Forming process of duralumin square shell cartridge, upsetting flange die and using method of upsetting flange die
Through multi-step stretching and annealing process combined with backextrusion forming technology and upsetting flange mold, the problems of surface oxidation, material waste and processing difficulties in traditional hard aluminum square shell processing are solved, and high precision and high strength Forming meets the tensile strength requirements of interfering cartridges, improving production efficiency and market competitiveness.
Patent Information
- Application Number
- CN202411047467.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-01
AI Technical Summary
The processing technology of traditional hard aluminum square shell cartridges has problems such as surface oxidation, material waste, difficult processing and low tensile strength. Especially when processing thin-wall shells and deep holes, wall thickness deviation is difficult to guarantee, resulting in high costs. and the quality is not up to standard.
Using multi-step stretching and annealing technology combined with backextrusion forming technology, the combination of precision cutting, shaping, backextrusion, stretching, solid solution heat treatment and upsetting flange mold can achieve high-precision and high-strength hard aluminum squares. The shell is formed and the finished product size and performance is ensured through quality inspection.
It realizes high-precision and high-strength forming of hard aluminum square shells, reduces material waste and processing difficulty, improves production efficiency and market competitiveness, and meets the tensile strength and elongation requirements of interfering cartridges.
Smart Images

Figure CN118875656A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of cartridge molding technology and mold technology, and in particular to a duralumin square shell cartridge molding technology, an upsetting flange mold and a use method thereof. Background Art
[0002] The hard aluminum square shell has a small density and high tensile strength, which plays a very important role in the military field, especially in the manufacture of jamming cartridges. The forging technology solution of the traditional processing technology and the hot extrusion forming of the aluminum alloy cartridge are prone to surface oxidation during the heating process of the billet, which affects the quality of the workpiece after forming and the life of the mold; the surface quality after hot extrusion cannot meet the requirements, and additional machining is required to meet the surface roughness requirements; in the machining process, for the thin-walled shell, there are not only problems such as difficult clamping, easy deformation, and material waste, but also the milling of rectangular thin-walled parts is difficult and the processing cost is high. In addition, the inner hole and outer circle of the milling process have obvious microscopic peaks and troughs, which will reduce the tensile strength, especially in the case of deep hole thin walls such as 1.1mm thick and 188mm deep, the wall thickness deviation after processing is difficult to guarantee. Summary of the invention
[0003] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a hard aluminum square shell cartridge forming process and a mold and a mold use method, which can achieve high-precision and high-strength hard aluminum square shell forming, while solving the problems of material waste and high processing difficulty in traditional processing technology.
[0004] The technical solution adopted by the present invention is: A forming process of a hard aluminum square shell cartridge, the specific process is: rectangular material cutting → shaping → first annealing → shot blasting → lubrication → reverse extrusion → second annealing → first stretching → third annealing → second stretching → solid solution heat treatment → flange upsetting → milling of both end surfaces → quality inspection → finished product; in the shaping and reverse extrusion steps, both are performed on a press using a mold; Rectangular material cutting: Select rectangular aluminum alloy profiles, determine the cutting height of the rectangular profiles according to the required weight of the forgings, use precision cutting equipment for cutting, and control the height tolerance to ±0.1㎜ to ensure the accuracy of material size and reduce material waste; Shaping: The cut aluminum alloy material is shaped in the die. This process is carried out on a press. After shaping, the outer contour of the blank is consistent with the shape of the reverse extrusion die, preparing for subsequent processes. The shaping pressure is 100 tons, and zinc stearate powder is used for lubrication. First annealing: Annealing is performed to soften the material, reduce internal stress, improve the plasticity of the material, and provide better forming conditions for reverse extrusion; the annealing requirements are to heat up to 410°C, keep at 410°C for 3 hours, then cool to 150°C with the furnace and air cool out of the furnace. After annealing, the hardness of the billet is below 60HB; Shot blasting: steel shot diameter 0.5mm, shot blasting time 15 minutes; Lubrication: Phosphorus saponification treatment is performed on the surface of the blank; the lubricant on the surface of the blank can reduce friction and heat generation during cold extrusion, extend the life of the die, and improve the surface quality of the blank formed part; Back extrusion: Use a die to apply high pressure to the blank at room temperature to form a square shell forging. According to the material properties, the back extrusion pressure is controlled to 125 tons, the deformation is 75-76%, and the wall thickness deviation is controlled within 0.1mm to ensure the forming quality; Second annealing: Annealing requires heating to 410℃, keeping at 410℃ for 3 hours, then cooling to 150℃ with the furnace and air cooling. After annealing, the hardness of the square shell forging is below 60HB; annealing after reverse extrusion helps to eliminate the residual stress generated in the previous extrusion process, so that the material has continuous plastic deformation ability and prepares for the stretching process; after annealing, the plastic deformation part of the square shell forging will restore the plastic ability, effectively reducing the internal stress of the square shell forging; First stretching: The square shell forging is stretched for the first time on the stretching hydraulic press, and the stretching coefficient is 0.71; the stretching process further thins the wall thickness of the square shell forging and improves the uniformity of the material; Third annealing: Annealing requires heating to 410℃, keeping at 410℃ for 3 hours, then cooling to 150℃ with the furnace and air cooling; after annealing, the plastically deformed part of the square shell forging will recover its plasticity, further reducing the internal stress of the square shell forging; Second stretching: The square shell forging is stretched for the second time on the stretching hydraulic press, with a stretching coefficient of 0.71. After stretching, the wall thickness of the square shell forging reaches the finished product size requirements; Solution heat treatment: Solution temperature is 495℃, keep warm for 0.5 hours and then cool by quenching. Place the square shell forging with the hole facing upward and put it into water vertically. Solution heat treatment dissolves the strengthening phase in the alloy, improves the plasticity of the alloy, and provides better material properties for the subsequent flange upsetting process. Upsetting flange: After the second stretching is completed, the upsetting operation is completed within 6 hours, and the flange part of the square shell forging is formed by the upsetting flange die; the force and shape are precisely controlled by the upsetting flange die to ensure the dimensional accuracy and integrity of the flange; Milling of both end faces: CNC machining or precision turning is used to finish the both end faces of the formed square shell forging to achieve the required dimensional accuracy and surface finish of the finished product; Quality inspection: Quality inspection is carried out after each key process to ensure that the product size, shape and performance meet the design requirements and the final product.
