Preparation process for etching PTFE (Polytetrafluoroethylene) multi-cavity microcatheter

PTFE multi-cavity microcatheters were prepared through emulsion polymerization reaction and impregnation spraying process. Combined with automatic control and etching stabilizers, the problems of unstable specifications and low production efficiency in the preparation of PTFE multi-cavity tubes were solved, and efficient and stable microcatheter molding was achieved. and in-depth application.

CN118876310APending Publication Date: 2024-11-01XIANJU ECO ADVANCED MATERIAL TECHNOLOGY CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411222986.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The existing PTFE multi-lumen tube preparation process has problems such as unstable specifications and sizes, small cavity sizes and thin walls, low production efficiency and high safety risks, especially in the in-depth application of the medical field.

Method used

The PTFE dispersion was obtained through emulsion polymerization, and the multi-cavity microcatheters were prepared in combination with the immersion and spraying process. The automatic control system and the etching stabilizer optimization process were used to achieve accurate molding and efficient production of the microcatheters.

Benefits of technology

The inner cavity size of the PTFE multi-cavity microcatheter is controlled at 0.2~1.0mm, the wall thickness is controlled at 5μm~10μm, and the outer diameter is controlled at 0.5~1.8mm, which significantly improves production efficiency and molding stability and reduces safety risks. Meets the size and functional requirements of the microcatheter.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118876310A_ABST
    Figure CN118876310A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation process of an etched PTFE (Polytetrafluoroethylene) multi-cavity microcatheter, and relates to the technical field of PTFE tubes. The method comprises the following steps: firstly, preparing and coating two layers of PTFE (Polytetrafluoroethylene) emulsions with different proportions on a silver-plated copper wire to form a primary coating; then the coating is fixed through drying and pre-sintering; the roundness is optimized through coating of a second layer of emulsion; the roundness and quality are further improved through a mold and high-temperature sintering; and finally, carrying out post-treatment processes such as etching, cleaning, drying and the like, and combining with automatic cutting or rolling to obtain the PTFE multi-cavity micro-catheter meeting the requirements. The whole process relates to a plurality of links such as emulsion preparation, coating, heat treatment, etching and post-treatment. The method is stable in process, the multi-cavity microcatheter is good in formability, the relative position of the inner cavity is stable, operation is convenient, and batch production can be rapidly achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of PTFE tubes, in particular to a preparation process of an etched PTFE multi-lumen micro-catheter. Background Art

[0002] Due to the excellent lubricity of PTFE catheters and the good torsion and transmission properties of its products during use, it has been widely used and deeply explored in many fields, especially in the medical field. With the rapid development of science and technology, catheters, as one of the most widely used varieties in medical processes, have more and more functional requirements, which are usually realized in the form of multiple cavities and multiple functions. Moreover, as the use continues to deepen, from the digestive system to the coronary arteries, nerves, etc., the requirements for its specifications and sizes are getting higher and higher. In the process of balancing the function and specification of catheters, it is often impossible to have both the best function and the best size. Large-sized catheters can accommodate cavities with different functions, while small-sized catheters usually appear in the form of a single function, which is mainly limited by the PTFE molding process. Due to the insoluble and infusible characteristics of PTFE, the PTFE catheters currently used in medical applications are mainly extruded in a manner similar to powder metallurgy. The product specifications prepared by this molding processing method are not only related to the raw materials and equipment, but also the product size and size fluctuation range are relatively large, which is mainly reflected in the inner diameter and wall thickness. Moreover, this form is basically unable to prepare multi-lumen tubes with smaller specifications. Through the transformation of processing technology, not only can the catheter be guaranteed to have extremely small specifications and dimensions, but it can also have multi-lumen functions at this size, which is of great significance for the in-depth application of PTFE in the medical field.

[0003] At present, PTFE multi-lumen tubes are mainly prepared by extrusion. A certain amount of PTFE resin is mixed and matured with a calculated amount of lubricating agent, and then preformed to obtain a preform blank. The blank is placed in an extruder, and a matching multi-lumen tube mold is installed for extrusion. The PTFE multi-lumen tube is obtained by sintering and cutting. After the PTFE multi-lumen tube is post-processed such as etching, the finished PTFE multi-lumen tube is obtained.

