A steel core high conductivity aluminum stranded wire for overhead conductor and a manufacturing method thereof

By optimizing the structure and manufacturing process, combining efficient refining agent and hydrogen removal treatment, the conductivity and strength of steel core aluminum stranded wires are improved, solving the problems of poor conductivity and high cost of traditional aluminum stranded wires, and achieving lower electrical energy Loss and higher transmission efficiency.

CN117995480BActive Publication Date: 2024-11-29广东中联电缆集团有限公司 +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410025713.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-08
Publication Date
2024-11-29
Estimated Expiration
2044-01-08

AI Technical Summary

Technical Problem

The conductivity of traditional steel core aluminum stranded wires is poor, resulting in high power loss and difficulty in taking into account both strength and conductivity. The existing overhead conductor manufacturing methods have problems of low efficiency and high cost.

Method used

Adopted an optimized structural design and manufacturing process, high-strength galvanized steel wire is used as the core wire, and the purity and conductivity of the hard aluminum wire is improved through efficient and environmentally friendly refining agent and hydrogen and slag removal treatment, and a helical winding structure is used to improve the conductivity. and strength.

Benefits of technology

It significantly reduces electrical energy loss, improves conductive performance and strength, extends service life, and reduces production and maintenance costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117995480B_ABST
    Figure CN117995480B_ABST
Patent Text Reader

Abstract

The present invention discloses a steel core high conductivity aluminum stranded wire for overhead conductors and a manufacturing method thereof, wherein the steel core high conductivity aluminum stranded wire is sequentially provided with a central galvanized steel wire, a galvanized steel wire middle layer, a galvanized steel wire outer layer, a hard aluminum wire inner layer, a hard aluminum wire middle layer and a hard aluminum wire outer layer in order from the center to the outside, and each layer is composed of multiple wires and is spirally wound on the inner layer in a direction opposite to the winding direction of the inner layer. The present invention scientifically designs the structure and manufacturing process of the steel core aluminum stranded wire, uses high-strength galvanized steel wire with a tensile strength of ≥1450MPa to replace ordinary galvanized steel wire, and uses high-conductivity hard aluminum wire with a conductivity of ≥63%IACS to replace ordinary hard aluminum wire, so that the steel core aluminum stranded wire has higher structural strength and lower resistance loss, meets the construction requirements of overhead power transmission lines in environments such as long distance, large span, high altitude, ice cover, strong wind, etc., reduces the power loss of the line, and improves the safety of line operation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of aluminum stranded wire manufacturing, and in particular relates to a steel core high-conductivity aluminum stranded wire for overhead conductors and a manufacturing method thereof. Background Art

[0002] Electricity is an indispensable energy source for the development of the national economy, and the power grid is a major infrastructure to ensure the smooth operation of the national economy and society. With the sustained and rapid development of my country's national economy and the continuous improvement of people's living standards, the demand for electricity continues to rise. However, my country's power resources and power load are inversely distributed. Coal-fired power is mainly distributed in the western and northern regions, hydropower is mainly distributed in the southwest, and power load is mainly concentrated in the eastern coastal areas. In order to solve the contradiction between supply and demand of power resources, the country has implemented the power grid development strategy of "sending electricity from west to east" and "supplied by north and south".

[0003] Steel-core aluminum stranded wire is the carrier of long-distance overhead power transmission, and its performance directly determines the power transmission capacity and power loss of the line. Traditional steel-core aluminum stranded wire has high resistivity and poor conductivity, resulting in small line transmission capacity and large power loss, causing huge waste of power resources. In addition, traditional steel-core aluminum stranded wire also has problems such as heavy weight, poor sag characteristics and corrosion resistance, short life cycle, and high maintenance cost, which can no longer adapt to the rapid development of the power industry.

[0004] In order to reduce the power loss of transmission lines and improve the transmission efficiency and power utilization efficiency, the conductivity of steel core aluminum stranded wire must be further improved. However, there is a problem of mutual restriction between the conductivity and strength of aluminum wire. The traditional method of adjusting the alloy composition makes it difficult to balance the improvement of conductivity and strength, resulting in the steel core aluminum stranded wire still generally having the problem of high strength and low conductivity or high conductivity and low strength. Therefore, the existing steel core aluminum stranded wire for overhead conductors and its manufacturing method still need to be improved and developed. Summary of the invention

[0005] The purpose of the present invention is to provide a steel core high conductivity aluminum stranded wire for overhead conductors and a manufacturing method thereof in view of the above-mentioned existing problems and shortcomings, and to improve the strength and conductivity of the steel core aluminum stranded wire by optimizing the structure and manufacturing process of the steel core aluminum stranded wire for overhead conductors, thereby reducing the line power loss of long-distance power transmission and improving the power transmission efficiency and power utilization rate.

