Aluminum-steel dissimilar metal based on laser cladding copper intermediate layer and welding method of aluminum-steel dissimilar metal
By using laser clad copper intermediate layer during welding of aluminum alloy and steel, the problem of the generation of hard and brittle phase intermetallic compounds in welding of aluminum alloy and steel is solved, the mechanical properties and forming quality of the welded joints are improved, and the heat is avoided Cracking generation.
Patent Information
- Application Number
- CN202411069276.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
During the welding process, aluminum alloy and steel are prone to defects such as pores, cracks and depressions due to differences in crystal structure, thermal physical properties and metallurgical compatibility. The hard and brittle phase intermetallic compounds affect the mechanical properties of the welded joints and are difficult to control well. Weld forming.
Laser cladding pure copper is used as the intermediate layer. After pretreating the steel plate substrate and the aluminum alloy plate substrate, the copper layer is laser clad on the steel plate and docked in the copper alloy back blowing device for laser welding. Welding conditions such as power, scanning speed and protective gas flow to prepare aluminum steel heterogeneous metal based on laser clad copper intermediate layer.
It effectively reduces the formation of Fe-Al intermetallic compounds, improves the weld forming quality, avoids thermal cracks, and significantly improves the mechanical properties of the welded joints, especially the tensile strength.
Smart Images

Figure CN118875540A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal material welding technology, and specifically relates to aluminum-steel dissimilar metals based on laser cladding of a copper intermediate layer and a welding method thereof. Background Art
[0002] Aluminum alloy and steel are widely used metals in today's industrial production. Both have excellent performance. Therefore, more and more fields combine the advantages of the two to optimize and upgrade products. In the field of automobile manufacturing, with the increasing tension of the world's energy supply and the continuous improvement of environmental protection requirements, people's economic investment and research efforts in energy conservation and emission reduction are increasing. Reducing the weight of the car while meeting the requirements of automobile mechanical performance and safety, and replacing the traditional steel structure car body with lightweight metal is an effective means to achieve automobile lightweight, energy conservation and emission reduction. In order to reduce the weight of the car body while ensuring the strength and safety of the car body, high-strength steel and aluminum alloy and their dissimilar materials welded components are increasingly widely used in the field of automobile manufacturing.
[0003] Although the application prospects of aluminum-steel welding are very broad, there are many problems in the welding process of aluminum alloy and steel due to the differences in crystal structure, thermophysical properties and metallurgical compatibility between the two. For example, the aluminum-steel welding process is unstable, and defects such as pores, cracks and depressions are easily generated after welding. In particular, the hard and brittle phase intermetallic compounds generated during the welding process greatly affect the mechanical properties of the welded joint. How to control the formation of a good weld is a difficulty in aluminum-steel welding. Therefore, it is necessary to study the aluminum / steel welding process in order to control the formation and growth of aluminum-steel intermetallic compounds.
[0004] In the existing research, in order to reduce the formation of hard and brittle intermetallic compounds in the laser welding process of aluminum and steel, Cu foil is generally added as an intermediate layer for laser welding. However, the thermal matching between Cu foil and aluminum alloy base material is not good, and thermal crack defects are easily generated, which seriously reduces the forming quality and mechanical properties of the welded joint. Summary of the invention
[0005] In order to overcome the shortcomings and disadvantages of the prior art, the primary purpose of the present invention is to provide a welding method for aluminum-steel dissimilar metals based on laser cladding of a copper intermediate layer. The welding method can not only reduce the formation of hard and brittle intermetallic compounds between aluminum and steel during laser welding, but also ensure the quality of the weld formation of the aluminum-steel joint and improve the mechanical properties of the welded joint.
[0006] The second object of the present invention is to provide an aluminum-steel dissimilar metal based on laser cladding of a copper intermediate layer.
[0007] The primary purpose of the present invention is achieved through the following technical solutions:
[0008] A method for welding dissimilar aluminum and steel metals based on laser cladding of a copper intermediate layer comprises the following steps:
[0009] (1) Pre-treating the steel plate substrate and aluminum alloy plate substrate to be welded;
[0010] (2) Laser cladding of pure copper as an intermediate layer on a steel substrate;
[0011] (3) The steel plate substrate to be welded with the clad copper intermediate layer and the aluminum plate substrate to be welded are butt-jointed and clamped in a copper alloy back-blowing device;
[0012] (4) using a laser welding method to weld the steel plate substrate and the aluminum alloy plate substrate to prepare an aluminum-steel dissimilar metal based on a laser cladding copper intermediate layer;
[0013] The laser cladding conditions in step (2) are: laser power 1200-1600 W, scanning speed 30-60 mm / s, powder feeding rate 14-18 g / min, spot diameter 2-2.5 mm;
[0014] The laser welding conditions in step (4) are: power 1300-1600 W, welding speed 30-60 mm / s, defocusing amount -2-+2 mm, front shielding gas flow rate 15-20 L / min, and back shielding gas flow rate 10-15 L / min.