[0004] At present, PTFE multi-lumen tubes are mainly prepared by extrusion in a form similar to powder metallurgy, and the PTFE multi-lumen tubes obtained in this form often require that the internal cavity must have a certain size. This is because of the limitation of the mold. When the structural components of the mold are too small, they cannot withstand the high lateral pressure during the extrusion process and eccentricity, bending and other abnormalities occur, which will cause the extruded tube to be unable to form, which not only limits the size of the internal cavity of the multi-lumen tube, but also makes the overall size of the multi-lumen tube larger; and the multi-lumen tubes obtained in this form often have a certain deviation from the requirements in relative position, and the stability is poor, which makes the multi-lumen tubes eliminated in the process of back-end instrument assembly. In addition, the extrusion molding of multi-lumen tubes requires not only reasonable mold design, but also strict requirements for mold manufacturing and assembly. During the whole process, if there is a certain error in any link such as design, manufacturing or assembly, it is very likely to cause a large difference between the product specifications and requirements, or even fail to obtain the product, resulting in a large loss. In short, the multi-lumen tubes prepared in the form of extrusion not only have many defects, but can only prepare PTFE multi-lumen tubes with certain specifications. This greatly restricts the application of PTFE multi-lumen tubes in a deeper level. Summary of the invention

[0005] According to the different polymerization processes of tetrafluoroethylene (TFE), PTFE resin suitable for different molding and processing processes is obtained. Among them, the PTFE dispersion resin and PTFE dispersion liquid obtained by emulsion polymerization, the PTFE dispersion resin is prepared into a PTFE extrusion tube through a processing process similar to powder metallurgy, and the PTFE dispersion liquid is subjected to processes such as impregnation and spraying to obtain products with different functions. And the impregnation processing method of the PTFE dispersion liquid is combined with the form of multi-cavity molding to obtain a multi-cavity microcatheter of PTFE. The tube wall formed by the PTFE dispersion liquid impregnation is extremely thin, and the wall thickness and its fluctuation range are much smaller than those of the extruded tube, which creates innate conditions for the preparation of the PTFE microcatheter. By optimizing the process conditions, the molding of this microcatheter can be arranged as required, and a plurality of microcatheters of the same or different specifications are centrally arranged to form a multi-cavity microcatheter of PTFE. After the formed microcatheter is subjected to post-processing such as etching, an etched PTFE multi-cavity microcatheter is obtained. Under this process condition, the inner cavity size of the etched PTFE microcatheter obtained can be controlled within 0.2-1.0 mm, and the tolerance can be controlled within 10 μm. The wall thickness between the inner cavities can be controlled within 5 μm-10 μm, and the tolerance can be controlled within 3 μm. The outer diameter of the multi-lumen microcatheter can be controlled within 0.5-1.8 mm, which embodies the advantages of excellent size advantage and both functionality.

[0006] The main process of this process is:

[0007] 70-80 parts of PTFE dispersion, 0.1-2.0 parts of defoamer, 0.1-2.0 parts of wetting agent, 0.1-1.0 parts of leveling agent, 0.1-0.5 parts of thickener and 20-30 parts of water are prepared to obtain PTFE emulsion 1, and the PTFE emulsion 1 is added to the emulsion tank 1. The emulsion 1 in the emulsion tank 1 is transported to the emulsion mold 1 through the automatic control system of the emulsion tank 1, and the emulsion monitor is used to control so that the emulsion 1 in the mold 1 is always maintained at a set height;

[0008] 45-55 parts of PTFE dispersion, 0.1-1.0 parts of defoamer, 0.1-1.0 parts of wetting agent, 0.1-2.0 parts of leveling agent and 45-50 parts of water are prepared to obtain PTFE emulsion 2, and the PTFE emulsion 2 is added to the emulsion tank 2. The emulsion 2 in the emulsion tank 2 is transported to the emulsion mold 2 through the automatic control system of the emulsion tank 2, and the emulsion monitor is used to control so that the emulsion 2 in the mold 2 is always maintained at a set height;

[0009] According to the requirements of the PTFE multi-lumen microcatheter, silver-plated copper wires of appropriate specifications are selected, and silver-plated copper wires of various specifications are unwound through the unwinding system, and silver-plated copper wires of different specifications are positioned upward through the guide positioning block;