[0006] The technical solution of the present invention is achieved in this way:

[0007] The first aspect of the present invention provides a steel core high conductivity aluminum stranded wire for overhead wires, which is characterized in that the steel core high conductivity aluminum stranded wire is sequentially provided with a central galvanized steel wire, a galvanized steel wire middle layer, a galvanized steel wire outer layer, a hard aluminum wire inner layer, a hard aluminum wire middle layer and a hard aluminum wire outer layer in order from the center to the outside, the galvanized steel wire middle layer and the galvanized steel wire outer layer are respectively composed of a plurality of galvanized steel wires, the hard aluminum wire inner layer, the hard aluminum wire middle layer and the hard aluminum wire outer layer are respectively composed of a plurality of hard aluminum wires, the galvanized steel wire The galvanized steel wire middle layer is spirally wound on the central galvanized steel wire, the galvanized steel wire outer layer is spirally wound on the galvanized steel wire middle layer in a direction opposite to the winding direction of the galvanized steel wire middle layer, the duraluminum wire inner layer is spirally wound on the galvanized steel wire outer layer in a direction opposite to the winding direction of the galvanized steel wire outer layer, the duraluminum wire middle layer is spirally wound on the duraluminum wire inner layer in a direction opposite to the winding direction of the duraluminum wire inner layer, and the duraluminum wire outer layer is spirally wound on the duraluminum wire middle layer in a direction opposite to the winding direction of the duraluminum wire middle layer.

[0008] Preferably, the diameter of the galvanized steel wire is 1.5-2 mm, the tensile strength of the galvanized steel wire is ≥1450 MPa, the stress at 1% elongation is ≥1310 MPa, and the elongation after fracture is ≥2.5%. Since the high-strength galvanized steel wire with a tensile strength of ≥1450 MPa is a mature product and can be purchased on the market, the manufacturing method of the galvanized steel wire is not described here.

[0009] Preferably, the diameter of the hard aluminum wire is 3-4 mm, the tensile strength of the hard aluminum wire is ≥200.9 MPa, the yield strength is ≥181.5 MPa, the elongation after fracture is ≥8.1%, and the DC resistivity at 20°C is ≤0.0272Ω·mm 2 / m, electrical conductivity ≥63.5%IACS.

[0010] Preferably, the hard aluminum wire is composed of the following components in mass percentage: Fe 0.23-0.27%, the balance being Al and unavoidable impurities, with a single impurity ≤0.05% and a total impurity content ≤0.1%.

[0011] A second aspect of the present invention provides a method for manufacturing a steel core high conductivity aluminum stranded wire for an overhead conductor, which is characterized by comprising the following steps in sequence:

[0012] Step 1: Melt and prepare aluminum liquid at 700-720℃ according to the composition and mass percentage of hard aluminum wire;

[0013] Step 2: Use argon gas with a purity of 99.99% and a refining agent accounting for 0.1-0.2% of the weight of the aluminum liquid to spray and refine the aluminum liquid in the smelting furnace for 10-20 minutes to remove the slag, and then scrape off the slag on the surface of the aluminum liquid;

[0014] Step 3: A mixed gas consisting of argon with a purity of 99.99% and chlorine with a purity of 99.99% is introduced through the air-permeable brick installed at the bottom of the smelting furnace to refine the aluminum liquid for 10-20 minutes to remove hydrogen;

[0015] Step 4: The aluminum liquid in the smelting furnace is introduced into the launder, and the aluminum liquid flows through the degassing box and the tubular filter box arranged on the launder in sequence to perform online hydrogen removal and slag removal treatment;

[0016] Step 5: Under the conditions of a casting wheel speed of 26-28 rpm and a cooling water flow rate of 9-11 liters / minute, the 680-690°C molten aluminum is continuously cast and extruded into a round aluminum rod with a diameter of 9.5 mm;

[0017] Step 6: Pull the round aluminum rod into a hard aluminum wire with a diameter of 3-4 mm;

[0018] Step 7: Twisting the hard aluminum wire and the galvanized steel wire to obtain the steel core high conductivity aluminum stranded wire for the overhead conductor.

[0019] Preferably, the refining agent in step 2 is composed of the following components in mass percentage: ZnCl2 44.6%, K2CO3 25.8%, NaNO3 7.9%, KF 10.5%, K2SO4 7.4%, and Li2SO4 3.8%.

[0020] Preferably, the production method of the refining agent in step 2 comprises the following steps in sequence:

[0021] (1) According to the composition and mass percentage of the refining agent, ZnCl2, K2CO3, NaNO3, KF, K2SO4, and Li2SO4 with a purity of ≥99.8% are selected as raw materials for batching;

[0022] (2) heating and melting the raw materials at 1150°C under the protection of argon gas with a purity of 99.99%, and then cooling and solidifying them into a bulk refining agent;

[0023] (3) crushing the bulk refining agent into powder with a particle size of ≤2 mm to obtain the refining agent.

[0024] Hydrogen pores and inclusions are common defects inside aluminum wires. They will split the aluminum matrix, hinder the movement of free electrons, and increase the scattering of free electrons, which will lead to an increase in the resistance of the aluminum wire and a decrease in the conductivity. Hydrogen pores and inclusions will also cause local stress concentration inside the aluminum wire, becoming the crack source and crack extension direction of the aluminum wire, thereby reducing the strength, plasticity and corrosion resistance of the aluminum wire. Therefore, in order to solve the problem of mutual restriction between strength and conductivity and improve the strength and conductivity of hard aluminum wire at the same time, the purity of hard aluminum wire must be improved.