[0015] Preferably, the pretreatment in step (1) is to use 600# sandpaper to polish the steel plate substrate and the aluminum alloy plate substrate respectively, then place them in an acetone solution and use an ultrasonic instrument to clean them, and then place them in a dryer to dry them.
[0016] Preferably, the steel plate substrate in step (1) is Q345 low alloy structural steel, and the aluminum alloy plate substrate is 7075-T6 super hard aluminum alloy.
[0017] Preferably, the laser cladding in step (2) adopts a coaxial powder feeding mode, the purity of the pure copper powder is above 99.8%, and the spherical particle size is 80-125 μm. Preferably, the laser cladding in step (2) is a single-pass cladding.
[0018] Preferably, the laser welding in step (4) is single-pass welding.
[0019] Preferably, during the laser welding in step (4), the laser beam deviates 0.1 to 0.3 mm toward the steel side. Preferably, the shielding gas in step (4) is argon gas with a purity of 99.999%.
[0020] Preferably, during the laser welding in step (4), the laser beam deviates toward the steel side by 0.1 to 0.3 mm.
[0021] The second object of the present invention is achieved by the following technical solutions:
[0022] An aluminum-steel dissimilar metal based on laser cladding of a copper intermediate layer is prepared by the above welding method.
[0023] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0024] (1) The present invention adds a copper intermediate layer by laser cladding, which effectively hinders the formation of Fe-Al intermetallic compounds in the subsequent welding process of aluminum alloy plates and steel plates, and significantly reduces the thickness of intermetallic compounds (IMC) at the interface. The weld is beautifully formed without defects such as spatter and cracks, and the mechanical properties of the joint are significantly improved.
[0025] (2) Compared with the prior art using a single Cu foil intermediate layer, the copper cladding layer of the present invention has better thermal matching performance, can more effectively reduce thermal stress and deformation of welding materials, and effectively avoid the generation of thermal cracks.
[0026] (3) The process of the present invention is simple and does not require expensive equipment or complicated procedures. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is a schematic diagram of the laser cladding copper layer on the steel plate described in Example 1;
[0028] Figure 2 This is a schematic diagram of the laser welding of aluminum-steel plates described in Comparative Example 1, wherein 1-laser beam, 2-powder feeding device, 3-copper powder, 4-aluminum alloy plate substrate, 5-clad copper intermediate layer, 6-steel plate substrate. DETAILED DESCRIPTION
[0029] The present invention is further described in detail below in conjunction with specific embodiments, but the embodiments of the present invention are not limited thereto. The materials used in the examples of the present invention can be purchased commercially. The present invention is further described below in conjunction with the accompanying drawings and embodiments: Figure 1 to Figure 2 .
[0030] The present invention provides a welding method of aluminum-steel dissimilar metals based on laser cladding of a copper intermediate layer, comprising the following steps:
[0031] (1) Pre-treating the steel plate substrate and aluminum alloy plate substrate to be welded;
[0032] (2) Laser cladding of pure copper as an intermediate layer on a steel substrate;
[0033] (3) The steel plate substrate to be welded with the clad copper intermediate layer and the aluminum plate substrate to be welded are butt-jointed and clamped in a copper alloy back-blowing device;
[0034] (4) The steel plate substrate and the aluminum alloy plate substrate to be welded are welded by laser welding to prepare aluminum-steel dissimilar metals based on laser cladding copper intermediate layer.
[0035] In the present invention, the steel plate substrate is preferably Q345 low alloy structural steel; the aluminum alloy plate substrate is preferably 7075-T6 superhard aluminum alloy. The present invention has no special requirements on the specific composition of the Q345 low alloy structural steel and the 7075-T6 superhard aluminum alloy, and the Q345 low alloy structural steel and the 7075-T6 superhard aluminum alloy commonly used in engineering can be used.
[0036] In an embodiment of the present invention, the element composition of the Q345 low alloy structural steel is, in terms of mass percentage (%), C 0.15, Si 0.45, Mn 1.5, P 0.03, S 0.03, V 0.13, Nb 0.07, Ti 0.19, and Fe balance; the element composition of the 7075-T6 super hard aluminum alloy is: Zn 5.54, Mg 2.43, Cu 1.30, Fe 0.05, Cr 0.10, Ti0.19, Si 0.25, Mn 0.05, Ni 0.04, and Al balance.