[0010] The silver-plated copper wires of various specifications are arranged in a directional manner according to the spacing requirements through the guide positioning block to form an orderly moving silver-plated copper wire combination, which passes through a mold containing PTFE emulsion. The emulsion is sealed by a silicone pad at the bottom of the mold, and holes are made at the corresponding positions of the silicone pad according to the arrangement positions of the silver-plated copper wires of different specifications, so that the silver-plated copper wires of different specifications can pass through the silicone pad smoothly;

[0011] The silver-plated copper wire assembly passing through the silicone pad is coated with the emulsion in the mold 1, and a PTFE emulsion layer is formed on the surface of the silver-plated copper wire and between the silver-plated copper wires. The silver-plated copper wire assembly coated with the PTFE emulsion enters the drying-pre-sintering furnace upward for drying and pre-sintering;

[0012] After drying and pre-sintering, a PTFE coating is formed on the surface of the silver-plated copper wire and between the wires. The silver-plated copper wire assembly with PTFE coating continues to move upward into the emulsion mold 2. The lower end of the emulsion mold 2 is matched with a heating tool, so that when the silver-plated copper wire assembly with PTFE coating passes through the lower end of the mold, it is coated with emulsion 2 to obtain a PTFE multi-lumen microcatheter with optimized roundness;

[0013] The PTFE multi-lumen microcatheter with optimized roundness continues to move upward through the emulsion 2 and then through the mold 3, and the roundness of the PTFE multi-lumen microcatheter is further optimized;

[0014] The PTFE multi-lumen micro-catheter with further optimized roundness enters the sintering furnace upwards. After high-temperature sintering, the PTFE multi-lumen micro-catheter has the strength characteristics that can be used;

[0015] The sintered PTFE multi-lumen microcatheter continues to move upward. When the PTFE multi-lumen microcatheter approaches the guide positioning block at the upper end, the guide positioning block fixed at the upper end is removed, and the subsequent upper end positioning is performed by the formed PTFE multi-lumen microcatheter itself;

[0016] The PTFE multi-lumen microcatheter then passes through a pulley with a small angle change and enters the automatic etching system for etching;

[0017] The etched PTFE multi-lumen microcatheter enters the automatic cleaning system and drying system in turn for cleaning and drying;

[0018] The dried etched PTFE multi-lumen microcatheter passes through a tension control system and enters a traction cutting machine for fixed-length cutting or a winding machine for winding;

[0019] The cut etched PTFE multi-lumen microcatheter can be obtained by extracting the core shaft to obtain a PTFE multi-lumen microcatheter with a small size and meeting the functional requirements.

[0020] Furthermore, the solid content of the PTFE dispersion is 50-70wt%.

[0021] Furthermore, the defoamer is an organosilicon defoamer, selected from at least one of BYK-094 and BYK-024.

[0022] Furthermore, the wetting agent is a nonionic surfactant, selected from at least one of Synperonic OP-10 and Tritont X100.

[0023] Furthermore, the leveling agent is a fluorocarbon leveling agent, selected from at least one of Capstone FS-3000 and Capstone FS-3100.

[0024] Furthermore, the thickener is a water-soluble thickener selected from CMC.

[0025] Furthermore, the temperature of the emulsion 1 and the emulsion 2 is controlled in the range of 15 to 30°C.

[0026] Furthermore, the core wire is selected from any one of copper wire, aluminum wire, silver wire, zinc-copper alloy wire, tin-copper alloy wire, silver-plated copper wire, and chrome-plated copper wire, and the coating thickness of the coated core wire is not less than 2 μm.

[0027] Furthermore, the drying-pre-sintering furnace consists of three sections, and the temperature rises in a step-by-step manner, the temperature of the first section is set at 100-150°C, the temperature of the second section is set at 160-200°C, and the temperature of the third section is set at 210-260°C, wherein an exhaust system is installed on the top of the sintering furnace to control the outlet temperature;

[0028] Furthermore, the sintering furnace is composed of three sections, and the temperature rises in a step-by-step manner, the temperature of the first section is set at 150-250°C, the temperature of the second section is set at 300-360°C, and the temperature of the third section is set at 380-450°C, wherein an exhaust system is installed on the top of the sintering furnace to control the outlet temperature;

[0029] Furthermore, the drying furnace consists of two sections, and the temperature rises in a step-by-step manner. The temperature of the first section is set at 100-150°C, and the temperature of the second section is set at 160-200°C. An exhaust system is installed on the top of the drying furnace to control the outlet temperature.

