CrSi target material as well as preparation method and application thereof
Through specific raw material mixing and stage-based procedural sintering processes, the problem of insufficient quality of CrSi targets is solved, and the preparation of CrSi targets with high density and high purity is achieved. It is suitable for industrial production and meets the quality requirements of the high-end electronics industry.
Patent Information
- Application Number
- CN202410981724.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-01
AI Technical Summary
The quality of existing CrSi targets is insufficient, the density and purity are difficult to reach high levels, the proportion of elements is unstable, and the profit margin and efficiency of traditional production methods are low, so they cannot meet the quality requirements of the high-end electronics industry.
Specific raw material mixing and stage-based procedural sintering processes, including ball milling treatment, segmented heating and pressure control, and through pre-pressure and pressure relief treatment, the raw materials are evenly dispersed and fully activated, forming a high-density and high-purity CrSi target material. .
Without relying on special equipment or strict conditions, the high density and purity of CrSi targets are achieved, ensuring the stability of Cr-Si element content, suitable for industrial mass production, and improving the comprehensive quality of the product .
Abstract
Description
Technical Field
[0001] The present invention relates to the field of metal processing, and in particular to a CrSi target material and a preparation method and application thereof. Background Art
[0002] CrSi target is a new type of vacuum coating sputtering target material suitable for the field of electronic gates and electronic thin films. However, the quality of CrSi targets produced by existing technologies is insufficient, and it is difficult to achieve sufficient density and purity. At the same time, it is difficult to control the proportion of elements during the processing to achieve a stable level, and the sputtering performance is poor, which cannot meet the requirements of the high-end electronics industry for target quality. Although the use of expensive equipment and strict production conditions can significantly improve the quality of the target, this production method has low profit margins and low production efficiency, and is not suitable for the industrialized industrial chain. Summary of the invention
[0003] Based on the defects of the prior art, the purpose of the present invention is to provide an efficient and cost-effective method for preparing CrSi target materials. Through specific raw material mixing and special stage-programmed sintering and pressure control processes, the prepared products can meet the requirements of high density and high purity without relying on special equipment or harsh conditions. At the same time, the content of Cr-Si elements is highly controlled and stable, the overall quality of the product is high, and industrial mass production can be realized.
[0004] In order to achieve the above object, the technical solution adopted by the present invention is:
[0005] A method for preparing a CrSi target material comprises the following steps:
[0006] (1) Si powder and Cr powder are mixed and ball-milled in a protective atmosphere to obtain a mixed powder having a particle size Dv 50 ≤50μm;
[0007] (2) pre-pressing the mixed powder in a vacuum environment to obtain a rough target blank;
[0008] (3) heating the rough target blank to 600-800° C. at a rate of 15-20° C. / min in a vacuum environment, and when the ambient pressure reaches 6-10 MPa, releasing the pressure at a rate of 1.5-3 MPa / min for 3-6 min;
[0009] (4) then heating the temperature to 1150-1250°C at a rate of 8-10°C / min for a second time, and simultaneously releasing the pressure at a rate of 1-2MPa / min for 2-5min when the ambient pressure reaches 5-8MPa;
[0010] (5) Keep the temperature at 1150-1250°C for 30-60 min, and release the pressure at a rate of 0.5-1 MPa / min for 3-6 min when the ambient pressure reaches 3-5 MPa;
[0011] (6) After the heat preservation is completed, the pressure is increased to 35-40 MPa at a rate of 0.3-0.5 MPa / min and the heat and pressure are continued for 90-150 minutes, and then cooled to obtain the CrSi target material.
[0012] Traditional CrSi targets are mainly prepared by vacuum hot pressing and sintering. Although this method is highly efficient, it is easy to cause target cracking, low density, low purity, and the element ratio cannot be effectively controlled. If high-end settings or some extreme conditions are used to prepare products, although the product quality is high, it cannot be widely used in industrial production. To this end, the technical solution of the present invention is improved on the basis of the existing traditional process, starting from powder pretreatment, staged sintering and pressure program control to solve the technical bottleneck: in the front stage of the process, in order to ensure the uniform dispersion of the raw materials, the raw material powder is processed after mixing and its size is controlled to be less than 50μm, and the powder will not agglomerate or agglomerate. The subsequent hot pressing and sintering can ensure that the product has sufficient density and the element ratio control stability is high; subsequently, when sintering, a two-stage heating and insulation method is adopted, and the pressure relief threshold is lowered by simultaneously controlling the pressure relief, so that the mixed powder can be fully activated, and after the insulation is completed, pressurized insulation treatment is performed, so that the powder can obtain sufficient activation energy without applying excessive pressure, forming a high-density alloy phase, and the density and purity are much higher than the traditional simultaneous heating and pressurization process products
[0013] Preferably, in the mixed powder, the mass content of Si powder is 35.5-45.5wt%.