[0037] In the present invention, before the laser cladding and laser welding, it is preferred that the steel material and the aluminum alloy material be pretreated; the pretreatment preferably includes: using 600# sandpaper to polish the steel plate and the aluminum alloy plate respectively, and then placing them in an acetone solution and cleaning them using an ultrasonic instrument, and then placing them in a dryer for drying.
[0038] In the present invention, the laser cladding position is the contact surface between the steel material and the aluminum alloy. Preferably, a synchronous powder feeding mode is adopted, and the purity of the cladding copper powder is 99.8%, and the spherical particle size is between 80 and 125 μm.
[0039] Example 1
[0040] The parent materials are 50mm×100mm×2mm Q345 low alloy structural steel and 50mm×100mm×2mm 7075-T6 super-hard aluminum alloy. The parent materials are placed in an acetone solution and cleaned with an ultrasonic instrument, and then placed in a dryer for drying. The copper layer is laser clad on the steel plate, with a single pass cladding. The laser cladding process parameters are: laser power 1500W, scanning speed 50mm / s, powder feeding rate 15g / min, and spot diameter 2mm. After cladding, the steel plate is butt-clamped with the aluminum alloy for laser welding. The process parameters of single-pass laser welding are: the laser beam deviates 0.2mm to the steel side, the power is 1500W, the welding speed is 30mm / s, the defocus is 0mm, the front protective gas flow is 15L / min, and the back protective gas flow is 10L / min. The tensile strength is tested by a universal tensile machine to reach 134Mpa.
[0041] Example 2
[0042] The parent materials are 50mm×100mm×2mm Q345 low alloy structural steel and 50mm×100mm×2mm 7075-T6 super-hard aluminum alloy. The parent materials are placed in an acetone solution and cleaned with an ultrasonic instrument, and then placed in a dryer for drying. The copper layer is laser clad on the steel plate, with a single pass cladding. The laser cladding process parameters are: laser power 1500W, scanning speed 50mm / s, powder feeding rate 15g / min, and spot diameter 2mm. After cladding, the steel plate is butt-clamped with the aluminum alloy for laser welding. The process parameters of single-pass laser welding are: the laser beam deviates 0.2mm to the steel side, the power is 1600W, the welding speed is 30mm / s, the defocus is 0mm, the front protective gas flow is 15L / min, and the back protective gas flow is 10L / min. The tensile strength is tested by a universal tensile machine to reach 129Mpa.
[0043] Example 3
[0044] The parent materials are 50mm×100mm×2mm Q345 low alloy structural steel and 50mm×100mm×2mm 7075-T6 super-hard aluminum alloy. The parent materials are placed in acetone solution and cleaned with an ultrasonic instrument, and then placed in a dryer for drying. The copper layer is laser clad on the steel plate, with a single pass cladding. The laser cladding process parameters are: laser power 1500W, scanning speed 50mm / s, powder feeding rate 15g / min, and spot diameter 2mm. After cladding, the steel plate is butt-clamped with the aluminum alloy for laser welding. The process parameters of single-pass laser welding are: the laser beam deviates 0.2mm to the steel side, the power is 1400W, the welding speed is 30mm / s, the defocus is 0mm, the front protective gas flow is 15L / min, and the back protective gas flow is 10L / min. The tensile strength is tested by a universal tensile machine to reach 124Mpa.
[0045] Comparative Example 1
[0046] The parent materials are 50mm×100mm×2mm Q345 low alloy structural steel and 50mm×100mm×2mm 7075-T6 super-hard aluminum alloy. The parent materials are placed in an acetone solution and cleaned using an ultrasonic instrument, and then placed in a dryer for drying. The steel plate and the aluminum alloy are directly butt-clamped for laser welding. The process parameters of single-pass laser welding are: the laser beam deviates 0.2mm to the steel side, the power is 1500W, the welding speed is 30mm / s, the defocus is 0mm, the front protective gas flow is 15L / min, and the back protective gas flow is 10L / min. The tensile strength is tested using a universal tensile machine and reaches 102Mpa.
[0047] Comparative Example 2
[0048] The parent materials are 50mm×100mm×2mm Q345 low alloy structural steel and 50mm×100mm×2mm 7075-T6 super-hard aluminum alloy. The parent materials are placed in an acetone solution and cleaned with an ultrasonic instrument, and then placed in a dryer for drying. A pure nickel layer is laser clad on the steel plate, with a single pass cladding. The laser cladding process parameters are: laser power 1500W, scanning speed 50mm / s, powder feeding rate 15g / min, and spot diameter 2mm. After cladding, the steel plate is butt-clamped with the aluminum alloy for laser welding. The process parameters for single-pass laser welding are: the laser beam deviates 0.2mm to the steel side, the power is 1500W, the welding speed is 30mm / s, the defocus is 0mm, the front protective gas flow is 15L / min, and the back protective gas flow is 10L / min. The tensile strength is tested by a universal tensile machine to reach 112Mpa.