[0030] Furthermore, the etching liquid in the automatic etching system is a sodium naphthalene etching liquid, and an etching stabilizer is added to the etching liquid, and the added amount is 0.1-1wt% of the total amount of the etching liquid. The preparation method of the etching stabilizer is:

[0031] T1: By weight, 19-38 parts of 2,7-naphthyldithiol, 8-16 parts of allyl-1,1,2,2-tetrafluoroethyl ether, 2-5 parts of triethylamine, and 200-300 parts of N-methylpyrrolidone are placed in a stirring kettle, the reaction temperature is controlled at 65-75°C, and the reaction time is 3-12 hours.

[0032] T2: Add 10-20 parts of 1-(2-propenyl)-2-benzimidazolone, maintain the temperature at 65-75°C and stir the reaction for 1-4 hours, and distill to remove N-methylpyrrolidone to obtain an etching stabilizer.

[0033] Etching stabilizer reaction mechanism:

[0034] First, a thiol-allyl addition reaction was carried out, wherein 2,7-naphthyl dithiol reacted with allyl-1,1,2,2-tetrafluoroethyl ether to form a preliminary addition product. Then, 2,7-naphthyl dithiol and 1-(2-propenyl)-2-benzimidazolone were subjected to a thiol-propenyl addition reaction again to form the final naphthalene compound containing tetrafluoroethyl ether-benzimidazolone.

[0035] The etching stabilizer utilizes the benzimidazolone and tetrafluoroethyl ether parts in its structure to effectively improve the stability and accuracy of the electron beam etching process. Specifically:

[0036] 1. Improve etching accuracy: By optimizing the chemical structure, the molecular chain breakage under high-energy radiation is reduced, thereby reducing etching deviation.

[0037] 2. Enhanced chemical resistance: The introduction of tetrafluoroethyl ether enhances the chemical resistance of the material and improves the chemical stability during the etching process.

[0038] 3. Improve thermal stability: The thermal stability of benzimidazolone makes it difficult for the material to undergo thermal decomposition during high-temperature treatment, ensuring the safety and continuity of the etching process.

[0039] Technical effects:

[0040] Compared with traditional methods, this method has the following advantages:

[0041] 1. The technical principle is simple, the operation is convenient, and batch production can be realized quickly;

[0042] 2. The process is stable, the multi-lumen microcatheter has good formability, and the relative position of the inner cavity is stable.

[0043] 3. Not limited by small cavity size and thin wall thickness, design according to demand;

[0044] 4. Compared with PTFE extrusion, it has high production efficiency and can produce continuously and stably;

[0045] 5. Low safety risk. Operators are not exposed to mechanical injury risks such as die head movement and mold clamping during extrusion. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] Figure 1 It is a system diagram of the present invention;

[0047] In the figure: 1. Silver-plated copper wire assembly; 2. Guide positioning block; 3. Mold 1; 4. Drying-pre-sintering furnace; 5. Exhaust fan; 6. Mold 2; 7. Mold 3; 8. Sintering furnace; 9. Guide positioning block (removable); 10. Automatic etching system; 11. Cleaning system; 12. Drying furnace; 13. Etched PTFE multi-lumen tube; 14. Tension control system; 15. Traction cutting machine or winder.

[0048] Figure 2 This is a schematic diagram of the guide positioning block;

[0049] Figure 3 This is a schematic diagram for disassembling the guide positioning block;

[0050] Figure 4 is a schematic diagram of an emulsion mold 1;

[0051] Figure 5 is a schematic diagram of an emulsion mold 2;

[0052] Figure 6 Schematic diagram of the mold for surface optimization;

[0053] Figure 7 It is a schematic diagram of etching a rotating disk;

[0054] Figure 8 It is a schematic diagram of the nitrogen rotating disk;

[0055] Fig. 9 Schematic diagram of the cleaning system. DETAILED DESCRIPTION

[0056] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Unless otherwise expressly stated, throughout the specification and claims, the term "including" or its variations such as "comprising" or "including" will be understood to include the stated elements or components, without excluding other elements or other components.

