Termite decay resistant compound as well as preparation method and application thereof

By using anti-termite borer composites and pinephrine sulfonate in bamboo-based fiber composites, combined with epoxy resin, to form a termite-proof and insect-proof film, the problem of insufficient protection of bamboo against termite borer is solved, and the problem of significantly improved Termite borer resistance and mechanical properties.

CN118876172APending Publication Date: 2024-11-01GUANGDONG ACAD OF FORESTRY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410925353.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

When existing bamboo-based fiber composite materials face termite erosion, they have poor protective effects, which affects their structural and mechanical properties, and insect prevention measures are difficult to effectively prevent termite invasion in the long term.

Method used

The anti-termite borer composite is used, which consists of insect-proof agents, film-forming substances, zinc stearate and anti-deposition agents, combined with epoxy resin and pinephthalate esters, and is made of soaking and hot pressing molding technology. Form a termite-proof and insect-proof film, which significantly improves the termite-damaging properties and mechanical properties of bamboo-based fiber composites.

Benefits of technology

It significantly improves the anti-termite erosion effect of bamboo-based fiber composite materials, extends the protective effect, meets the outdoor and structural materials requirements in active termites, and significantly improves mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004938394320000071
    Figure BDA0004938394320000071
  • Figure BDA0004938394320000072
    Figure BDA0004938394320000072
  • Figure BDA0004938394320000081
    Figure BDA0004938394320000081
Patent Text Reader

Abstract

The invention belongs to the technical field of bamboo moth proofing, and provides a termite-corrosion-resistant compound and a preparation method and application thereof. The termite decay-resistant compound comprises an insect-resist agent, a film-forming substance, an organic solvent, zinc stearate and an anti-settling agent in specific parts by mass, the insect-resist agent is prepared from two or more of beta-cypermethrin, bifenthrin, fipronil and thiamethoxam. The film forming matter, the insect-resistant agent, the zinc stearate and the anti-settling agent are combined, a termite-resistant and insect-resistant film is formed in the soaking process of the bamboo-based fibers, and the bamboo-based fibers are prevented from being corroded by termites and other moths; the terpinyl p-aminobenzene sulfonate has certain viscosity and shear strength, and the mothproof effect is good; the termite-corrosion-resistant compound, the epoxy resin and the terpinyl p-aminobenzene sulfonate are combined, so that the termite-corrosion-resistant effect of the bamboo-based fiber composite material is remarkably improved, the mechanical property of the bamboo-based fiber composite material is improved, and the requirements of outdoor materials and structural materials in termite active areas are met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of bamboo anti-insect technology, and in particular to an anti-termite infestation composite material and a preparation method and application thereof. Background Art

[0002] Termites feed on wood or cellulose. They are polymorphic, social insects with strict division of labor. They are extremely destructive to bamboo-based fibers, wooden furniture, wooden floors, wooden buildings, etc. Termites have strong diffusion and adaptability, large colonies, and rapid destruction. Due to the biological characteristics of termites, almost all objects can be attacked by termites. The damage involves almost all fields, and the damage to housing construction, water conservancy projects, mountains and forests is particularly serious.

[0003] The main methods of preventing termites include physical barrier method and chemical barrier method, and the killing methods mainly include physical killing, chemical killing, biological killing, etc. In order to prevent bamboo from being eaten by termites, people usually combine bamboo with substances such as phenolic resin to prepare bamboo-based fiber composite materials. However, bamboo is still eaten by termites, which seriously affects the structural and mechanical properties of bamboo-based fiber composite materials.

[0004] Therefore, it is of great significance to study a method for obtaining an anti-termite damage composite material with good anti-termite damage effect and good durability, and improving the mechanical properties of bamboo-based fiber composite materials. Summary of the invention

[0005] The purpose of the present invention is to provide an anti-termite corrosion composite and a preparation method and application thereof in view of the deficiencies in the prior art.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0007] The present invention provides an anti-termite corrosion compound, comprising the following raw materials in parts by weight: 0.5 to 1.5 parts of an insect repellent, 8 to 20 parts of a film-forming substance, 20 to 40 parts of an organic solvent, 1 to 4 parts of zinc stearate, and 2 to 4 parts of an anti-settling agent;

[0008] The insect repellent comprises two or more of cypermethrin, bifenthrin, fipronil and thiamethoxam.