[0014] Preferably, the purity of the Si powder is ≥5N, and the purity of the Cr powder is ≥3N.
[0015] More preferably, the particle size D of the Si powder is v50 The particle size of Cr powder is 5~8μm. v50 30~45μm.
[0016] Preferably, in the step (1), the particle size of the grinding balls during ball milling is 10 to 20 mm, the ball-to-material ratio is 1:(2 to 3), the ball milling speed is 300 to 350 r / min, and the ball milling time is 24 to 28 h.
[0017] More preferably, the particle size Dv of the mixed powder is 50 ≤45μm.
[0018] The particle size and dispersibility of the mixed powder prepared by using different ball milling parameters are different. In the case where the size differences of Cr powder and Si powder in the mixed powder of the present invention are large, improper selection of ball milling parameters will lead to the size of the mixed powder after ball milling not meeting the standards, and may even cause partial agglomeration or agglomeration. Naturally, it is impossible to ensure that a higher density is achieved after subsequent sintering and hot pressing. However, the above-mentioned preferred ball milling parameters can achieve the expected effect.
[0019] Preferably, the pre-pressing treatment in step (2) is performed in a graphite mold.
[0020] More preferably, the set pressure during the pre-pressing treatment is 6 to 10 MPa, the pressure increase rate is 0.1 to 0.3 MPa / min, and the pre-pressing treatment time is 10 to 15 min.
[0021] The pre-pressing treatment can not only ensure the shape and size of the product, but also ensure the high density and better dispersion of the powders during the subsequent hot pressing and sintering process.
[0022] Preferably, in step (3), the pressure in the vacuum environment is less than 5 Pa.
[0023] Preferably, the ambient pressure after depressurization in steps (3) to (5) is 0.5 to -0.5 MPa.
[0024] By increasing the temperature in stages and setting up a real-time pressure relief process during the heating and insulation process, it can be ensured that the pressure in the product environment will not be too high instantly, so that when the powder forms the target material, it will not crack due to local excessive temperature while ensuring sufficient activation energy, and the flatness is high.
[0025] Another object of the present invention is to provide a CrSi target material prepared by the preparation method of the CrSi target material.
[0026] The purity of the CrSi target material prepared by the preparation method of the present invention can reach more than 99.95%, the density can reach more than 96.5%, the batch stability is high, and there is no cracking phenomenon and high flatness, which is very suitable for sputtering during vacuum coating.
[0027] The beneficial effect of the present invention is that the present invention provides an efficient and cost-effective method for preparing CrSi target materials. Through specific raw material mixing and special stage-programmed sintering and pressure control processes, the prepared products can meet the requirements of high density and high purity without relying on special equipment or harsh conditions. At the same time, the content of Cr-Si elements is highly controlled and stable, the comprehensive quality of the products is high, and industrial mass production can be realized.
[0028] Instruction Manual
[0029] Figure 1 This is a schematic diagram of a scanning electron microscope at a magnification of 200 times of the CrSi target obtained in Example 1 of the present invention.
[0030] Figure 2 This is a surface morphology of the CrSi target material obtained in Example 1 of the present invention. DETAILED DESCRIPTION
[0031] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments and comparative examples, the purpose of which is to understand the content of the present invention in detail, rather than to limit the present invention. All other embodiments obtained by those of ordinary skill in the art without making creative work premise belong to the protection scope of the present invention. The experimental reagents and instruments involved in the implementation of the present invention, unless otherwise specified, are all commonly used common reagents and instruments.
[0032] Example 1
[0033] An embodiment of a CrSi target material and a preparation method thereof according to the present invention comprises the following steps:
[0034] (1) Purity 5N, particle size D v50 6μm Si powder and purity 3N5, particle size D v50 Cr powder with a mass ratio of 40:60 wt % was mixed, and a mixed powder was obtained after ball milling in an argon protective atmosphere using a drum ball mill. The particle size of the mixed powder was Dv 50 The particle size of the ball mill used in the drum ball mill was 10 mm, the ball-to-material ratio was 1:2, the ball milling speed was 300 r / min, and the ball milling time was 24 h.