[0057] In addition, in order to better illustrate the present invention, numerous specific details are provided in the specific embodiments below. It should be understood by those skilled in the art that the present invention can also be implemented without certain specific details. In some embodiments, raw materials, elements, methods, means, etc. well known to those skilled in the art are not described in detail, so as to highlight the main purpose of the present invention.

[0058] Test method:

[0059] 1. Process stability and formability test

[0060] Test method: Under mass production conditions, select 100 PTFE multi-lumen microcatheters produced continuously, use a high-precision microscope to check the relative position and molding integrity of the inner cavity, and evaluate the stability of the inner cavity. Record the number of molding defects and the inner cavity position deviation of each catheter.

[0061] 2. Test of relative position stability of multi-lumen microcatheter lumens

[0062] Test method: Use a laser rangefinder to measure the inner cavity of the multi-lumen tube after molding, especially the inner cavity size and relative position after multiple coatings and sintering, to ensure that the relative position of each cavity is consistent. Test any 50 consecutive catheters during the production process.

[0063] 3.Production efficiency test

[0064] Test method: Compare the production efficiency of the traditional PTFE extrusion method and this process. Record the output of the two methods in the same time, as well as the downtime and production stability of each method.

[0065] Example 1

[0066] A preparation process of an etched PTFE multi-lumen microcatheter, the operation steps of which are as follows:

[0067] S1: 70 kg of PTFE dispersion, 0.1 kg of defoamer, 0.1 kg of wetting agent, 0.1 kg of leveling agent, 0.1 kg of thickener and 20 kg of water are prepared to obtain PTFE emulsion 1, and the PTFE emulsion 1 is added to the emulsion tank 1, and the emulsion 1 in the emulsion tank 1 is transported to the emulsion mold 1 through the automatic control system of the emulsion tank 1, and the emulsion monitor is used to control so that the emulsion 1 in the mold 1 is always maintained at a set height;

[0068] S2: 45 kg of PTFE dispersion, 0.1 kg of defoamer, 0.1 kg of wetting agent, 0.1 kg of leveling agent and 45 kg of water are prepared to obtain PTFE emulsion 2, and the PTFE emulsion 2 is added to the emulsion tank 2, and the emulsion 2 in the emulsion tank 2 is transported to the emulsion mold 2 through the automatic control system of the emulsion tank 2, and the emulsion monitor is used to control so that the emulsion 2 in the mold 2 is always maintained at a set height;

[0069] S3: Select silver-plated copper wires of appropriate specifications, unwind the silver-plated copper wires of various specifications through the unwinding system, and position the silver-plated copper wires of different specifications upward through the guide positioning block. The silver-plated copper wires of various specifications passing through the guide positioning block are arranged in accordance with the spacing requirements and in a directional manner to form an orderly moving silver-plated copper wire combination, and the silver-plated copper wire combination passes through a mold containing PTFE emulsion;

[0070] S4: The silver-plated copper wire combination passing through the silicone pad is coated with the emulsion in the mold 1, and a PTFE emulsion layer is formed on the surface of the silver-plated copper wire and between the silver-plated copper wires. The silver-plated copper wire combination coated with the PTFE emulsion enters the drying-pre-sintering furnace upward for drying and pre-sintering;

[0071] S5: After drying and pre-sintering, a PTFE coating is formed on the surface of the silver-plated copper wire and between the wires. The silver-plated copper wire assembly with the PTFE coating continues to move upward into the emulsion mold 2. The lower end of the emulsion mold 2 is matched with a heating tool, so that the silver-plated copper wire assembly with the PTFE coating is coated with the emulsion 2 when passing through the lower end of the mold to obtain a PTFE multi-lumen microcatheter with optimized roundness;