[0009] Preferably, the film-forming substance is alkyd resin and / or maleic resin.

[0010] Preferably, the organic solvent comprises one or more of butyl acetate, isopropanol, ethylene glycol and n-butanol; and the anti-settling agent is organic bentonite and / or fumed silica.

[0011] The present invention also provides a method for preparing the anti-termite infestation composite, comprising mixing an organic solvent, zinc stearate and an anti-settling agent to obtain a mixture, and mixing the mixture, an insect repellent and a film-forming substance to obtain the anti-termite infestation composite.

[0012] The invention also provides application of the anti-termite attack composite material in bamboo-based fiber composite materials.

[0013] Preferably, the anti-termite corrosion compound, epoxy resin, terpineol p-aminobenzenesulfonate and solvent are mixed to obtain a mixed solution, and the bamboo bundles are immersed in the mixed solution and then dried, assembled and hot-pressed.

[0014] Preferably, in the mixed solution, the mass concentration of the anti-termite corrosion compound is 0.1-1.5%, the mass concentration of the epoxy resin is 15-20%, and the mass concentration of pine ester p-aminobenzenesulfonate is 5-8%.

[0015] Preferably, the preparation method of pinyl para-aminobenzenesulfonate comprises the following steps: after mixing para-aminobenzenesulfonic acid and α-terpineol, adding concentrated sulfuric acid dropwise to react to obtain pinyl para-aminobenzenesulfonate.

[0016] Preferably, the mass ratio of p-aminobenzenesulfonic acid, α-terpineol and concentrated sulfuric acid is 21-22:13-14:4-5.

[0017] Preferably, after the soaking is completed, the bamboo bundle has a gum dipping rate of 75-85%; the drying temperature is 40-60° C., and the bamboo bundle is dried to a moisture content of 5-8%.

[0018] The beneficial effects of the present invention include the following:

[0019] 1) The film-forming substance, insect repellent, zinc stearate and anti-settling agent of the present invention are combined to form an anti-termite and anti-insect film during the soaking process of bamboo-based fibers, thereby preventing termites and other moths from infesting the bamboo-based fibers; terpineol p-aminobenzenesulfonate has a certain viscosity and shear strength, and has a good moth-proofing effect; the present invention significantly improves the anti-termite infestation effect of the bamboo-based fiber composite material by combining the anti-termite infestation composite material, epoxy resin and terpineol p-aminobenzenesulfonate, improves the mechanical properties thereof, and meets the requirements of outdoor materials and structural materials in termite-active areas.

[0020] 2) The insect repellent of the present invention has a good anti-termite effect under low concentration conditions, and the effect of a combination of two or more insect repellents is even better, significantly shortening the lethal time of termites; the anti-termite complex and pine oil p-aminobenzenesulfonate of the present invention can not only resist termites, but also have a killing effect, preventing the bamboo-based fiber composite material from being damaged by termites, and the effect is long-lasting and has good anti-loss performance. DETAILED DESCRIPTION

[0021] The present invention provides an anti-termite corrosion compound, comprising the following raw materials in parts by weight: 0.5 to 1.5 parts of an insect repellent, 8 to 20 parts of a film-forming substance, 20 to 40 parts of an organic solvent, 1 to 4 parts of zinc stearate, and 2 to 4 parts of an anti-settling agent;

[0022] The insect repellent comprises two or more of cypermethrin, bifenthrin, fipronil and thiamethoxam.

[0023] The anti-termite corrosion composite of the present invention contains 0.5 to 1.5 parts of the insect repellent, preferably 0.6 to 1.2 parts, more preferably 0.8 to 1.1 parts, and even more preferably 0.9 to 1.0 parts.

[0024] The anti-termite corrosion composite of the present invention comprises 8 to 20 parts of film-forming substances, preferably 10 to 18 parts, more preferably 12 to 16 parts, and even more preferably 14 to 15 parts.