[0025] Traditional refining agents are mainly made of raw materials such as sodium salt, fluoride salt, chloride salt, hexachloroethane, etc., which are directly crushed and mixed. The interaction between the raw materials is not brought into play, resulting in a high melting point of the refining agent and low slag removal efficiency. In order to improve the slag removal efficiency of aluminum liquid in the furnace, the inventor has developed a highly efficient and environmentally friendly refining agent through a large number of experimental studies. The refining agent is mainly composed of ZnCl2 and K2CO3, and a small amount of NaNO3, KF, K2SO4, and Li2SO4 are added. The raw materials are first heated and melted at 1150°C under argon protection, and then cooled, solidified and crushed into a powdery refining agent. The melting point of ZnCl2 is about 290°C, the melting point of NaNO3 is 306.8°C, the melting point of K2CO3 is 891°C, the melting point of KF is 858°C, the melting point of K2SO4 is 1069°C, and the melting point of Li2SO4 is 85 9℃, although K2CO3, KF, K2SO4, Li2SO4 have high melting points, through melting and solidification crystallization, K2CO3 and KF form KF·K2CO3 eutectic with a melting point of only 688℃, and K2SO4 and Li2SO4 form K2SO4·Li2SO4 eutectic with a melting point of only 716℃, which greatly reduces the melting point of the refining agent, and the refining agent is easier to dissolve in the aluminum liquid. ZnCl2 decomposes Cl2, K2CO3 decomposes CO2, and NaNO3 decomposes N2, CO2 and NO gas. A large number of bubbles capture inclusions in the aluminum liquid during the floating process, which has a slag removal effect. The K2SO4·Li2SO4 eutectic melts into liquid molten salt, which has a good wetting and spheroidizing effect on inclusions such as alumina, promotes the separation of inclusions from aluminum liquid, and improves the slag removal efficiency. In addition, the refining agent does not contain sodium salt and hexachloroethane, but only contains a small amount of fluoride salt, and is more environmentally friendly to use.

[0026] Preferably, the volume percentage of chlorine in the mixed gas in step three is 3-5%, and the flow rate of the mixed gas is 1-2 cubic meters per minute.

[0027] The main function of spraying refining agent on aluminum liquid in the furnace is to remove slag. Although it also has a dehydrogenation effect, the dehydrogenation effect is poor because the refining agent inevitably contains moisture, which will cause the aluminum liquid to absorb hydrogen during refining. In order to reduce the hydrogen content of the aluminum liquid in the furnace, the present invention installs a plurality of porous air-permeable bricks in the smelting furnace, and then passes a mixed gas composed of argon and chlorine into the aluminum liquid in the furnace through the air-permeable bricks. After the mixed gas passes through the porous air-permeable bricks, it is decomposed into small and uniform small bubbles. The small bubbles capture the hydrogen in the aluminum liquid during the floating process, and then float up and take out the aluminum liquid, which plays a role in dehydrogenation. Since a plurality of porous air-permeable bricks are evenly installed at the bottom of the smelting furnace, the bubbles are evenly distributed in the aluminum liquid. At the same time, the bubbles have a stirring effect on the aluminum liquid when floating, avoiding the dead corner of degassing in the aluminum liquid in the furnace, and improving the dehydrogenation efficiency of the aluminum liquid. Chlorine is added to the mixed gas, because chlorine has a stronger binding force with hydrogen atoms, thereby further improving the dehydrogenation effect. After dehydrogenation through the air-permeable bricks at the bottom of the furnace, the hydrogen content of the molten aluminum in the smelting furnace can be reduced to below 0.2ml / 100gAl, thereby greatly improving the purity of the molten aluminum in the furnace.

[0028] Preferably, in the step 4, the rotation speed of the graphite rotor in the degassing box is 600-700 rpm, the gas flow on the graphite rotor is 1-2 cubic meters per hour, the gas pressure is 0.8-1MPa, and the gas is a mixture of argon with a purity of 99.99% and chlorine with a purity of 99.9%, and the volume percentage of chlorine in the mixed gas is 3-5%.

[0029] The high-speed rotating graphite rotor in the degassing box breaks the mixed gas composed of argon and chlorine into tiny bubbles and enters into the molten aluminum. The hydrogen atoms in the molten aluminum are continuously diffused into the bubbles by utilizing the partial pressure difference of hydrogen between the molten aluminum and the bubbles, and then float up and escape from the molten aluminum with the bubbles, thus removing hydrogen. After dehydrogenation in the degassing box, the hydrogen content of the molten aluminum can be reduced to below 0.08ml / 100gAl, thereby greatly improving the purity of the molten aluminum and ultimately improving the strength and conductivity of the hard aluminum wire.

[0030] The filter medium of the tubular filter box in step four is a ceramic filter tube. The ceramic filter tube is made of silicon nitride ceramic particles with a particle size of 3-6mm and a binder sintered at high temperature. There are a large number of tortuous pores inside. When the aluminum liquid flows through the ceramic filter tube, inclusions are adsorbed or blocked on the surface of the ceramic filter tube and the inner wall of the pores, thereby achieving the effect of filtering and removing slag. The structure and use of the tubular filter box are available in public literature and will not be repeated here. Tubular filtration is a high-precision filtration. After tubular filtration, the removal rate of inclusions larger than 5μm in the aluminum liquid can reach more than 98%, and the slag content of the aluminum liquid can be reduced to 0.05mm 2 / kgAl or less, thereby greatly improving the purity of molten aluminum and increasing the strength and conductivity of hard aluminum wire.