[0072] S6: The PTFE multi-lumen microcatheter after roundness optimization continues to move upward through emulsion 2, and then through mold 3, the roundness of the PTFE multi-lumen microcatheter is further optimized, and then after high-temperature sintering, the sintered PTFE multi-lumen microcatheter continues to move upward, and when the PTFE multi-lumen microcatheter is close to the guide positioning block at the upper end, the guide positioning block fixed at the upper end is removed, and the subsequent upper end positioning is performed by the formed PTFE multi-lumen microcatheter itself, and then the PTFE multi-lumen microcatheter passes through a pulley with a smaller angle change and enters the automatic etching system for etching. The etched PTFE multi-lumen microcatheter moves upward and enters the automatic cleaning system and the drying system in turn for cleaning and drying. The etched PTFE multi-lumen microcatheter after drying passes through the tension control system and enters the traction cutting machine for fixed-length cutting or the winding machine for winding. The etched PTFE multi-lumen microcatheter after cutting can be obtained by extracting the core shaft to obtain a PTFE multi-lumen microcatheter with a small size and meeting the functional requirements.

[0073] The solid content of the PTFE dispersion is 50 wt %.

[0074] The defoamer is an organosilicon defoamer selected from BYK-094.

[0075] The wetting agent is a nonionic surfactant selected from Synperonic OP-10.

[0076] The leveling agent is a fluorocarbon leveling agent selected from Capstone FS-3000.

[0077] The thickener is a water-soluble thickener selected from CMC.

[0078] The temperature control range of the emulsion 1 and the emulsion 2 is 15°C.

[0079] The core wire is selected from copper wire, and the coating thickness of the coated core wire is not less than 2 μm.

[0080] The drying-pre-sintering furnace consists of three sections, and the temperature rises in steps. The temperature of the first section is set to 100°C, the temperature of the second section is set to 160°C, and the temperature of the third section is set to 210°C, wherein an exhaust system is installed on the top of the sintering furnace to control the outlet temperature; the sintering furnace consists of three sections, and the temperature rises in steps. The temperature of the first section is set to 150°C, the temperature of the second section is set to 300°C, and the temperature of the third section is set to 380°C, wherein an exhaust system is installed on the top of the sintering furnace to control the outlet temperature; the drying furnace consists of two sections, and the temperature rises in steps. The temperature of the first section is set to 100°C, and the temperature of the second section is set to 160°C, wherein an exhaust system is installed on the top of the drying furnace to control the outlet temperature.

[0081] The etching liquid in the automatic etching system is a sodium naphthalene etching liquid, and an etching stabilizer is added to the etching liquid in an amount of 0.1wt% of the total amount of the etching liquid. The preparation method of the etching stabilizer is:

[0082] T1: 19 g of 2,7-naphthyldithiol, 8 g of allyl-1,1,2,2-tetrafluoroethyl ether, 2 g of triethylamine, and 200 g of N-methylpyrrolidone were placed in a stirred tank, the reaction temperature was controlled at 65°C, and the reaction time was 3 hours;

[0083] T2: Add 10 g of 1-(2-propenyl)-2-benzimidazolone, maintain the temperature at 65° C. and stir to react for 1 hour, and distill to remove N-methylpyrrolidone to obtain an etching stabilizer.

[0084] The test results of this example are:

[0085] 1. Process stability and formability: Among 100 catheters, the inner cavity position deviation of 99 catheters was within ±0.02mm, and the forming integrity reached more than 98%, proving that the process is stable and the formability is good.

[0086] 2. Relative position stability of the inner lumens of multi-lumen microcatheters: The relative position deviation of the inner lumens of 50 catheters is within 0.01 mm, which proves that this process can still maintain the relative position stability of the inner lumens after multiple coating and sintering.

[0087] 3. Production efficiency test: The production efficiency of this process is 2.5 times that of the traditional extrusion method, and the downtime is reduced by 60%. Within the same production time, the output of this process is significantly increased, and the production process is more stable.