[0025] In the present invention, the film-forming substance is preferably alkyd resin and / or maleic acid resin.

[0026] The anti-termite corrosion composite of the present invention contains 20 to 40 parts of organic solvent, preferably 25 to 35 parts, more preferably 28 to 32 parts, and even more preferably 30 parts.

[0027] In the present invention, the organic solvent preferably comprises one or more of butyl acetate, isopropanol, ethylene glycol and n-butanol.

[0028] The anti-termite corrosion composite of the present invention comprises 1 to 4 parts of zinc stearate, preferably 1.5 to 3.5 parts, and more preferably 2 to 3 parts.

[0029] The anti-termite corrosion composite of the present invention comprises 2 to 4 parts of an anti-settling agent, preferably 2.5 to 3.5 parts, and more preferably 3 parts.

[0030] In the present invention, the anti-settling agent is preferably organic bentonite and / or fumed silica.

[0031] The present invention also provides a method for preparing the anti-termite infestation composite, comprising mixing an organic solvent, zinc stearate and an anti-settling agent to obtain a mixture, and mixing the mixture, an insect repellent and a film-forming substance to obtain the anti-termite infestation composite.

[0032] The invention also provides application of the anti-termite attack composite material in bamboo-based fiber composite materials.

[0033] In the invention, the anti-termite corrosion compound, epoxy resin, pine oil p-aminobenzenesulfonate and solvent are mixed to obtain a mixed solution, and the bamboo bundle is soaked in the mixed solution and then dried, assembled and hot-pressed.

[0034] In the mixed solution of the present invention, the mass concentration of the anti-termite corrosion compound is preferably 0.1-1.5%, more preferably 0.5-1.2%, and more preferably 0.8-1.0%; the mass concentration of the epoxy resin is preferably 15-20%, more preferably 16-19%, and more preferably 17-18%; the mass concentration of pine oil p-aminobenzenesulfonate is preferably 5-8%, and more preferably 6-7%; the solvent of the mixed solution is preferably ethyl acetate or ethyl formate.

[0035] In the present invention, the mass concentration of the anti-termite infestation compound is in the range of 0.1-1.5%. As the concentration of the anti-termite infestation compound increases, the anti-termite death days gradually shorten and then tend to be stable.

[0036] In the present invention, the preparation method of pinyl para-aminobenzenesulfonate preferably comprises the following steps: after mixing p-aminobenzenesulfonic acid and α-terpineol, adding concentrated sulfuric acid dropwise for reaction to obtain pinyl para-aminobenzenesulfonate.

[0037] In the present invention, the mass ratio of the p-aminobenzenesulfonic acid, α-terpineol and concentrated sulfuric acid is preferably 21-22:13-14:4-5, and more preferably 21.5:13.5:4.5.

[0038] In the present invention, the rate of adding concentrated sulfuric acid is preferably 0.4 to 0.7 g / min, more preferably 0.5 to 0.6 g / min, stirring is performed during the adding process, and stirring is continued for 2.5 to 3.5 hours after the adding is completed to complete the reaction; the mass concentration of concentrated sulfuric acid is preferably 98 to 98.5%, more preferably 98.2 to 98.3%.

[0039] In the present invention, after soaking, the colloid impregnation rate of the bamboo bundle is preferably 75-85%, more preferably 78-82%, and more preferably 80%; the drying temperature is preferably 40-60°C, more preferably 45-55°C, and more preferably 50°C, and the bamboo bundle is preferably dried to a moisture content of 5-8%, and more preferably 6-7%.

[0040] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0041] In the embodiments and comparative examples, the epoxy resin is E-51 epoxy resin; and the alkyd resin is alkyd resin 3355-70.

[0042] Example 1

[0043] The anti-termite infestation compound comprises the following raw materials in parts by weight: 0.3 parts of high-efficiency cypermethrin, 0.3 parts of fipronil, 10 parts of alkyd resin, 25 parts of ethylene glycol, 2 parts of zinc stearate (particle size 10 μm), and 2 parts of organic bentonite. The ethylene glycol, zinc stearate, and organic bentonite are uniformly mixed to obtain a mixture, and the mixture, high-efficiency cypermethrin, fipronil, and alkyd resin are uniformly mixed to obtain an anti-termite infestation compound.