[0031] The continuous casting and extrusion in step five is to pour the aluminum liquid into the continuous casting and extrusion machine, and extrude the aluminum liquid through the mold after cooling by the casting and extrusion wheel to obtain a round aluminum rod. Continuous casting and extrusion is a highly efficient short-process forming technology. Compared with conventional continuous casting and rolling, it has the advantages of small investment and small footprint. The specific structure and operation method of continuous casting and extrusion can be found in the literature, so they will not be repeated here. The twisting and forming described in step seven is to twist the hard aluminum wire and the steel wire on a twisting machine according to the structure of the steel core high conductivity aluminum stranded wire. Since the twisting machine is a conventional mechanical equipment, there is a large amount of literature available, so the structure and use of the twisting machine will not be repeated.

[0032] Compared with the prior art, the present invention has the following beneficial effects:

[0033] The present invention optimizes the structure and manufacturing process of the steel core high conductivity aluminum stranded wire for overhead conductors, adopts high-strength galvanized steel wire instead of ordinary steel wire as the core wire of the aluminum stranded wire, and adopts high-conductivity hard aluminum alloy wire instead of ordinary hard aluminum wire on the outside. Therefore, compared with the traditional steel core aluminum stranded wire, under the condition of equal cross-sectional area, the steel core high conductivity aluminum stranded wire for overhead conductors of the present invention has lower resistance and higher conductivity, which can reduce the power loss of the line, increase the power transmission capacity of the line, and improve the power transmission efficiency of the line. Since the high conductivity hard aluminum wire has higher strength and better corrosion resistance, the steel core high conductivity aluminum stranded wire for overhead conductors of the present invention also has the advantages of light weight, large tensile force to weight ratio, good sag characteristics, long life cycle, and low maintenance cost. In addition, compared with the traditional continuous casting and rolling process, the manufacturing process of the present invention is shorter, the equipment investment is small, the floor space is small, the production efficiency is high, and the production cost of the steel core high conductivity aluminum stranded wire for overhead conductors can be greatly reduced. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 This is a schematic structural diagram of the steel core high conductivity aluminum stranded wire for overhead conductors described in Example 1 of the present invention.

[0035] Figure 2 This is a schematic structural diagram of the steel core high conductivity aluminum stranded wire for overhead conductors described in Example 2 of the present invention.

[0036] Figure 3 This is a schematic structural diagram of the steel core high conductivity aluminum stranded wire for overhead conductors described in Example 3 of the present invention. DETAILED DESCRIPTION

[0037] The technical solution of the present invention is further described below in conjunction with specific embodiments and the accompanying drawings.

[0038] Embodiment 1:

[0039] A steel core high conductivity aluminum stranded wire for overhead conductors, such as Figure 1As shown, in order from the center to the outside, a central galvanized steel wire 101, a galvanized steel wire middle layer 102, a galvanized steel wire outer layer 103, a hard aluminum wire inner layer 201, a hard aluminum wire middle layer 202 and a hard aluminum wire outer layer 203 are sequentially arranged, the galvanized steel wire middle layer 102 is composed of 6 galvanized steel wires, the galvanized steel wire outer layer 103 is composed of 12 galvanized steel wires, the hard aluminum wire inner layer 201 is composed of 10 hard aluminum wires, the hard aluminum wire middle layer 202 is composed of 17 hard aluminum wires, the hard aluminum wire outer layer 203 is composed of 23 hard aluminum wires, the galvanized steel wire middle layer 102 is spirally connected to the hard aluminum wire inner layer 201, and the hard aluminum wire outer layer 203 is spirally connected to the hard aluminum wire inner layer 201. The galvanized steel wire outer layer 103 is spirally wound on the galvanized steel wire middle layer 102 in a direction opposite to the winding direction of the galvanized steel wire middle layer 102; the hard aluminum wire inner layer 201 is spirally wound on the galvanized steel wire outer layer 103 in a direction opposite to the winding direction of the galvanized steel wire outer layer 103; the hard aluminum wire middle layer 202 is spirally wound on the hard aluminum wire inner layer 201 in a direction opposite to the winding direction of the hard aluminum wire inner layer 201; the hard aluminum wire outer layer 203 is spirally wound on the hard aluminum wire middle layer 202 in a direction opposite to the winding direction of the hard aluminum wire middle layer 202.

[0040] The diameter of the galvanized steel wire is 1.5 mm. After testing, the tensile strength of the galvanized steel wire is 1482 MPa, the stress at 1% elongation is 1327 MPa, and the elongation after fracture is 2.5%.

[0041] The diameter of the hard aluminum wire is 3 mm, and the hard aluminum wire is composed of the following components in mass percentage: Fe 0.25%, and the balance is Al and inevitable impurities, with a single impurity ≤0.05% and a total impurity content ≤0.1%.