[0005] A hard aluminum square shell cartridge upsetting flange die, comprising an upper male die assembly and a lower female die assembly; The upper punch assembly comprises an upper die flange plate, an upper die pad, an upper die mounting plate, an upper die outer ring and an upper punch; a U-shaped groove for connecting with the movable crossbeam plate of the press is evenly arranged on the circumference of the upper die flange plate, a step groove is arranged at the center of the lower surface, and a circle of mounting holes is evenly arranged around the step groove; a step through hole is arranged at the center of the upper die outer ring, the upper die pad is arranged in the upper part of the step through hole, the upper punch is arranged in the lower part of the step through hole, and a circular boss protruding from the lower surface of the upper die outer ring is arranged at the center of the lower end surface of the upper punch; a circle of mounting steps is arranged on the outer edge of the upper end of the upper die outer ring, and the upper end of the upper die outer ring is located in the step groove in the center of the upper die flange plate; the upper die mounting plate is matched with the upper die outer ring mounting step and is arranged on the outside of the upper die outer ring, and holes corresponding to the mounting holes on the lower surface of the upper die flange plate are arranged on the upper die mounting plate, and bolts pass through the corresponding holes and mounting holes respectively to connect the upper die mounting plate and the upper die flange plate; The lower die assembly comprises a large die base, a lower die pad, a lower die outer ring, upper and lower die positioning rings, upper and lower die positioning ring hard rings, a clamping flange, a long bolt, a lower die, an upper die, a lower die mandrel, a push piece and a push rod; the large die base is a cylindrical structure with an open upper end, and bolt holes are evenly arranged on the upper end surface of the large die base, and a center hole is arranged at the center of the bottom; the lower die pad is a circular plate matching the inner diameter of the large die base, and a center hole corresponding to the center of the large die base is also arranged at the center of the lower die pad; the lower die outer ring The ring is concentrically arranged with the large die base on the lower die pad in the large die base, the height of the lower die outer ring is greater than the height of the large die base, and a step portion is arranged on the outer edge of the upper end of the lower die outer ring; the upper and lower die positioning rings are arranged on the step portion of the lower die outer ring, and a circle of steps is arranged on the inner wall and outer edge of the upper end of the upper and lower die positioning rings; the hard rings of the upper and lower die positioning rings are arranged on the steps of the inner wall of the upper and lower die positioning rings, and the inner diameters of the hard rings of the upper and lower die positioning rings match the outer diameter of the upper die outer ring; the clamping flange is arranged on the steps of the outer edges of the upper and lower die positioning rings The clamping flange is provided with holes corresponding to the bolt holes on the upper end face of the large die seat; the long bolts are screwed into the bolt holes on the large die seat through the holes on the clamping flange to fix the outer ring of the lower die in the large die seat; the lower concave die is arranged at the lower part of the outer ring of the lower die, the upper concave die is arranged above the lower concave die, the upper end face of the upper concave die is flush with the outer ring of the lower die, the center of the upper end face is provided with a circular groove matching the circular boss on the lower end face of the upper convex die, the center of the bottom of the circular groove is provided with a square hole matching the outer diameter of the square shell forging, the square hole A step is provided at the upper end for forming a square flange at the bottom of the square shell forging; the lower die core shaft is arranged in the lower die and the upper die, the lower end of the lower die core shaft is arranged in a circle, and the upper part is arranged in a square shape matching the inner hole of the square shell forging, and a through hole corresponding to the center hole of the lower die pad is arranged in the center of the lower die core shaft; the ejector is arranged in the through hole in the center of the lower die core shaft, and the length of the ejector is the same as the length of the lower die core shaft; the ejector rod is passed through the center holes of the lower die pad and the large die base, and the upper end of the ejector rod is in contact with the lower end of the ejector rod.
[0006] Specifically, a strain hole for reducing extrusion pressure and forging deformation is provided at the center of the upper punch.
[0007] Specifically, a circle of step flange is arranged at the lower end of the large die base, and U-shaped grooves for fixing the large die base on the workbench of the press are evenly arranged on the circumference of the step flange.
[0008] Specifically, the lower end of the ejector device and the upper end of the ejector rod are both provided with anti-slip steps.