[0035] (2) placing the mixed powder in a graphite mold and paving it flat, then evacuating it to 0 MPa, increasing the pressure to 6 MPa at a rate of 0.2 MPa / min under a vacuum environment, performing a pre-pressing treatment and maintaining the pressure for 10 minutes, and releasing the pressure to 0 MPa to obtain a rough target blank;
[0036] (3) The rough target blank is heated to 700°C at a rate of 15°C / min in a vacuum environment of 0 MPa. When the ambient pressure reaches 6 MPa, the pressure is released at a rate of 2 MPa / min for 3 min until the ambient pressure reaches 0 MPa, and the pressure is released 5 times during the process;
[0037] (4) Then, the temperature was raised to 1250°C at a rate of 8°C / min, and when the ambient pressure reached 5 MPa, the pressure was released at a rate of 2 MPa / min for 2.5 min until the ambient pressure reached 0 MPa, during which the pressure was released 5 times;
[0038] (5) Keep the temperature at 1250°C for 60 min, and release the pressure at a rate of 1 MPa / min for 3 min until the ambient pressure reaches 0 MPa when the ambient pressure reaches 3 MPa, during which the pressure is released 5 times;
[0039] (6) After the heat preservation is completed, the pressure is increased to 35 MPa at a rate of 0.5 MPa / min and the heat and pressure are continued for 120 min, and then cooled to obtain the CrSi target.
[0040] Example 2
[0041] The embodiment of a CrSi target material and a preparation method thereof described in the present invention is different from the embodiment 1 only in that the step (1) is:
[0042] (1) Purity 5N, particle size D v50 6μm Si powder and purity 3N5, particle size D v50 Cr powder with a mass ratio of 40:60 wt % was mixed, and a mixed powder was obtained after ball milling in an argon protective atmosphere using a drum ball mill. The particle size of the mixed powder was Dv 50 The particle size of the balls used in the drum ball mill was 15 mm, the ball-to-material ratio was 1:2, the ball milling speed was 350 r / min, and the ball milling time was 28 h.
[0043] Example 3
[0044] The embodiment of a CrSi target material and a preparation method thereof described in the present invention is different from the embodiment 1 only in that the step (1) is:
[0045] ((1) Purity 5N, particle size D v50 6μm Si powder and purity 3N5, particle size D v50 Cr powder with a mass ratio of 40:60 wt % was mixed, and a mixed powder was obtained after ball milling in an argon protective atmosphere using a drum ball mill. The particle size of the mixed powder was Dv 50 The particle size of the balls used in the drum ball mill is 10 mm, the ball-to-material ratio is 1:3, the ball milling speed is 300 r / min, and the ball milling time is 24 h.
[0046] Example 4
[0047] An embodiment of a CrSi target material and a preparation method thereof according to the present invention comprises the following steps:
[0048] (1) Same as step (1) of Example 1;
[0049] (2) Same as step (2) of Example 1;
[0050] (3) The rough target blank is heated to 700° C. at a rate of 15° C. / min in a vacuum environment of 0 MPa. When the ambient pressure reaches 7 MPa, the pressure is released at a rate of 2 MPa / min for 3.5 min until the ambient pressure reaches 0 MPa, during which the pressure is released three times;
[0051] (4) Then, the temperature was raised to 1250°C at a rate of 8°C / min, and when the ambient pressure reached 6 MPa, the pressure was released at a rate of 2 MPa / min for 3 min until the ambient pressure reached 0 MPa, during which the pressure was released 4 times;
[0052] (5) Keep at 1250°C for 60 min, and when the ambient pressure reaches 4 MPa, release the pressure at a rate of 1 MPa / min for 4 min until the ambient pressure reaches 0 MPa, during which the pressure is released three times;
[0053] (6) After the heat preservation is completed, the pressure is increased to 35 MPa at a rate of 0.5 MPa / min and the heat and pressure are continued for 120 min, and then cooled to obtain the CrSi target.