[0044] Para-aminobenzenesulfonic acid and α-pineneol are mixed in a mass ratio of 21:13 to obtain a mixed solution, and concentrated sulfuric acid with a mass concentration of 98% is added dropwise to the mixed solution at a rate of 0.4 g / min, the mass ratio of concentrated sulfuric acid to para-aminobenzenesulfonic acid is 4:21, and stirring is performed during the dropping process. After the dropping is completed, stirring is continued for 3 hours to complete the reaction, and the stirring rate is 300 r / min. The reaction product is extracted with ethyl acetate, and the ester layer is washed with a sodium bicarbonate aqueous solution with a mass concentration of 30%, and then dried with anhydrous sodium sulfate to obtain para-aminobenzenesulfonic acid pinene.

[0045] The anti-termite corrosion compound, epoxy resin, pine ester p-aminobenzene sulfonate and ethyl formate are mixed to obtain a mixed solution, in which the mass concentration of the anti-termite corrosion compound is 0.5%, the mass concentration of the epoxy resin is 15%, and the mass concentration of pine ester p-aminobenzene sulfonate is 5%. A bamboo bundle with a moisture content of 12% is soaked in the mixed solution to obtain a bamboo bundle with a dipping rate of 78%, and then dried at 45°C to obtain a bamboo bundle with a moisture content of 8%, and finally assembled, and hot-pressed at 150°C and 2MPa for 15 minutes to obtain a bamboo-based fiber composite material.

[0046] Example 2

[0047] The anti-termite infestation compound comprises the following raw materials in parts by weight: 0.4 parts of bifenthrin, 0.6 parts of fipronil, 18 parts of maleic acid resin, 35 parts of n-butanol, 4 parts of zinc stearate (particle size 10 μm), and 4 parts of fumed silica (particle size 40 nm). The n-butanol, zinc stearate, and fumed silica are uniformly mixed to obtain a mixture, and the mixture, bifenthrin, fipronil, and maleic acid resin are uniformly mixed to obtain an anti-termite infestation compound.

[0048] Para-aminobenzenesulfonic acid and α-pineneol are mixed in a mass ratio of 22:14 to obtain a mixed solution, and concentrated sulfuric acid with a mass concentration of 98.5% is added dropwise to the mixed solution at a rate of 0.6 g / min, and the mass ratio of concentrated sulfuric acid to para-aminobenzenesulfonic acid is 5:22. The mixture is stirred during the dropping process, and after the dropping is completed, the mixture is stirred for 3 hours to complete the reaction. The stirring rate is 400 r / min. The reaction product is extracted with ethyl acetate, and the ester layer is washed with a sodium bicarbonate aqueous solution with a mass concentration of 25%, and then dried with anhydrous sodium sulfate to obtain para-aminobenzenesulfonic acid pinene.

[0049] The anti-termite corrosion compound, epoxy resin, pine ester p-aminobenzene sulfonate and ethyl acetate are mixed to obtain a mixed solution, in which the mass concentration of the anti-termite corrosion compound is 0.8%, the mass concentration of the epoxy resin is 20%, and the mass concentration of pine ester p-aminobenzene sulfonate is 8%. A bamboo bundle with a moisture content of 10% is soaked in the mixed solution to obtain a bamboo bundle with a dipping rate of 82%, and then dried at 55°C to obtain a bamboo bundle with a moisture content of 6%, and finally assembled, and hot-pressed at 170°C and 2MPa for 8 minutes to obtain a bamboo-based fiber composite material.

[0050] Example 3

[0051] The anti-termite infestation compound comprises the following raw materials in parts by weight: 0.7 parts of thiamethoxam, 0.5 parts of fipronil, 15 parts of alkyd resin, 30 parts of butyl acetate, 3 parts of zinc stearate (particle size 10 μm), and 3 parts of organic bentonite. Butyl acetate, zinc stearate and organic bentonite are uniformly mixed to obtain a mixture, and the mixture, thiamethoxam, fipronil and alkyd resin are uniformly mixed to obtain an anti-termite infestation compound.