[0009] Specifically, the upper and lower concave dies and the outer ring of the lower die are all in a conical interference fit, and the lower die core shaft and the lower concave die are in a transition fit.
[0010] A method for using a hard aluminum square shell cartridge upsetting flange mold, the specific steps are: S1: upper punch assembly; a. Press the upper punch forcefully into the outer ring of the upper die; b. Place the upper die pad into the outer ring of the upper die; c. Put the upper die mounting plate on the upper die outer ring mounting step, put the upper end of the upper die outer ring into the step groove of the upper die flange plate, and then use bolts to coaxially connect the upper die mounting plate with the upper die and lock them; S2: lower punch assembly; a. Press the upper die into the outer ring of the lower die with force, and the conical surfaces of the two are interference fit. b. Press the lower die into the outer ring of the lower die with force, the conical surfaces of the two are interference fit, and the lower plane of the upper die fits the upper plane of the lower die; c. Use a copper rod or aluminum rod to knock the lower die core shaft into the lower concave die, and the lower die core shaft and the lower concave die are in a transition fit state; d. The hard ring of the upper and lower die positioning rings is a shrink fit with the upper and lower die positioning rings; e. The upper and lower die positioning rings are clearance matched with the lower die outer ring, and the clearance is controlled to 0.01-0.03mm; f. Place the ejector into the lower die mandrel, the lower die pad and ejector rod into the large die base, and then place the upper die, lower die, lower die mandrel, ejector, and lower die outer ring assembled as a whole into the large die base, place the clamping flange on the upper and lower die positioning rings, and tighten the long bolts; S3: Upsetting flange operation; After the upper punch assembly and the lower die assembly are aligned with the outer circle of the upper die outer ring and the inner hole of the hard ring of the upper and lower die positioning rings, the upper punch assembly and the lower die assembly are ensured to be concentric, the upper punch assembly and the movable crossbeam plate of the press are reliably connected by bolts, and the lower die assembly is fixed to the lower template of the press by bolts. The movable crossbeam of the press rises to drive the upper punch assembly to move. When it leaves the lower die assembly for a certain distance, the square shell forging after the second stretching process is placed between the lower die of the lower die assembly and the lower die core shaft. The movable crossbeam of the press drives the upper punch assembly to press downward. After the circular boss of the upper punch contacts with the square shell forging, it continues to press downward and enters the circular groove of the upper die to extrude the flange part of the square shell forging; the movable crossbeam drives the upper punch assembly to move upward, the lower ejector cylinder of the press moves, and the ejector is ejected by the ejector rod. The ejector ejects the forging to complete the flange upsetting process.
[0011] Due to the adoption of the above-mentioned technical solution, the present invention has the following advantages: In the forming process of the present invention, a multi-step stretching and annealing process is adopted, combined with the reverse extrusion forming technology, and the wall thickness is accurately controlled to improve the product quality, thereby realizing the high-precision and high-strength forming of the hard aluminum square shell; the tensile strength of the hard aluminum square shell is further improved by solid solution heat treatment, meeting the tensile strength and elongation requirements of the jamming cartridge; shortening the forming process, improving production efficiency, reducing production costs, and improving market competitiveness; through the cooperation of the forming process and the upsetting flange mold, the near-net forming characteristics of the material can be utilized, the hole depth of the forging is greater than the hole depth of the finished product, the outer end face of the flange needs to be processed, and the end face of the flange on the side of the barrel is directly forged and formed, and this face does not need to be processed. With a small amount of mechanical processing, high-precision ultra-thin wall deep hole flange parts can be obtained, ensuring high-precision processing while improving production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1 It is a schematic diagram of the change of forgings in the forming process of the present invention; In the figure: a is the blanking stage, b is after shaping, c is after reverse extrusion, d is after the first stretching, e is after the second stretching, and f is after flange upsetting.
[0013] Figure 2 It is a schematic diagram of the overall assembly of the upsetting flange die of the present invention.
[0014] Figure 3 yes Figure 2 Schematic cross-sectional view of .
[0015] Figure 4 It is a schematic diagram of the lower die mandrel of the upsetting flange die of the present invention.
[0016] Figure 5 It is a schematic diagram of the upper concave die of the upsetting flange die of the present invention.
[0017] Figure 6 It is a perspective schematic diagram of the lower concave die of the upsetting flange die of the present invention.
[0018] In the figure: 1-upper die flange plate, 2-upper die pad, 3-upper die mounting plate, 4-upper die outer ring, 5-upper punch, 6-large die seat, 7-lower die pad, 8-lower die outer ring, 9-upper and lower die positioning rings, 10-upper and lower die positioning ring hard rings, 11-clamping flange, 12-long bolts, 13-lower die, 14-upper die, 15-lower die mandrel, 16-ejector, 17-ejector rod, 18-square shell forging. DETAILED DESCRIPTION
[0019] The present invention will be further explained below in conjunction with the accompanying drawings and embodiments, which should not be used to limit the protection scope of the present invention. The purpose of disclosing the present invention is to protect all technical improvements within the scope of the present invention.
[0020] Combined with Figure 1-6The forming process of a hard aluminum square shell cartridge shown in the figure has the following specific process: rectangular material cutting → shaping → first annealing → shot blasting → lubrication → reverse extrusion → second annealing → first stretching → third annealing → second stretching → solution heat treatment → flange upsetting → milling of both end faces → quality inspection → finished product.