[0054] Example 5
[0055] An embodiment of a CrSi target material and a preparation method thereof according to the present invention comprises the following steps:
[0056] (1) Same as step (1) of Example 1;
[0057] (2) Same as step (2) of Example 1;
[0058] (3) The rough target blank is heated to 700° C. at a rate of 15° C. / min in a vacuum environment of 0 MPa. When the ambient pressure reaches 8 MPa, the pressure is released at a rate of 2 MPa / min for 4 min until the ambient pressure reaches 0 MPa, during which the pressure is released twice;
[0059] (4) Then, the temperature was raised to 1250°C at a rate of 8°C / min, and when the ambient pressure reached 7 MPa, the pressure was released at a rate of 2 MPa / min for 3.5 min until the ambient pressure reached 0 MPa, during which the pressure was released twice;
[0060] (5) Keep the temperature at 1250°C for 60 min, and when the ambient pressure reaches 4 MPa, release the pressure at a rate of 1 MPa / min for 4 min until the ambient pressure reaches 0 MPa, with the pressure released twice during this period;
[0061] (6) After the heat preservation is completed, the pressure is increased to 35 MPa at a rate of 0.5 MPa / min and the heat and pressure are continued for 120 min, and then cooled to obtain the CrSi target.
[0062] Example 6
[0063] An embodiment of a CrSi target material and a preparation method thereof according to the present invention comprises the following steps:
[0064] (1) Same as step (1) of Example 1;
[0065] (2) Same as step (2) of Example 1;
[0066] (3) The rough target blank is heated to 700°C at a rate of 15°C / min in a vacuum environment of 0 MPa. When the ambient pressure reaches 10 MPa, the pressure is released at a rate of 2 MPa / min for 5 min until the ambient pressure reaches 0 MPa, during which the pressure is released twice;
[0067] (4) Then, the temperature was raised to 1250°C at a rate of 8°C / min, and when the ambient pressure reached 8 MPa, the pressure was released at a rate of 2 MPa / min for 4 min until the ambient pressure reached 0 MPa, during which the pressure was released once;
[0068] (5) Keep at 1250°C for 60 min, and when the ambient pressure reaches 5 MPa, release the pressure at a rate of 1 MPa / min for 5 min until the ambient pressure reaches 0 MPa, with one pressure release during this period;
[0069] (6) After the heat preservation is completed, the pressure is increased to 35 MPa at a rate of 0.5 MPa / min and the heat and pressure are continued for 120 min, and then cooled to obtain the CrSi target.
[0070] Comparative Example 1
[0071] An embodiment of a CrSi target material and a method for preparing the same differs from embodiment 1 only in that step (1) is:
[0072] (1) Purity 5N, particle size D v50 6μm Si powder and purity 3N5, particle size D v50 Cr powder with a mass ratio of 40:60 wt % was mixed, and a mixed powder was obtained after ball milling in an argon protective atmosphere using a drum ball mill. The particle size of the mixed powder was Dv 50 The particle size of the balls used in the drum ball mill was 15 mm, the ball-to-material ratio was 1:3, the ball milling speed was 350 r / min, and the ball milling time was 28 h.
[0073] Comparative Example 2
[0074] An embodiment of a CrSi target material and a method for preparing the same differs from embodiment 1 only in that step (1) is:
[0075] (1) Purity 5N, particle size D v506μm Si powder and purity 3N5, particle size D v50 Cr powder with a mass ratio of 40:60 wt % was mixed, and a mixed powder was obtained after ball milling in an argon protective atmosphere using a drum ball mill. The particle size of the mixed powder was Dv 50 The particle size of the balls used in the drum ball mill was 10 mm, the ball-to-material ratio was 1:4, the milling speed was 300 r / min, and the milling time was 24 h.
[0076] Comparative Example 3
[0077] An embodiment of a CrSi target material and a method for preparing the same differs from embodiment 1 only in that step (1) is:
[0078] (1) Purity 5N, particle size D v50 40μm Si powder and purity 3N5, particle size D v50 6 μm Cr powder was mixed in a mass ratio of (40:60wt%), and ball milled in a drum ball mill under an argon protective atmosphere to obtain a mixed powder. The particle size of the mixed powder was Dv 50 The particle size of the balls used in the drum ball mill was 15 mm, the ball-to-material ratio was 1:4, the ball milling speed was 350 r / min, and the ball milling time was 28 h.
[0079] Comparative Example 4
[0080] An embodiment of a CrSi target material and a preparation method thereof, the preparation method comprising the following steps:
[0081] (1) Same as step (1) of Example 1;
[0082] (2) Same as step (2) of Example 1;
[0083] (3) heating the rough target blank to 700° C. at a rate of 15° C. / min in a vacuum environment of 0 MPa without depressurizing the target blank;
[0084] (4) heating the temperature to 1250°C at a rate of 8°C / min for a second time without depressurizing the temperature;
[0085] (5) Keep at 1250°C for 60 min without releasing the pressure;
[0086] (6) After the heat preservation is completed, the pressure is increased to 35 MPa at a rate of 0.5 MPa / min and the heat and pressure are continued for 120 min, and then cooled to obtain the CrSi target.