[0042] The manufacturing method of steel core high conductivity aluminum stranded wire for overhead conductor comprises the following steps in sequence:

[0043] Step 1: Melt and prepare aluminum liquid at 710℃ according to the composition and mass percentage of the hard aluminum wire;

[0044] Step 2: Use argon gas with a purity of 99.99% and a refining agent accounting for 0.15% of the weight of the aluminum liquid to spray and refine the aluminum liquid in the smelting furnace for 15 minutes to remove the slag, and then scrape off the slag on the surface of the aluminum liquid;

[0045] Step 3: A mixed gas consisting of argon with a purity of 99.99% and chlorine with a purity of 99.99% is introduced through the air-permeable brick installed at the bottom of the smelting furnace to refine the aluminum liquid for 15 minutes to remove hydrogen. The volume percentage of chlorine in the mixed gas is 4%, and the flow rate of the mixed gas is 1.5 cubic meters / minute;

[0046] Step 4: introducing the aluminum liquid in the smelting furnace into the launder, and making the aluminum liquid flow through the degassing box and the tubular filter box arranged on the launder in turn for online dehydrogenation and slag removal treatment, the rotation speed of the graphite rotor in the degassing box is 650 rpm, the gas flow rate on the graphite rotor is 1.5 cubic meters per hour, and the gas pressure is 0.9 MPa. The gas is a mixed gas composed of argon with a purity of 99.99% and chlorine with a purity of 99.99%, and the volume percentage of chlorine in the mixed gas is 4%;

[0047] Step 5: Under the conditions of a casting wheel speed of 27 rpm and a cooling water flow rate of 10 liters / minute, the 685°C aluminum liquid is continuously cast and extruded into a round aluminum rod with a diameter of 9.5 mm;

[0048] Step 6: Pull the round aluminum rod into a hard aluminum wire with a diameter of 3 mm;

[0049] Step 7: Twisting the hard aluminum wire and the galvanized steel wire to obtain the steel core high conductivity aluminum stranded wire for the overhead conductor.

[0050] Embodiment 2:

[0051] A steel core high conductivity aluminum stranded wire for overhead conductors, such as Figure 2 As shown, in order from the center to the outside, a central galvanized steel wire 101, a galvanized steel wire middle layer 102, a galvanized steel wire outer layer 103, a hard aluminum wire inner layer 201, a hard aluminum wire middle layer 202 and a hard aluminum wire outer layer 203 are sequentially arranged, the galvanized steel wire middle layer 102 is composed of 6 galvanized steel wires, the galvanized steel wire outer layer 103 is composed of 12 galvanized steel wires, the hard aluminum wire inner layer 201 is composed of 10 hard aluminum wires, the hard aluminum wire middle layer 202 is composed of 17 hard aluminum wires, the hard aluminum wire outer layer 203 is composed of 23 hard aluminum wires, the galvanized steel wire middle layer 102 is spirally connected to the hard aluminum wire inner layer 201, and the hard aluminum wire outer layer 203 is spirally connected to the hard aluminum wire inner layer 201. The galvanized steel wire outer layer 103 is spirally wound on the galvanized steel wire middle layer 102 in a direction opposite to the winding direction of the galvanized steel wire middle layer 102; the hard aluminum wire inner layer 201 is spirally wound on the galvanized steel wire outer layer 103 in a direction opposite to the winding direction of the galvanized steel wire outer layer 103; the hard aluminum wire middle layer 202 is spirally wound on the hard aluminum wire inner layer 201 in a direction opposite to the winding direction of the hard aluminum wire inner layer 201; the hard aluminum wire outer layer 203 is spirally wound on the hard aluminum wire middle layer 202 in a direction opposite to the winding direction of the hard aluminum wire middle layer 202.

[0052] The diameter of the galvanized steel wire is 2 mm. After testing, the tensile strength of the galvanized steel wire is 1450 MPa, the stress at 1% elongation is 1310 MPa, and the elongation after fracture is 2.9%.

[0053] The diameter of the hard aluminum wire is 4 mm, and the hard aluminum wire is composed of the following components in mass percentage: Fe 0.23%, and the balance is Al and inevitable impurities, with a single impurity ≤0.05% and a total impurity content ≤0.1%.

[0054] The manufacturing method of steel core high conductivity aluminum stranded wire for overhead conductor comprises the following steps in sequence:

[0055] Step 1: Melt and prepare aluminum liquid at 700℃ according to the composition and mass percentage of hard aluminum wire;

[0056] Step 2: Use argon gas with a purity of 99.99% and a refining agent accounting for 0.2% of the weight of the aluminum liquid to spray and refine the aluminum liquid in the smelting furnace for 20 minutes to remove the slag, and then scrape off the slag on the surface of the aluminum liquid;

[0057] Step 3: A mixed gas consisting of argon with a purity of 99.99% and chlorine with a purity of 99.99% is introduced through the air-permeable brick installed at the bottom of the smelting furnace to refine the aluminum liquid for 10 minutes to remove hydrogen. The volume percentage of chlorine in the mixed gas is 5%, and the flow rate of the mixed gas is 2 cubic meters / minute;

[0058] Step 4: introducing the aluminum liquid in the smelting furnace into the launder, and making the aluminum liquid flow through the degassing box and the tubular filter box arranged on the launder in turn for online dehydrogenation and slag removal treatment, the rotation speed of the graphite rotor in the degassing box is 600 rpm, the gas flow rate on the graphite rotor is 2 cubic meters / hour, the gas pressure is 1MPa, and the gas is a mixed gas composed of argon with a purity of 99.99% and chlorine with a purity of 99.99%, and the volume percentage of chlorine in the mixed gas is 5%;

[0059] Step 5: Under the conditions of a casting wheel speed of 28 rpm and a cooling water flow rate of 9 liters / minute, the 680°C aluminum liquid is continuously cast and extruded into a round aluminum rod with a diameter of 9.5 mm;

[0060] Step 6: Pull the round aluminum rod into a 4mm diameter hard aluminum wire;

[0061] Step 7: Twisting the hard aluminum wire and the galvanized steel wire to obtain the steel core high conductivity aluminum stranded wire for the overhead conductor.