[0021] Cutting of rectangular materials: Select rectangular 2A14 aluminum alloy material with a profile size of 43.5×30.5mm. According to the required weight of the forging, determine the height of the rectangular profile. The required size is 43.5×30.5×35㎜ in length×width×height. Use precision cutting equipment for cutting. The tolerance in the height direction is controlled at ±0.1㎜ to ensure the accuracy of the material size and reduce material waste.
[0022] Shaping: The cut aluminum alloy material is shaped in the mold. This process is carried out on a press. After shaping, the outer contour of the blank is consistent with the shape of the reverse extrusion die, preparing for subsequent processes. The shaping pressure is 100 tons and zinc stearate powder is used for lubrication.
[0023] First annealing: Annealing treatment is performed to soften the material, reduce internal stress, improve the plasticity of the material, and provide better forming conditions for reverse extrusion; the annealing requirements are to heat up to 410℃, keep at 410℃ for 3 hours, then cool to 150℃ with the furnace and air cool after taking out of the furnace. After annealing, the hardness of the billet is below 60HB; Comparative Example 1: Annealing requirements are to heat to 370℃, keep at 370℃ for 3 hours, then cool to 150℃ with the furnace and air cool out of the furnace. The hardness of the billet after annealing is below 60HB; under the same shot blasting and lubrication conditions, reverse extrusion is carried out. After reverse extrusion, more microcracks will be generated on the outer contour surface. In the process of subsequent stretching, the cracks will expand. Comparative Example 2: Annealing requirements are to heat to 390°C, keep at 390°C for 3 hours, then cool to 150°C with the furnace and air cool out of the furnace. The hardness of the billet after annealing is below 60HB; under the same shot blasting and lubrication conditions, reverse extrusion is carried out. Microcracks will appear on the surface of the outer contour after reverse extrusion. The number of cracks has a tendency to decrease compared with the case of 370°C. In the subsequent stretching process, cracks still expand.
[0024] Shot blasting: Steel shot diameter 0.5mm, shot blasting time 15 minutes.
[0025] Lubrication: The surface of the blank is treated with phosphorus saponification. The lubricant on the surface of the blank can reduce friction and heat generation during cold extrusion, extend the life of the die, and improve the surface quality of the blank formed part.
[0026] Back extrusion: high pressure is applied to the blank at room temperature to form it in the die; according to the high strength characteristics of 2A14 aluminum alloy, the deformation amount of this process is controlled to 76%, and the wall thickness of the square shell forging 18 formed after extrusion is 2.2mm, and the wall thickness deviation is controlled to within 0.1mm to ensure the forming quality; Comparative Example 1: When the reverse extrusion deformation is controlled to 79%, the extrusion wall thickness is 2mm, the extrusion wall thickness deviation will reach 0.15mm-0.2mm, and some reverse extrusion parts will have cracks in the hole wall. At this time, the limit deformation of the material has been exceeded and it tends to be unstable. Comparative Example 2: When the reverse extrusion deformation is controlled to 74%, the extruded wall thickness is 2.5 mm, and the reverse extrusion is also in a stable state, but one more annealing and one more stretching are required, the process will become longer, and the cost will increase.
[0027] Second annealing: Annealing after extrusion helps eliminate the residual stress generated in the previous extrusion process, so that the material has continuous plastic deformation ability and prepares for the stretching process; annealing requires heating to 410℃, keeping at 410℃ for 3 hours, and then cooling to 150℃ with the furnace and air cooling after taking out of the furnace. After annealing, the plastic deformation of the square shell forging 18 will recover its plastic ability, effectively reducing the internal stress of the square shell forging 18; Comparative Example 1: Annealing requirements are to heat to 370℃, keep at 370℃ for 3 hours, then cool to 150℃ and air cool after being taken out of the furnace. During the subsequent stretching process, the hole wall of the stretched part will crack, resulting in stretching failure; Comparative Example 2: Annealing requirements are to heat to 390°C, keep at 370°C for 3 hours, then cool to 150°C and air cool after being taken out of the furnace. During the subsequent stretching process, the hole wall of the stretched part will crack, resulting in stretching failure.
[0028] First stretching: Through the stretching process, the wall thickness of the square shell forging 18 is further thinned to improve the uniformity of the material; for 2A14 aluminum alloy, the stretching should control the appropriate deformation to avoid excessive hardening or cracking; the stretching force is 6 tons, and the process is operated on a stretching hydraulic press. After stretching, the wall thickness of the square shell forging 18 is 1.55mm, and the stretching coefficient is 0.71; Comparative Example 1: When the stretch coefficient of the first stretching is adjusted to 0.65, the wall thickness of the square shell forging 18 after stretching is 1.43mm. There are two results after stretching. Result 1: When stretched to the middle of the length, the stretched piece breaks. Result 2: After the stretching is completed, there will be cracks on the rectangular wall, and they are through-type cracks. Comparative Example 2: When the stretching coefficient of the first stretching is adjusted to 0.8, the wall thickness of the shell forging 18 after stretching is 1.76 mm, and the stretched part is also in a stable state, but it is necessary to add one more annealing and one more stretching, the process will be longer, and the cost will increase.