[0087] Comparative Example 5
[0088] An embodiment of a CrSi target material and a preparation method thereof, the preparation method comprising the following steps:
[0089] (1) Same as step (1) of Example 1;
[0090] (2) Same as step (2) of Example 1;
[0091] (3) The rough target blank was heated to 1250° C. at a rate of 15° C. / min in a vacuum environment of 0 MPa, and when the ambient pressure reached 6 MPa, the pressure was released at a rate of 2 MPa / min for 3 min until the ambient pressure reached 0 MPa, during which the pressure was released 8 times;
[0092] (4) Keep the temperature at 1250°C for 60 min, and release the pressure at a rate of 1 MPa / min for 3 min until the ambient pressure reaches 0 MPa when the ambient pressure reaches 3 MPa, during which the pressure is released 5 times;
[0093] (5) After the heat preservation is completed, the pressure is increased to 35 MPa at a rate of 0.5 MPa / min and the heat and pressure are continued for 120 minutes, and then cooled to obtain the CrSi target material.
[0094] Comparative Example 6
[0095] An embodiment of a CrSi target material and a preparation method thereof, the preparation method comprising the following steps:
[0096] (1) Same as step (1) of Example 1;
[0097] (2) Same as step (2) of Example 1;
[0098] (3) The rough target blank is heated to 700°C at a rate of 15°C / min in a vacuum environment of 0 MPa. When the ambient pressure reaches 6 MPa, the pressure is released at a rate of 2 MPa / min for 3 min until the ambient pressure reaches 0 MPa, and the pressure is released 5 times during the process;
[0099] (4) Then, the temperature was raised to 1250° C. at a rate of 8° C. / min, and the pressure was increased to 35 MPa at a rate of 0.5 MPa / min. The temperature and pressure were maintained for 180 min, and the mixture was cooled to obtain the CrSi target.
[0100] Effect Example 1
[0101] In order to verify the effect of the ball milling process of the present invention, the mixed powders obtained in Examples 1 to 3 and Comparative Examples 1 to 3 were observed to confirm whether there was agglomeration or agglomeration. The results are shown in Table 1.
[0102] Table 1
[0103] product Product Status Example 1 No agglomeration or caking Example 2 No agglomeration or caking Example 3 Partial agglomeration, no agglomeration Comparative Example 1 Agglomeration and no agglomeration Comparative Example 2 Agglomeration and agglomeration Comparative Example 3 Agglomeration and agglomeration
[0104] It can be seen from Table 1 that the particle dispersion of the precursor mixed powders prepared by different ball milling processes is different. Some processes may cause agglomeration and agglomeration, which makes the powder size larger, which is not conducive to the subsequent preparation of high-density target materials.
[0105] Effect Example 2
[0106] In order to verify the performance effect of the product described in the present invention, the target material products prepared in each embodiment and comparative example were tested for purity and Si element content, and then the density of the product was tested by the drainage method, and the visual method was used to confirm whether there were defects or cracks on the surface of the product. Ten parallel samples were taken for the test, and the test results were averaged. If a parallel sample had defects or cracks during the appearance test, it was directly recorded as the result of the corresponding embodiment or comparative example product, as shown in Table 2.
[0107] Table 2
[0108] product purity(%) Density(%) Si content (wt%) Appearance Example 1 >99.95% 99.8 40.12 No flaws, no cracks Example 2 >99.95% 99.6 39.39 No flaws, no cracks Example 3 >99.95% 99.2 40.34 No flaws, no cracks Example 4 >99.95% 98.7 38.98 No flaws, no cracks Example 5 >99.95% 97.8 40.45 No flaws, no cracks Example 6 >99.95% 96.6 39.68 No flaws, no cracks Comparative Example 1 >99.95% 95.3 40.32 No flaws, no cracks Comparative Example 2 <99.95% 94.8 39.97 Defective, no cracks Comparative Example 3 <99.95% 93.9 39.41 Defective, no cracks Comparative Example 4 <99.95% 97.5 40.48 Target cracking Comparative Example 5 <99.95% 96.1 40.16 Target cracking Comparative Example 6 <99.95% 92.6 39.43 Defective, no cracks
[0109] It can be seen from Table 2 that the CrSi target material products prepared in the embodiments of the present invention have high batch stability, the purity can reach more than 99.95%, and the density can reach more than 96.5%, the highest is close to 100%, the product surface is flat and flawless, and there is no cracking. Among them, the quality of the product obtained in Example 1 is the best. The product is observed by scanning electron microscope and visual observation. Figure 1 and 2 As shown, the product has a smooth macroscopic surface and uniform morphology at the microscopic level, which fully demonstrates that the raw materials Cr and Si have fully formed a uniform alloy phase. According to the comparison between Example 1 and Examples 4 to 6, it can be seen that in the sintering hot pressing process of the present invention, the real-time program pressure relief has a certain relationship with the quality of the product. When the pressure relief threshold is higher, of course, the number of pressure relief times is less, but relatively speaking, the quality of the product is also reduced to a certain extent.