[0062] Embodiment 3:

[0063] A steel core high conductivity aluminum stranded wire for overhead conductors, such as Figure 3As shown, in order from the center to the outside, a central galvanized steel wire 101, a galvanized steel wire middle layer 102, a galvanized steel wire outer layer 103, a hard aluminum wire inner layer 201, a hard aluminum wire middle layer 202 and a hard aluminum wire outer layer 203 are sequentially arranged, the galvanized steel wire middle layer 102 is composed of 6 galvanized steel wires, the galvanized steel wire outer layer 103 is composed of 12 galvanized steel wires, the hard aluminum wire inner layer 201 is composed of 11 hard aluminum wires, the hard aluminum wire middle layer 202 is composed of 17 hard aluminum wires, the hard aluminum wire outer layer 203 is composed of 23 hard aluminum wires, the galvanized steel wire middle layer 102 is spirally connected to the hard aluminum wire inner layer 201, and the hard aluminum wire outer layer 203 is spirally connected to the hard aluminum wire inner layer 201. The galvanized steel wire outer layer 103 is spirally wound on the galvanized steel wire middle layer 102 in a direction opposite to the winding direction of the galvanized steel wire middle layer 102; the hard aluminum wire inner layer 201 is spirally wound on the galvanized steel wire outer layer 103 in a direction opposite to the winding direction of the galvanized steel wire outer layer 103; the hard aluminum wire middle layer 202 is spirally wound on the hard aluminum wire inner layer 201 in a direction opposite to the winding direction of the hard aluminum wire inner layer 201; the hard aluminum wire outer layer 203 is spirally wound on the hard aluminum wire middle layer 202 in a direction opposite to the winding direction of the hard aluminum wire middle layer 202.

[0064] The diameter of the galvanized steel wire is 1.8 mm. After testing, the tensile strength of the galvanized steel wire is 1471 MPa, the stress at 1% elongation is 1318 MPa, and the elongation after fracture is 2.7%.

[0065] The diameter of the hard aluminum wire is 3.5 mm, and the hard aluminum wire is composed of the following components in mass percentage: Fe 0.27%, and the balance is Al and inevitable impurities, with a single impurity ≤0.05% and a total impurity content ≤0.1%.

[0066] The manufacturing method of steel core high conductivity aluminum stranded wire for overhead conductor comprises the following steps in sequence:

[0067] Step 1: Melt and prepare aluminum liquid at 720℃ according to the composition and mass percentage of hard aluminum wire;

[0068] Step 2: Use argon gas with a purity of 99.99% and a refining agent accounting for 0.1% of the weight of the aluminum liquid to spray and refine the aluminum liquid in the smelting furnace for 10 minutes to remove the slag, and then scrape off the slag on the surface of the aluminum liquid;

[0069] Step 3: A mixed gas consisting of argon with a purity of 99.99% and chlorine with a purity of 99.99% is introduced through the air-permeable brick installed at the bottom of the smelting furnace to remove hydrogen from the aluminum liquid for 20 minutes. The volume percentage of chlorine in the mixed gas is 3%, and the flow rate of the mixed gas is 1 cubic meter / minute;

[0070] Step 4: introducing the aluminum liquid in the smelting furnace into the launder, and making the aluminum liquid flow through the degassing box and the tubular filter box arranged on the launder in turn for online dehydrogenation and slag removal treatment, the rotation speed of the graphite rotor in the degassing box is 700 rpm, the gas flow rate on the graphite rotor is 1 cubic meter / hour, the gas pressure is 0.8MPa, and the gas is a mixed gas composed of argon with a purity of 99.99% and chlorine with a purity of 99.99%, and the volume percentage of chlorine in the mixed gas is 3%;

[0071] Step 5: Under the conditions of a casting wheel speed of 28 rpm and a cooling water flow rate of 11 liters / minute, the 690°C aluminum liquid is continuously cast and extruded into a round aluminum rod with a diameter of 9.5 mm;

[0072] Step 6: Pull the round aluminum rod into a hard aluminum wire with a diameter of 3.5 mm;

[0073] Step 7: Twisting the hard aluminum wire and the galvanized steel wire to obtain the steel core high conductivity aluminum stranded wire for the overhead conductor.

[0074] In Examples 1-3, the refining agent in step 2 is composed of the following components in mass percentage: ZnCl2 44.6%, K2CO3 25.8%, NaNO3 7.9%, KF 10.5%, K2SO4 7.4%, and Li2SO4 3.8%. The production method of the refining agent comprises the following steps in sequence: (1) selecting ZnCl2, K2CO3, NaNO3, KF, K2SO4, and Li2SO4 with a purity of ≥99.8% as raw materials for batching according to the composition and mass percentage of the refining agent; (2) heating the raw materials at 1150°C to melt under the protection of argon gas with a purity of 99.99%, and then cooling and solidifying them into a bulk refining agent; (3) crushing the bulk refining agent into powder with a particle size of ≤2 mm to obtain the refining agent.