[0029] The third annealing is required to heat to 410°C, keep at 410°C for 3 hours, and then cool to 150°C with the furnace and then air-cool. After annealing, the plastic deformation of the square shell forging 18 will recover its plasticity, effectively reducing the internal stress of the square shell forging 18; Comparative Example 1: Annealing requirements are to heat to 370℃, keep at 370℃ for 3 hours, then cool to 150℃ and air cool after being taken out of the furnace. During the subsequent stretching process, the hole wall of the stretched part will crack, resulting in stretching failure; Comparative Example 2: Annealing requirements are to heat to 390°C, keep at 370°C for 3 hours, then cool to 150°C and air cool after being taken out of the furnace. During the subsequent stretching process, the hole wall of the stretched part will crack, resulting in stretching failure.
[0030] Second stretching: the tensile force is 6 tons. After stretching, the wall thickness of the shell forging 18 reaches the finished product size requirement of 1.1mm, and the tensile coefficient is 0.71.
[0031] Solution heat treatment: Solution heat treatment can dissolve the strengthening phase in the alloy, improve the plasticity of the alloy, and provide better material properties for the subsequent flange upsetting process; the solution temperature is 495℃, and after keeping warm for 0.5 hours, it is quenched and cooled in water. The square shell forging 18 is placed with the hole facing up and put into the water vertically.
[0032] Upsetting flange: The flange part of the square shell forging 18 is formed by the upsetting process, and the force and shape are precisely controlled to ensure the dimensional accuracy and integrity of the flange; the forming force is 80 tons, and the upsetting operation is completed within 6 hours after the second stretching is completed, otherwise the 2A14 aluminum alloy will increase in hardness over time, which will cause the step size of the flange part to change; Comparative example: When the upsetting is performed 12 hours after the second stretching is completed, the forming force will increase by 90 tons; when the upsetting is performed 18 hours after the second stretching is completed, the forming force will increase by 100 tons; when the upsetting is performed 24 hours after the second stretching is completed, the forming force will increase by 110 tons.
[0033] Milling of both end faces: CNC machining or precision turning is used to finish the both end faces of the formed square shell forging 18 to achieve the dimensional accuracy and surface finish required for the finished product.
[0034] Quality inspection: Quality inspection is carried out after each key process to ensure that the product size, shape and performance meet the design requirements and the final product.
[0035] Among them, the stretching die adopts an upper punching structure: since the wall thickness of the part is 1.1mm and the hole depth is more than 7 times the width of the square inner hole, the conventional lower unloading plate device will cause the overall thin wall to bend and deform, and the uneven stress state will cause the hole mouth to deform, and even the unloading plate blade will be worn and unable to unload, so that the punch returns with the stretched part. During the return process, the unloading plate will scratch the surface of the forging, causing the stretched forging to be scrapped; while adopting the punch hollow punching structure, the punching rod moves from the hollow position of the punch to eject the forging, avoiding the stress on the thin-walled part of the hole, thereby ensuring that the entire thin-walled part is not affected by compressive stress and the hole will not bend and deform.
[0036] A hard aluminum square shell cartridge upsetting flange die comprises an upper convex die assembly and a lower concave die assembly.
[0037] The upper punch assembly includes an upper die flange plate 1, an upper die cushion block 2, an upper die mounting plate 3, an upper die outer ring 4 and an upper punch 5; the upper die flange plate 1 is evenly provided with U-shaped grooves for connecting with the movable crossbeam plate of the press, a step groove is provided at the center of the lower surface, and a circle of mounting holes is evenly provided around the step groove; a step through hole is provided at the center of the upper die outer ring 4, the upper die cushion block 2 is provided in the upper part of the step through hole, the upper punch 5 is provided in the lower part of the step through hole, a strain hole for reducing the extrusion pressure and the deformation of the forging is provided at the center of the upper punch 5, and a strain hole for reducing the extrusion pressure and the deformation of the forging is provided at the center of the lower die. A circular boss protruding from the lower surface of the upper mold outer ring 4 is provided at the center of the end face; a circle of mounting steps is provided at the outer edge of the upper end of the upper mold outer ring 4, and the upper end of the upper mold outer ring 4 is located in the step groove at the center of the upper mold flange plate 1; the upper mold mounting plate 3 cooperates with the mounting step of the upper mold outer ring 4, and the upper mold mounting plate 3 is arranged on the outer side of the upper mold outer ring 4 through the mounting step, and the upper mold mounting plate 3 is provided with holes corresponding to the mounting holes on the lower surface of the upper mold flange plate 1, and the bolts pass through the corresponding holes and mounting holes respectively to connect the upper mold mounting plate 3 and the upper mold flange plate 1.