[0110] It can be seen from the products of Examples 1 to 3 and Comparative Examples 1 to 3 that if the quality of the mixed powder prepared in the early stage is poor, the density and other properties of the target material finally prepared will inevitably fail to meet the standards. Therefore, in addition to the hot pressing and sintering process, the early powder processing is also the key to the quality of the products described in the present invention meeting the standards.
[0111] On the other hand, the process described in Comparative Example 4 did not perform any pressure relief operation during the heating period, and the temperature field and pressure during the heating process were unstable, which would eventually cause cracks in the target blank of the product; although the process described in Comparative Example 5 implemented a pressure relief step, a one-step heating method was used during the heating process. This process made it impossible for the powder to be fully and evenly activated, and the quality of the product could not meet expectations, and cracks in the target blank also occurred; Comparative Example 6 is an existing traditional process for preparing target materials by simultaneously increasing temperature and pressure. Even if the same final pressure is applied in such a process, the activation energy obtained by the product is still insufficient, and the density of the product is low.
[0112] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A method for preparing a CrSi target, characterized in that: The following steps are involved: (1) Si powder and Cr powder are mixed and ball-milled in a protective atmosphere to obtain a mixed powder having a particle size Dv 50 ≤50μm; (2) pre-pressing the mixed powder in a vacuum environment to obtain a rough target blank; (3) heating the rough target blank to 600-800° C. at a rate of 15-20° C. / min in a vacuum environment, and when the ambient pressure reaches 6-10 MPa, releasing the pressure at a rate of 1.5-3 MPa / min for 3-6 min; (4) then heating the temperature to 1150-1250°C at a rate of 8-10°C / min for a second time, and simultaneously releasing the pressure at a rate of 1-2MPa / min for 2-5min when the ambient pressure reaches 5-8MPa; (5) Keep the temperature at 1150-1250°C for 30-60 min, and release the pressure at a rate of 0.5-1 MPa / min for 3-6 min when the ambient pressure reaches 3-5 MPa; (6) After the heat preservation is completed, the pressure is increased to 35-40 MPa at a rate of 0.3-0.5 MPa / min and the heat and pressure are continued for 90-150 minutes, and then cooled to obtain the CrSi target material.
2. The method for preparing a CrSi target according to claim 1, characterized in that: In the mixed powder, the mass content of Si powder is 35.5-45.5wt%.
3. The method for preparing a CrSi target according to claim 1, characterized in that: The particle size D of the Si powder v50 The particle size of Cr powder is 5~8μm. v50 30~45μm.
4. The method for preparing a CrSi target material according to claim 1, characterized in that: In the step (1), the particle size of the grinding balls during ball milling is 10 to 20 mm, the ball-to-material ratio is 1:(2 to 3), the ball milling speed is 300 to 350 r / min, and the ball milling time is 24 to 28 h.
5. The method for preparing a CrSi target material according to claim 1, characterized in that: The particle size Dv of the mixed powder 50 ≤45μm.
6. The method for preparing a CrSi target material according to claim 1, characterized in that: The set pressure during the pre-pressing treatment is 6-10 MPa, the pressure increase rate is 0.1-0.3 MPa / min, and the pre-pressing treatment time is 10-15 minutes.
7. The method for preparing a CrSi target material according to claim 1, characterized in that: In the step (3), the pressure in the vacuum environment is less than 5 Pa.
8. The method for preparing a CrSi target material according to claim 1, characterized in that: The ambient pressure after depressurization in steps (3) to (5) is 0.5 to -0.5 MPa.