of this step is to remove the nano-scale ultrafine red iron oxide particles in the slurry, so that the particle size distribution of the red iron oxide is more uniform;

[0046] S3: The washed red iron oxide slurry is filtered and dehydrated by a filter press to obtain a filter cake, and then the filter cake is placed in a drum dryer for high-temperature drying, and the dried filter cake is crushed by a pulverizer to obtain red iron oxide powder with an average particle size of 5 μm;

[0047] S4: placing the iron oxide red powder into an atmosphere rotary furnace for high-temperature one-step direct reduction, and then performing surface passivation treatment on the reduced iron powder to obtain ultrafine iron powder; specifically, placing the iron oxide red powder into an atmosphere rotary furnace, reducing it at a reduction temperature of 700°C for 10 hours, the reducing atmosphere being a mixture of hydrogen and nitrogen, the ratio of hydrogen to nitrogen being 3:1, after the temperature of the rotary furnace drops to 300°C, introducing a passivation gas to perform surface passivation treatment on the reduced iron powder, the passivation gas volume being 3L / min, the passivation time being 30min, the passivation gas used being a mixture of nitrogen and oxygen, the ratio of nitrogen to oxygen being 95:5, the purity of the iron powder obtained after passivation being 98.5%, and the average particle size being 8μm;

[0048] S5: The surface passivated iron powder is placed in a planetary ball mill for high-speed ball milling. During the ball milling process, the ball mill needs to be ventilated with nitrogen for inert protection. The ball milling dispersant is anhydrous ethanol and the addition amount is 9wt%, the ball-to-material ratio is 10:1, the rotation speed is 300r / min, and the ball milling time is 20h;

[0049] S6: The flaky iron powder slurry after ball milling is placed in a vacuum drying oven and dried at 50° C. for 48 hours. The dried powder is then crushed by a crusher and passed through a 325-mesh vibrating sieve to obtain flaky iron powder with an average particle size of 8 μm.

[0050] The main raw material used in the scheme of the present invention is iron oxide powder, which is iron concentrate processed by various mineral processing processes of specularite, with a particle size of 200-350 meshes, an iron grade of 69.5%, and lower contents of other elements at the ppm level, and an irregular block shape. The gas used in the present invention is hydrogen, nitrogen, and a mixture of nitrogen and oxygen. The grinding dispersant used in the present invention is deionized water and anhydrous ethanol.

[0051] The equipment used in the invention includes a sand mill, a filter press, a drum dryer, a pulverizer, an atmosphere rotary furnace, a planetary ball mill, a vacuum drying box and a vibrating screen.

[0052] It should be noted that:

[0053] 1. Other dehydration and drying schemes include centrifugation and filter pressing for dehydration, and drum drying, box drying, belt drying, flash evaporation, spray drying, etc. The filter press dehydration and drum drying equipment used in the present invention are the optimal schemes after non-limited experimental verification, and the scheme has the highest production efficiency.

[0054] 2. Selection of reducing agent in the reduction process: carbon monoxide, hydrogen, coke oven gas, coke powder, graphite powder, etc. The reducing agent used in the present invention is hydrogen, which is obtained by decomposing liquid ammonia. Compared with other reducing agents, it is clean and pollution-free, and the reducing agent has better reduction efficiency after comprehensive comparison.

[0055] 3. The reduction temperature during the reduction process is 650-800°C, the reduction time is 8-12h, and the passivation time is 0.5-2h. The reduction process conditions of the present invention are a reduction temperature of 700°C, a reduction time of 10h, and a passivation time of 0.5h. This process is the best condition after a limited number of experimental verifications. Other conditions have their own shortcomings, either the reduction effect is not the best, or the energy consumption increases during the reduction process.

[0056] 4. Types of dispersants in the planetary ball milling process: anhydrous ethanol, liquid paraffin, silane coupling agent and calcium stearate, etc., the amount of dispersant added is 8wt% to 12wt%, the ball mill speed is 250 to 400r / min, and the ball milling time is 15 to 30h. The dispersant used in the present invention is anhydrous ethanol, which should have a better dispersion effect after experimental control. Ball milling process: the amount of dispersant added is 9wt%, the ball mill speed is 300r / min, the ball-to-material ratio is 10:1, and the ball milling time is 20h. This process is the optimal condition obtained through a large number of non-limited experiments. Some other process conditions cannot obtain the optimal results, and some have too high energy consumption.

[0057]

[0058] Table 1 Effect of passivation time on iron powder passivation results

[0059]

[0060] Table 2 Effect of different ball milling factors on the diameter-thickness ratio of flaky iron powder

[0061]

[0062] Table 3 Iron content test results of flaky iron powder

[0063]

[0064] Table 4 Density comparison of flaky iron powder and carbonyl iron powder Although the above describes the specific embodiments of the present invention, it should be understood by those skilled in the art that this is only an example, and the scope of protection of the present invention is defined by the appended claims. Those skilled in the art may make various changes or modifications to these embodiments without departing from the principle and essence of the present invention, but these changes and modifications all fall within the scope of protection of the present invention.

Claims

1. A flaky iron powder lightweight absorbing material, characterized in that: Its average particle size is 8μm, the iron grade is 98.5%, the bulk density and tap density are 1 / 3 of carbonyl iron powder, the lamellar morphology is good and the diameter-to-thickness ratio is 15:

1.

2. A method for preparing a flaky iron powder lightweight absorbing material, characterized in that: The steps include: S1: Wet-grind 325-mesh iron oxide powder with a sand mill to obtain an iron oxide red slurry with an average particle size of 5 μm; S2: repeatedly washing the ground red iron oxide slurry with water to obtain a red iron oxide slurry with a relatively uniform particle size; S3: The washed red iron oxide slurry is filtered and dehydrated by a filter press to obtain a filter cake, and then the filter cake is placed in a drum dryer for high-temperature drying, and the dried filter cake is crushed by a pulverizer to obtain red iron oxide powder with an average particle size of 5 μm; S4: placing the iron oxide red powder into an atmosphere rotary furnace for high-temperature one-step direct reduction, and then performing surface passivation treatment on the reduced iron powder to obtain ultrafine iron powder; S5: The surface passivated iron powder is placed in a planetary ball mill for high-speed ball milling. During the ball milling process, the ball mill tank needs to be ventilated with nitrogen for inert protection. The ball milling dispersant is anhydrous ethanol and the addition amount is 9wt%, the ball-to-material ratio is 10:1, the rotation speed is 300r / min, and the ball milling time is 20h; S6: The flaky iron powder slurry after ball milling is placed in a vacuum drying oven and dried at 50° C. for 48 hours. The dried powder is then crushed by a crusher and passed through a 325-mesh vibrating sieve to obtain flaky iron powder with an average particle size of 8 μm.

3. The method for preparing the flaky iron powder lightweight absorbing material according to claim 2, characterized in that: The grinding dispersant in step S1 is deionized water, the grinding solid-liquid ratio is 40%, and the grinding time is 20 min.