[0038] The lower die assembly includes a large die base 6, a lower die pad 7, a lower die outer ring 8, upper and lower die positioning rings 9, upper and lower die positioning ring hard rings 10, a clamping flange 11, a long bolt 12, a lower die 13, an upper die 14, a lower die mandrel 15, a pusher 16 and a push rod 17; the large die base 6 is a cylindrical structure with an open upper end, and bolt holes are evenly arranged on the upper end surface of the large die base 6, a center hole is arranged at the center of the bottom, and a circle of step flanges are arranged at the lower end, and U-shaped grooves for fixing the large die base 6 on the press workbench are evenly arranged on the circumference of the step flange; the lower die pad 7 is a circular plate matching the inner diameter of the large die base 6, and the lower die pad A center hole corresponding to the center of the large die base 6 is also provided at the center of the plate 7; the lower die outer ring 8 is concentrically arranged with the large die base 6 on the lower die pad 7 inside the large die base 6, the height of the lower die outer ring 8 is greater than the height of the large die base 6, and a step portion is provided at the outer edge of the upper end of the lower die outer ring 8; the upper and lower die positioning rings 9 are arranged on the step portion of the lower die outer ring 8, and a circle of steps is respectively provided on the inner wall and the outer edge at the upper end of the upper and lower die positioning rings 9; the upper and lower die positioning ring hard rings 10 are arranged on the steps of the inner wall of the upper and lower die positioning rings 9, and the inner diameters of the upper and lower die positioning ring hard rings 10 match the outer diameter of the upper die outer ring 4; the clamping flange 11 is arranged on the outer edge of the upper and lower die positioning rings 9 On the step, the clamping flange 11 is provided with holes corresponding to the bolt holes on the upper end surface of the large die seat 6; the long bolts 12 pass through the holes on the clamping flange 11 and are screwed into the bolt holes on the large die seat 6 to fix the lower die outer ring 8 in the large die seat 6; the lower concave die 13 is arranged at the lower part of the lower die outer ring 8, and the upper concave die 14 is arranged above the lower concave die 13. The upper end surface of the upper concave die 14 is flush with the lower die outer ring 8, and a circular groove matching the circular boss on the lower end surface of the upper punch 5 is arranged at the center of the upper end surface. A square hole matching the outer diameter of the square shell forging 18 is arranged at the center of the bottom of the circular groove, and a square hole for the square shell forging 18 is arranged at the upper end of the square hole. 8. The bottom square flange is formed by steps; the lower die core shaft 15 is arranged in the lower die 13 and the upper die 14, the lower end of the lower die core shaft 15 is arranged in a circle, and the upper part is arranged in a square shape matching the inner hole of the square shell forging 18, and the center of the lower die core shaft 15 is provided with a through hole corresponding to the center hole of the lower die pad 7; the ejector 16 is arranged in the through hole in the center of the lower die core shaft 15, and the length of the ejector 16 is the same as that of the lower die core shaft 15; the ejector rod 17 is passed through the center holes of the lower die pad 7 and the large die base 6, the upper end of the ejector rod 17 is in contact with the lower end of the ejector rod 16, and the lower end of the ejector rod 16 and the upper end of the ejector rod 17 are provided with anti-slip steps.
[0039] A method for using a hard aluminum square shell cartridge upsetting flange mold, the specific steps are: S1: upper punch assembly; a. Press the upper punch 5 forcefully into the upper die outer ring 4; b. Place the upper die block 2 into the upper die outer ring 4; c. Put the upper die mounting plate 3 on the mounting step of the upper die outer ring 4, put the upper end of the upper die outer ring 4 into the step groove of the upper die flange plate 1, and then use bolts to coaxially connect the upper die mounting plate 3 with the upper die flange plate 1 and lock them; S2: assembly of the lower die assembly; a. Press the upper die 14 into the outer ring 8 of the lower die with force, and the conical surfaces of the two are interference fit, with a taper of 1.5° on one side and an interference amount of 5‰; b. Press the lower die 13 into the outer ring 8 of the lower die with force, and the conical surfaces of the two are interference fit, the taper is 1.5° on one side, the interference is 3‰, and the lower plane of the upper die 14 fits with the upper plane of the lower die 13; c. Use a copper rod or an aluminum rod to knock the lower die core shaft 15 into the lower die 13, and the lower die core shaft 15 and the lower die 13 are in a transition fit state; d. The upper and lower mold positioning ring hard ring 10 and the upper and lower mold positioning ring 9 are shrink-fitted; the upper and lower mold positioning ring 9 are heated to 400°C; e. The upper and lower die positioning rings 9 and the lower die outer ring 8 are clearance matched, and the clearance is controlled to 0.01-0.03mm; f. Place the ejector 16 into the lower die core shaft 15, the lower die pad 7 and the ejector 17 into the large die base 6, and then place the upper die 14, lower die 13, lower die core shaft 15, ejector 16, and lower die outer ring 8 assembled as a whole in the above steps into the large die base 6, put the clamping flange 11 on the upper and lower die positioning rings 9, and tighten the long bolts 12; S3: Upsetting flange operation; After the upper punch assembly and the lower die assembly are aligned with the outer circle of the upper die outer ring 4 and the inner hole of the hard ring 10 of the upper and lower die positioning rings, the upper punch assembly and the lower die assembly are ensured to be concentric, the upper punch assembly and the movable crossbeam plate of the press are reliably connected by bolts, and the lower die assembly is fixed to the lower template of the press by bolts. The movable crossbeam of the press rises to drive the upper punch assembly to move. When it leaves the lower die assembly for a certain distance, the square shell forging 18 after the second stretching process is placed between the lower die 13 of the lower die assembly and the lower die core shaft 15. The movable crossbeam of the press drives the upper punch assembly to press downward. After the circular boss of the upper punch 5 contacts with the square shell forging 18, it continues to press downward and enters the circular groove of the upper die 14 to extrude the flange part of the square shell forging 18; the movable crossbeam drives the upper punch assembly to move upward, and the lower ejector cylinder of the press moves, and the ejector 16 is ejected by the ejector rod 17. The ejector 16 ejects the forging to complete the flange upsetting process.