[0049] Based on the data of the above Examples 1 to 3 and Comparative Examples 1 to 2, the present invention uses a laser cladding method to clad a pure copper layer on a steel plate substrate, and then connects the Q345 low-alloy structural steel and the 7075-T6 super-hard aluminum alloy, and uses the clad copper layer as an intermediate layer for laser welding. The present invention can effectively reduce thermal stress and prevent the occurrence of thermal cracks during the welding process. The copper cladding layer serves as a buffer zone, has good thermal conductivity and plasticity, and is completely melted during welding, which effectively reduces the mutual diffusion of Fe and Al elements, inhibits the formation of Fe-Al intermetallic compounds in the aluminum / steel laser welded joint, and improves the tensile strength of the joint.
[0050] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A welding method for aluminum and steel dissimilar metals based on laser cladding of copper intermediate layer, It is characterized in that The following steps are included: (1) Pre-treating the steel plate substrate and aluminum alloy plate substrate to be welded; (2) Laser cladding pure copper on a steel substrate as an intermediate layer; (3) butting and clamping the steel plate substrate to be welded with the clad copper intermediate layer and the aluminum plate substrate to be welded in a copper alloy back blowing device; (4) using a laser welding method to weld the steel plate substrate and the aluminum alloy plate substrate to prepare aluminum-steel dissimilar metals based on a laser cladding copper intermediate layer; The laser cladding conditions in step (2) are: laser power 1200-1600 W, scanning speed 30-60 mm / s, powder feeding rate 14-18 g / min, spot diameter 2-2.5 mm; The laser welding conditions in step (4) are: power 1300-1600 W, welding speed 30-60 mm / s, defocusing amount -2-+2 mm, front shielding gas flow rate 15-20 L / min, and back shielding gas flow rate 10-15 L / min.
2. The aluminum-steel dissimilar metal welding method based on laser cladding of a copper intermediate layer according to claim 1, It is characterized in that The pretreatment in step (1) is to use 600# sandpaper to polish the steel plate substrate and the aluminum alloy plate substrate respectively, then put them in an acetone solution and use an ultrasonic instrument to clean them, and then put them in a dryer to dry.
3. The aluminum-steel dissimilar metal welding method based on laser cladding of a copper intermediate layer according to claim 1, It is characterized in that The steel plate substrate in step (1) is Q345 low alloy structural steel, and the aluminum alloy plate substrate is 7075-T6 super hard aluminum alloy.
4. The aluminum-steel dissimilar metal welding method based on laser cladding of a copper intermediate layer according to claim 1, It is characterized in that The laser cladding in step (2) adopts a coaxial powder feeding mode, the purity of the pure copper powder is above 99.8%, and the spherical particle size is 80 to 125 μm.
5. The aluminum-steel dissimilar metal welding method based on laser cladding of a copper intermediate layer according to claim 1, It is characterized in that The laser cladding in step (2) is a single-pass cladding.
6. The aluminum-steel dissimilar metal welding method based on laser cladding of a copper intermediate layer according to claim 1, It is characterized in that The laser welding in step (4) is single-pass welding.
7. The aluminum-steel dissimilar metal welding method based on laser cladding of a copper intermediate layer according to claim 1, It is characterized in that During the laser welding in step (4), the laser beam deviates toward the steel side by 0.1 to 0.3 mm.
8. The aluminum-steel dissimilar metal welding method based on laser cladding of a copper intermediate layer according to claim 1, It is characterized in that The protective gas in step (4) is argon gas with a purity of 99.999%.
9. The aluminum-steel dissimilar metal welding method based on laser cladding of a copper intermediate layer according to claim 1, It is characterized in that During the laser welding in step (4), the laser beam deviates toward the steel side by 0.1 to 0.3 mm.
10. A dissimilar aluminum-steel metal based on laser cladding copper intermediate layer, It is characterized in that Prepared by the welding method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Aluminum-steel dissimilar material laser welding method
CN112894132A
High-strength steel-aluminum alloy dissimilar metal plasma arc welding method assisted by transition layer
CN113510354A
Aluminum / steel laser welding method based on in-situ synthesis of AlXCoCrFeNi high-entropy alloy interlayer
CN114951997A
Optimization method for high entropy of welding seam of titanium steel metal connecting piece
CN116329755A
Steel-aluminum dissimilar metal laser-electric arc hybrid welding method for preparing pure nickel transition layer based on laser cladding
CN117600657A
Cited By
Method for preparing copper-aluminum layered composite board by introducing laser into middle layer
CN120169868A
Self-lubricating thrust knuckle bearing and preparation method thereof
CN120868132A