[0075] Comparative Example 1:

[0076] The structure of the steel core aluminum stranded wire, the composition of the hard aluminum wire and the manufacturing method are the same as those in Example 1, except that the refining agent used in step 2 is a currently commonly used commercially available refining agent, and the refining agent is composed of the following components in mass percentage: 26.1% NaCl, 10.6% Na2SiF6, 17.1% Na2SO4, 6.9% CaF2, 9.3% C6Cl6, 14.3% Na2S2O3 and 15.7% NaF. The production method of the refining agent is to directly crush the raw materials into powder with a particle size of ≤2 mm and then mix them.

[0077] Comparative Example 2:

[0078] The structure of the steel core aluminum stranded wire, the composition of the hard aluminum wire and the manufacturing method are the same as those in Example 2, except that in step three, a mixed gas consisting of argon and chlorine is not introduced into the aluminum liquid in the furnace through the air-permeable bricks at the bottom of the furnace for dehydrogenation treatment.

[0079] Comparative Example 3:

[0080] The structure of the steel core aluminum stranded wire, the composition of the hard aluminum wire and the manufacturing method are the same as those in Example 3, except that in step 4, no tubular filter box is used to filter the aluminum liquid.

[0081] Verification Example 1:

[0082] The melting points of the refining agents used in Example 1 and Comparative Example 1 were respectively detected by using an OXFORD-DSC500 differential scanning calorimeter, and the results are shown in Table 1. As can be seen from Table 1, the melting start temperature of the refining agent in Example 1 is 290°C, and the melting end temperature is only 716°C. The melting start temperature of the refining agent in Comparative Example 1 is 564°C, and the melting end temperature is 1249°C. By comparison, it can be seen that the refining agent developed by the present invention has a lower melting start temperature and melting end temperature, indicating that the refining agent developed by the present invention is easier to dissolve in aluminum liquid, which is beneficial to improving the slag removal effect.

[0083] Table 1 Melting point of refining agent in Example 1 and Comparative Example 1

[0084] Example 1 Comparative Example 1 Melting start temperature / ℃ 290 564 Melting end temperature / ℃ 716 1249

[0085] Verification Example 2:

[0086] The hydrogen content and slag content of the aluminum liquid before casting and extrusion of Examples 1-3 and Comparative Examples 1-3 were tested on site using a HDA-V hydrogen meter and an Analyze PoDFA slag meter. The results are shown in Table 2. As can be seen from Table 2, the hydrogen content of the aluminum liquid in Examples 1-3 is less than 0.08 ml / 100 gAl, and the slag content is less than 0.05 mm 2 / kgAl. Comparative Example 1 uses a traditional commercial refining agent for in-furnace spray refining, Comparative Example 2 does not use a ventilation brick at the bottom of the furnace for refining, and Comparative Example 3 does not use a tubular filter box for filtration, resulting in the gas slag content of the aluminum liquid being significantly higher than that of the aluminum liquid in the embodiment. By comparison, it can be seen that the present invention can greatly improve the purity of the hard aluminum wire.

[0087] Table 2 Hydrogen content and slag content of aluminum liquid before casting

[0088] Hydrogen content / (ml / 100gAl) <![CDATA[Sludge content / (mm 2 / kg)]]> Example 1 0.076 0.047 Example 2 0.066 0.046 Example 3 0.074 0.041 Comparative Example 1 0.087 0.076 Comparative Example 2 0.129 0.056 Comparative Example 3 0.078 0.121

[0089] Verification Example 3:

[0090] Samples were taken from the hard aluminum wires of Examples 1-3 and Comparative Examples 1-3, and then the room temperature tensile mechanical properties, DC resistivity and conductivity of the hard aluminum wires were tested respectively. The results are shown in Table 3. As can be seen from Table 3, the tensile strength of the hard aluminum wires of Examples 1-3 is ≥200.9 MPa, the yield strength is ≥181.5 MPa, the elongation after fracture is ≥8.1%, and the DC resistivity at 20°C is ≤0.0272Ω·mm 2 / m, conductivity ≥ 63.5% IACS. Comparative Example 1 uses a traditional commercial refining agent for furnace spray refining, Comparative Example 2 does not use the furnace bottom air brick for ventilation refining, and Comparative Example 3 does not use a tubular filter box for filtration, resulting in the strength and conductivity of the hard aluminum wire being significantly lower than the strength and conductivity of the hard aluminum wire in the embodiment. By comparison, it can be seen that the present invention can greatly improve the strength and conductivity of the hard aluminum wire by improving the purity of the hard aluminum wire.

[0091] Table 3 Room temperature tensile mechanical properties, DC resistivity and conductivity of hard aluminum wire at 20℃

[0092]

[0093]

[0094] The present invention is described by way of embodiments, but does not constitute a limitation to the present invention. With reference to the description of the present invention, other changes to the disclosed embodiments are easily conceivable to professionals in the field, and such changes should fall within the scope defined by the claims of the present invention.