[0040] Parts of the present invention not described in detail are prior art.
[0041] The embodiments selected herein for the purpose of disclosing the invention are currently considered to be suitable, but it should be understood that the invention is intended to include all changes and modifications of the embodiments that fall within the scope of the concept and invention.
Claims
1. A forming process for a hard aluminum square shell cartridge, characterized in that: The specific process is: rectangular material cutting → shaping → first annealing → shot blasting → lubrication → reverse extrusion → second annealing → first stretching → third annealing → second stretching → solution heat treatment → flange upsetting → milling of both end faces → quality inspection → finished product; Rectangular material cutting: Select rectangular aluminum alloy profiles, determine the cutting height of the rectangular profiles according to the required weight of the forgings, use precision cutting equipment for cutting, and control the height tolerance to ±0.1㎜; Shaping: The cut aluminum alloy material is shaped in the die. This process is carried out on a press. After shaping, the outer contour of the blank is consistent with the shape of the reverse extrusion die, preparing for subsequent processes. The shaping pressure is 100 tons, and zinc stearate powder is used for lubrication. First annealing: annealing treatment is performed to soften the material. The annealing requirements are to heat up to 410℃, keep at 410℃ for 3 hours, then cool to 150℃ with the furnace and air cool out of the furnace. After annealing, the hardness of the billet is below 60HB; Shot blasting: steel shot diameter 0.5mm, shot blasting time 15 minutes; Lubrication: Phosphorus saponification treatment is performed on the surface of the blank; Back extrusion: Use a die to apply high pressure to the blank at room temperature to form a square shell forging. The back extrusion pressure is 125 tons, the deformation is 75-76%, and the wall thickness deviation is controlled within 0.1mm; Second annealing: The annealing requirement is to heat up to 410℃, keep at 410℃ for 3 hours, then cool to 150℃ with the furnace and then air-cool. After annealing, the hardness of the square shell forging is below 60HB; First stretching: The square shell forging is stretched for the first time on the stretching hydraulic press, and the stretching coefficient is 0.71; Third annealing: annealing requires heating to 410℃, keeping at 410℃ for 3 hours, then cooling to 150℃ with the furnace and air cooling; Second stretching: The square shell forging is stretched for the second time on the stretching hydraulic press, with a stretching coefficient of 0.
71. After stretching, the wall thickness of the square shell forging reaches the finished product size requirements; Solution heat treatment: solution temperature 495℃, keep warm for 0.5 hours, then quench and cool in water, place the square shell forging with the hole facing upwards, and put it into water vertically; Upsetting flange: After the second stretching is completed, the upsetting operation is completed within 6 hours, and the flange part of the square shell forging is formed by the upsetting flange die; Milling of both end faces: CNC machining or precision turning is used to finish the both end faces of the formed square shell forging to achieve the required dimensional accuracy and surface finish of the finished product; Quality inspection: Quality inspection is carried out after each key process to ensure that the product size, shape and performance meet the design requirements and the final product.
2. A hard aluminum square shell cartridge upsetting flange die, characterized in that: It includes an upper male mold component and a lower female mold component; The upper punch assembly comprises an upper die flange plate, an upper die pad, an upper die mounting plate, an upper die outer ring and an upper punch; a U-shaped groove for connecting with the movable crossbeam plate of the press is evenly arranged on the circumference of the upper die flange plate, a step groove is arranged at the center of the lower surface, and a circle of mounting holes is evenly arranged around the step groove; a step through hole is arranged at the center of the upper die outer ring, the upper die pad is arranged in the upper part of the step through hole, the upper punch is arranged in the lower part of the step through hole, and a circular boss protruding from the lower surface of the upper die outer ring is arranged at the center of the lower end surface of the upper punch; a circle of mounting steps is arranged on the outer edge of the upper end of the upper die outer ring, and the upper end of the upper die outer ring is located in the step groove in the center of the upper die flange plate; the upper die mounting plate is matched with the upper die outer ring mounting step and is arranged on the outside of the upper die outer ring, and holes corresponding to the mounting holes on the lower surface of the upper die flange plate are arranged on the upper die mounting plate, and bolts pass through the corresponding holes and mounting holes respectively to connect the upper die mounting plate and the upper die flange plate; The lower die assembly comprises a large die base, a lower die pad, a lower die outer ring, upper and lower die positioning rings, upper and lower die positioning ring hard rings, a clamping flange, a long bolt, a lower die, an upper die, a lower die mandrel, a push piece and a push rod; the large die base is a cylindrical structure with an open upper end, and bolt holes are evenly arranged on the upper end surface of the large die base, and a center hole is arranged at the center of the bottom; the lower die pad is a circular plate matching the inner diameter of the large die base, and a center hole corresponding to the center of the large die base is also arranged at the center of the lower die pad; the lower die outer ring The ring is concentrically arranged with the large die base on the lower die pad in the large die base, the height of the lower die outer ring is greater than the height of the large die base, and a step portion is arranged on the outer edge of the upper end of the lower die outer ring; the upper and lower die positioning rings are arranged on the step portion of the lower die outer ring, and a circle of steps is arranged on the inner wall and outer edge of the upper end of the upper and lower die positioning rings; the hard rings of the upper and lower die positioning rings are arranged on the steps of the inner wall of the upper and lower die positioning rings, and the inner diameters of the hard rings of the upper and lower die positioning rings match the outer diameter of the upper die outer ring; the clamping flange is arranged on the steps of the outer edges of the upper and lower die positioning rings The clamping flange is provided with holes corresponding to the bolt holes on the upper end face of the large die seat; the long bolts are screwed into the bolt holes on the large die seat through the holes on the clamping flange to fix the outer ring of the lower die in the large die seat; the lower concave die is arranged at the lower part of the outer ring of the lower die, the upper concave die is arranged above the lower concave die, the upper end face of the upper concave die is flush with the outer ring of the lower die, the center of the upper end face is provided with a circular groove matching the circular boss on the lower end face of the upper convex die, the center of the bottom of the circular groove is provided with a square hole matching the outer diameter of the square shell forging, the square hole A step is provided at the upper end for forming a square flange at the bottom of the square shell forging; the lower die core shaft is arranged in the lower die and the upper die, the lower end of the lower die core shaft is arranged in a circle, and the upper part is arranged in a square shape matching the inner hole of the square shell forging, and a through hole corresponding to the center hole of the lower die pad is arranged in the center of the lower die core shaft; the ejector is arranged in the through hole in the center of the lower die core shaft, and the length of the ejector is the same as the length of the lower die core shaft; the ejector rod is passed through the center holes of the lower die pad and the large die base, and the upper end of the ejector rod is in contact with the lower end of the ejector rod.