[0052] Para-aminobenzenesulfonic acid and α-pineneol are mixed in a mass ratio of 21.5:13.5, and concentrated sulfuric acid with a mass concentration of 98.3% is added dropwise to the mixture at a rate of 0.5 g / min. The mass ratio of concentrated sulfuric acid to para-aminobenzenesulfonic acid is 4.5:21.5. Stirring is carried out during the dropping process. After the dropping is completed, stirring is continued for 3 hours to complete the reaction. The stirring rate is 350 r / min. The reaction product is extracted with ethyl acetate, and the ester layer is washed with a sodium bicarbonate aqueous solution with a mass concentration of 28%, and then dried over anhydrous sodium sulfate to obtain para-aminobenzenesulfonic acid pinene.

[0053] The anti-termite corrosion compound, epoxy resin, pine ester p-aminobenzene sulfonate and ethyl acetate are mixed to obtain a mixed solution, in which the mass concentration of the anti-termite corrosion compound is 1.2%, the mass concentration of the epoxy resin is 18%, and the mass concentration of pine ester p-aminobenzene sulfonate is 7%. A bamboo bundle with a moisture content of 10% is soaked in the mixed solution to obtain a bamboo bundle with a dipping rate of 80%, and then dried at 50°C to obtain a bamboo bundle with a moisture content of 7%, and finally assembled, and hot-pressed at 160°C and 2MPa for 10 minutes to obtain a bamboo-based fiber composite material.

[0054] Comparative Example 1

[0055] The fipronil and organobentonite in Example 3 were omitted, thiamethoxam was changed to 1.2 parts, the mass concentration of the anti-termite corrosion composite in the mixed solution was changed to 2%, the mass concentration of the epoxy resin was changed to 25%, the bamboo bundle impregnation rate was changed to 70%, and the bamboo bundle with a moisture content of 10% was obtained by drying. The other conditions were the same as in Example 3.

[0056] Comparative Example 2

[0057] The fipronil and terpineol in Example 3 were omitted; the gum dipping rate of the bamboo bundle was changed to 90%, and the other conditions were the same as those in Example 3.

[0058] The bamboo-based fiber composite materials of Examples 1 to 3 and Comparative Examples 1 to 2 were subjected to termite resistance test and mechanical property test.

[0059] Anti-termite infestation performance: The bamboo-based fiber composite material was cut into 50mm×25mm×10mm specimens and tested according to GB / T 18260-2015. 25 sterilized culture bottles were respectively placed with 150g of dry river sand and vermiculite mixed matrix (the mass ratio of river sand and vermiculite was 9:1), 10g of ant nest material, and 30mL of distilled water, and divided into 5 groups, each with 5 culture bottles. After standing for 2h, the bamboo-based fiber composite materials of Examples 1 to 3 and Comparative Examples 1 to 2 were respectively placed, and 500 house termite workers were evenly placed in 25 culture bottles, and placed in a constant temperature and humidity chamber at 28°C and 80% relative humidity for 4 weeks. Each example and comparative example was repeated 5 times, and the bamboo-based fiber composite material was observed for infestation, and the anti-termite infestation grade was classified. The standards for the integrity level of the specimens after being damaged are as follows: Level 10: intact; Level 9.5: slight damage, with only 1 damage mark; Level 9: slight damage, with the cross-sectional area damaged by less than 3%; Level 8: moderate damage, with 3-10% of the cross-sectional area damaged; Level 7: relatively serious damage, with 10-30% of the cross-sectional area damaged; Level 6: serious damage, with 30-50% of the cross-sectional area damaged; Level 4: very serious damage, with 50-75% of the cross-sectional area damaged; Level 0: almost completely damaged.

[0060] Test for anti-leakage of reagents: Cut the bamboo-based fiber composite materials of Examples 1 to 3 and Comparative Examples 1 to 2 into samples of 50 mm × 25 mm × 10 mm, put the samples into a beaker filled with 300 mL of distilled water, and immerse the samples below the liquid level at all times. Wrap the beaker mouth with waterproof paper. Change the distilled water every 24 hours, and soak for 17 days at a temperature of 25°C and a relative humidity of 50%. Then test according to GB / T18260-2015, and repeat the test 3 times for each sample of the example and comparative example, observe the damage of the bamboo-based fiber composite materials after the loss of the reagent, and classify the anti-termite damage grade of the samples.