Claims

1. A steel core high conductivity aluminum stranded wire for overhead conductors, It is characterized in that A central galvanized steel wire, a galvanized steel wire middle layer, a galvanized steel wire outer layer, a hard aluminum wire inner layer, a hard aluminum wire middle layer and a hard aluminum wire outer layer are sequentially arranged from the center to the outside, the galvanized steel wire middle layer and the galvanized steel wire outer layer are respectively composed of a plurality of galvanized steel wires, the hard aluminum wire inner layer, the hard aluminum wire middle layer and the hard aluminum wire outer layer are respectively composed of a plurality of hard aluminum wires, the galvanized steel wire middle layer is spirally wound on the central galvanized steel wire, the galvanized steel wire outer layer is spirally wound on the galvanized steel wire middle layer in a direction opposite to the winding direction of the galvanized steel wire middle layer, the hard aluminum wire inner layer is spirally wound on the galvanized steel wire outer layer in a direction opposite to the winding direction of the galvanized steel wire outer layer, the hard aluminum wire middle layer is spirally wound on the hard aluminum wire inner layer in a direction opposite to the winding direction of the hard aluminum wire inner layer, and the hard aluminum wire outer layer is spirally wound on the hard aluminum wire middle layer in a direction opposite to the winding direction of the hard aluminum wire middle layer; the manufacturing method of steel core high conductivity aluminum stranded wire comprises the following steps in sequence: Step 1: Melt and prepare aluminum liquid at 700-720℃ according to the composition and mass percentage of hard aluminum wire; Step 2: Use argon gas with a purity of 99.99% and a refining agent accounting for 0.1-0.2% of the weight of the aluminum liquid to spray and refine the aluminum liquid in the smelting furnace for 10-20 minutes to remove the slag, and then scrape off the slag on the surface of the aluminum liquid; Step 3: A mixed gas consisting of argon with a purity of 99.99% and chlorine with a purity of 99.99% is introduced through the air-permeable brick installed at the bottom of the smelting furnace to refine the aluminum liquid for 10-20 minutes to remove hydrogen; Step 4: Introduce the aluminum liquid in the smelting furnace into the launder, and make the aluminum liquid flow through the degassing box and the tubular filter box arranged on the launder in sequence to perform online hydrogen removal and slag removal treatment; Step 5: Under the conditions of a casting wheel speed of 26-28 rpm and a cooling water flow rate of 9-11 liters / minute, the 680-690°C molten aluminum is continuously cast and extruded into a round aluminum rod with a diameter of 9.5 mm; Step 6: Pull the round aluminum rod into a hard aluminum wire with a diameter of 3-4 mm; Step 7: twisting the hard aluminum wire and the galvanized steel wire to obtain the steel core high conductivity aluminum stranded wire for the overhead conductor; The refining agent in step 2 is composed of the following components in percentage by mass: ZnCl 2 44.6%, K 2 CO 3 25.8%, NaNO 3 7.9%, KF 10.5%, K 2 SO 4 7.4%, Li 2 SO 4 3.8%; the production method of the refining agent comprises the following steps in sequence: (1) Select ZnCl with a purity of ≥99.8% according to the composition and mass percentage of the refining agent. 2 , K 2 CO 3 、NaNO 3 , KF, K 2 SO 4 , Li 2 SO 4 batching of raw materials; (2) The raw materials are heated and melted at 1150°C under the protection of argon gas with a purity of 99.99%, and then cooled and solidified into a bulk refining agent; (3) Crushing the bulk refining agent into powder with a particle size of ≤2 mm to obtain the refining agent.

2. The steel core high conductivity aluminum stranded wire for overhead conductor according to claim 1, It is characterized in that The diameter of the galvanized steel wire is 1.5-2 mm, the tensile strength of the galvanized steel wire is ≥1450 MPa, the stress at 1% elongation is ≥1310 MPa, and the elongation after fracture is ≥2.5%.

3. The steel core high conductivity aluminum stranded wire for overhead conductor according to claim 1, It is characterized in that The diameter of the hard aluminum wire is 3-4 mm, the tensile strength of the hard aluminum wire is ≥200.9 MPa, the yield strength is ≥181.5 MPa, the elongation after fracture is ≥8.1%, and the DC resistivity at 20°C is ≤0.0272 Ω•mm 2 / m, electrical conductivity ≥63.5%IACS.

4. The steel core high conductivity aluminum stranded wire for overhead conductor according to claim 1, It is characterized in that The hard aluminum wire is composed of the following components in mass percentage: Fe 0.23-0.27%, the balance being Al and inevitable impurities, with a single impurity ≤0.05% and a total impurity content ≤0.1%.

5. The steel core high conductivity aluminum stranded wire for overhead conductor according to claim 1, It is characterized in that The volume percentage of chlorine in the mixed gas in step 3 is 3-5%, and the flow rate of the mixed gas is 1-2 cubic meters per minute.

6. The steel core high conductivity aluminum stranded wire for overhead conductor according to claim 1, It is characterized in that In the step 4, the rotation speed of the graphite rotor in the degassing box is 600-700 rpm, the gas flow on the graphite rotor is 1-2 cubic meters per hour, the gas pressure is 0.8-1 MPa, and the gas is a mixed gas consisting of argon with a purity of 99.99% and chlorine with a purity of 99.99%, and the volume percentage of chlorine in the mixed gas is 3-5%.

Citation Information

Patent Citations

  • Super-high-strength galvanized steel strand for large-span transmission line and twisting method of galvanized steel strand

    CN109338770A

  • High-conductivity hard aluminum alloy conductor and manufacturing method thereof

    CN115821125A

  • Efficient and environment-friendly aluminum alloy refining agent and preparation method thereof

    CN117887994A

  • High-strength heat-resistant aluminum alloy stranded wire with extra-strong steel core

    CN216623857U