3. The hard aluminum square shell cartridge upsetting flange mold according to claim 2, characterized in that: The center of the upper punch is provided with a strain hole for reducing the extrusion pressure and the deformation of the forging.
4. The duralumin square shell cartridge upsetting flange die according to claim 2, characterized in that: A circle of step flange is arranged at the lower end of the large die base, and U-shaped grooves for fixing the large die base on the workbench of the press are evenly arranged on the circumference of the step flange.
5. The hard aluminum square shell cartridge upsetting flange mold according to claim 2, characterized in that: The lower end of the ejector and the upper end of the ejector rod are both provided with anti-dropping steps.
6. The duralumin square shell cartridge upsetting flange die according to claim 2, characterized in that: The upper and lower concave dies and the outer ring of the lower die are all in conical interference fit, and the lower die core shaft and the lower concave die are in transition fit.
7. A method for using the hard aluminum square shell cartridge upsetting flange mold as described in any one of claims 2 to 6, characterized in that: The specific steps are: S1: upper punch assembly; a. Press the upper punch forcefully into the outer ring of the upper die; b. Place the upper die pad into the outer ring of the upper die; c. Put the upper die mounting plate on the upper die outer ring mounting step, put the upper end of the upper die outer ring into the step groove of the upper die flange plate, and then use bolts to coaxially connect the upper die mounting plate and the upper die flange plate and lock them; S2: assembly of the lower die assembly; a. Press the upper die into the outer ring of the lower die with force, and the conical surfaces of the two are interference fit; b. Press the lower die into the outer ring of the lower die with force, the conical surfaces of the two are interference fit, and the lower plane of the upper die fits the upper plane of the lower die; c. Use a copper rod or aluminum rod to knock the lower die core shaft into the lower concave die, and the lower die core shaft and the lower concave die are in a transition fit state; d. The hard ring of the upper and lower die positioning rings is a shrink fit with the upper and lower die positioning rings; e. The upper and lower die positioning rings are clearance matched with the lower die outer ring, and the clearance is controlled to 0.01-0.03mm; f. Place the ejector into the lower die mandrel, the lower die pad and ejector rod into the large die base, and then place the upper die, lower die, lower die mandrel, ejector, and lower die outer ring assembled as a whole into the large die base, place the clamping flange on the upper and lower die positioning rings, and tighten the long bolts; S3: Upsetting flange operation; After the upper punch assembly and the lower die assembly are aligned with the outer circle of the upper die outer ring and the inner hole of the hard ring of the upper and lower die positioning rings, the upper punch assembly and the lower die assembly are ensured to be concentric, the upper punch assembly and the movable crossbeam plate of the press are reliably connected by bolts, and the lower die assembly is fixed to the lower template of the press by bolts. The movable crossbeam of the press rises to drive the upper punch assembly to move. When it leaves the lower die assembly for a certain distance, the square shell forging after the second stretching process is placed between the lower die of the lower die assembly and the lower die core shaft. The movable crossbeam of the press drives the upper punch assembly to press downward. After the circular boss of the upper punch contacts with the square shell forging, it continues to press downward and enters the circular groove of the upper die to extrude the flange part of the square shell forging; the movable crossbeam drives the upper punch assembly to move upward, the lower ejector cylinder of the press moves, and the ejector is ejected by the ejector rod. The ejector ejects the forging to complete the flange upsetting process.
Citation Information
Patent Citations
Machining method of high-precision and large-diameter ultralong and ultrathin shell
CN105171356A
Cold forging forming process and forming die for thin-wall deep-hole flanged part
CN112828117A
Cold backward extrusion process for aluminum alloy rectangular box-shaped thin-wall shell
CN114798786A
Forming method of ultrahigh-strength aluminum alloy cartridge case
CN117702013A
Cartridge assembly
JP2007095143A
Cited By
Die and process for manufacturing rectangular-wave micro-channel part of radiator
CN121571486A
Improved ammunition storage case