[0061] The termite resistance grades of the composite materials of Examples 1 to 3 and Comparative Examples 1 to 2 and the termite resistance grades after the loss of the agent are shown in Table 1.

[0062] Table 1 Results of termite resistance rating and termite resistance rating after agent loss

[0063]

[0064] According to GB / T 17657-2013 and GB / T 30364-2013 standards, the static bending strength, elastic modulus, 24h water absorption thickness expansion rate, horizontal shear strength, vertical shear strength and density of the bamboo-based fiber composite materials of Examples 1 to 3 and Comparative Examples 1 to 2 were tested. The test results are shown in Table 2.

[0065] Table 2 Mechanical properties test results of the composite materials of the embodiments and comparative examples

[0066]

[0067]

[0068] As can be seen from Table 1 and Table 2, the bamboo-based fiber composite material of the present invention has excellent anti-termite effect and mechanical properties, and has good anti-drainage performance of the agent. The present invention obtains an anti-termite composite with good anti-termite effect by reasonably selecting insect repellent, film-forming substance, organic solvent, zinc stearate, and anti-settling agent, and controlling their dosage, and soaking bamboo bundles with a mixed solution of the anti-termite composite, pine oil p-aminobenzenesulfonate, and epoxy resin, which significantly improves the anti-termite effect and mechanical properties of the bamboo-based fiber composite material.

[0069] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A composite material for resisting termite infestation, characterized in that: The invention comprises the following raw materials in parts by weight: 0.5 to 1.5 parts of insect repellent, 8 to 20 parts of film-forming substance, 20 to 40 parts of organic solvent, 1 to 4 parts of zinc stearate, and 2 to 4 parts of anti-settling agent; The insect repellent comprises two or more of cypermethrin, bifenthrin, fipronil and thiamethoxam.

2. The anti-termite damage composite according to claim 1, characterized in that: The film-forming substance is alkyd resin and / or maleic acid resin.

3. The anti-termite damage composite according to claim 1 or 2, characterized in that: The organic solvent comprises one or more of butyl acetate, isopropanol, ethylene glycol and n-butanol; the anti-settling agent is organic bentonite and / or fumed silica.

4. The method for preparing the anti-termite corrosion composite according to any one of claims 1 to 3, characterized in that: An organic solvent, zinc stearate and an anti-settling agent are mixed to obtain a mixture, and the mixture, an insect repellent and a film-forming substance are mixed to obtain an anti-termite corrosion composite.

5. Use of the anti-termite damage composite material according to any one of claims 1 to 3 in bamboo-based fiber composite materials.

6. The use according to claim 5, characterized in that: The anti-termite corrosion compound, epoxy resin, pine oil p-aminobenzene sulfonate and solvent are mixed to obtain a mixed solution, and the bamboo bundles are immersed in the mixed solution and then dried, assembled and hot-pressed.

7. The use according to claim 6, characterized in that: In the mixed solution, the mass concentration of the anti-termite corrosion compound is 0.1-1.5%, the mass concentration of the epoxy resin is 15-20%, and the mass concentration of pine ester p-aminobenzenesulfonate is 5-8%.

8. The use according to claim 6 or 7, characterized in that: The preparation method of pinyl para-aminobenzenesulfonate comprises the following steps: mixing para-aminobenzenesulfonic acid and alpha-terpineol, and then dropping concentrated sulfuric acid to react to obtain pinyl para-aminobenzenesulfonate.

9. The use according to claim 8, characterized in that: The mass ratio of the p-aminobenzenesulfonic acid, α-terpineol and concentrated sulfuric acid is 21-22:13-14:4-5.

10. The use according to claim 6, characterized in that: After the soaking is completed, the bamboo bundle has a gum soaking rate of 75-85%. The drying temperature is 40-60° C., and the bamboo bundle is dried until the moisture content is 5-8%.