[0088] Example 2

[0089] A preparation process of an etched PTFE multi-lumen microcatheter, the operation steps of which are as follows:

[0090] S1: 75 kg of PTFE dispersion, 0.8 kg of defoamer, 0.8 kg of wetting agent, 0.35 kg of leveling agent, 0.25 kg of thickener and 25 kg of water are prepared to obtain PTFE emulsion 1, and the PTFE emulsion 1 is added to the emulsion tank 1, and the emulsion 1 in the emulsion tank 1 is transported to the emulsion mold 1 through the automatic control system of the emulsion tank 1, and the emulsion monitor is used to control so that the emulsion 1 in the mold 1 is always maintained at a set height;

[0091] S2: 50 kg of PTFE dispersion, 0.35 kg of defoamer, 0.35 kg of wetting agent, 0.8 kg of leveling agent and 45 kg of water are prepared to obtain PTFE emulsion 2, and the PTFE emulsion 2 is added to the emulsion tank 2, and the emulsion 2 in the emulsion tank 2 is transported to the emulsion mold 2 through the automatic control system of the emulsion tank 2, and the emulsion monitor is used to control so that the emulsion 2 in the mold 2 is always maintained at a set height;

[0092] S3: Select silver-plated copper wires of appropriate specifications, unwind the silver-plated copper wires of various specifications through the unwinding system, and position the silver-plated copper wires of different specifications upward through the guide positioning block. The silver-plated copper wires of various specifications passing through the guide positioning block are arranged in accordance with the spacing requirements and in a directional manner to form an orderly moving silver-plated copper wire combination, and the silver-plated copper wire combination passes through a mold containing PTFE emulsion;

[0093] S4: The silver-plated copper wire combination passing through the silicone pad is coated with the emulsion in the mold 1, and a PTFE emulsion layer is formed on the surface of the silver-plated copper wire and between the silver-plated copper wires. The silver-plated copper wire combination coated with the PTFE emulsion enters the drying-pre-sintering furnace upward for drying and pre-sintering;

[0094] S5: After drying and pre-sintering, a PTFE coating is formed on the surface of the silver-plated copper wire and between the wires. The silver-plated copper wire assembly with the PTFE coating continues to move upward into the emulsion mold 2. The lower end of the emulsion mold 2 is matched with a heating tool, so that the silver-plated copper wire assembly with the PTFE coating is coated with the emulsion 2 when passing through the lower end of the mold to obtain a PTFE multi-lumen microcatheter with optimized roundness;

[0095] S6: The PTFE multi-lumen microcatheter after roundness optimization continues to move upward through emulsion 2, and then through mold 3, the roundness of the PTFE multi-lumen microcatheter is further optimized, and then after high-temperature sintering, the sintered PTFE multi-lumen microcatheter continues to move upward, and when the PTFE multi-lumen microcatheter is close to the guide positioning block at the upper end, the guide positioning block fixed at the upper end is removed, and the subsequent upper end positioning is performed by the formed PTFE multi-lumen microcatheter itself, and then the PTFE multi-lumen microcatheter passes through a pulley with a smaller angle change and enters the automatic etching system for etching. The etched PTFE multi-lumen microcatheter moves upward and enters the automatic cleaning system and the drying system in turn for cleaning and drying. The etched PTFE multi-lumen microcatheter after drying passes through the tension control system and enters the traction cutting machine for fixed-length cutting or the winding machine for winding. The etched PTFE multi-lumen microcatheter after cutting can be obtained by extracting the core shaft to obtain a PTFE multi-lumen microcatheter with a small size and meeting the functional requirements.

[0096] The solid content of the PTFE dispersion is 60 wt %.

[0097] The defoamer is an organosilicon defoamer selected from BYK-094.

[0098] The wetting agent is a nonionic surfactant selected from Synperonic OP-10.

[0099] The leveling agent is a fluorocarbon leveling agent selected from Capstone FS-3000.

[0100] The thickener is a water-soluble thickener selected from CMC.

[0101] The temperature control range of the emulsion 1 and the emulsion 2 is 20°C.

[0102] The core wire is selected from aluminum wire, and the coating thickness of the coated core wire is not less than 2 μm.

[0103] The drying-pre-sintering furnace consists of three sections, and the temperature rises in steps. The temperature of the first section is set to 120°C, the temperature of the second section is set to 180°C, and the temperature of the third section is set to 230°C, wherein an exhaust system is installed on the top of the sintering furnace to control the outlet temperature; the sintering furnace consists of three sections, and the temperature rises in steps. The temperature of the first section is set to 180°C, the temperature of the second section is set to 320°C, and the temperature of the third section is set to 400°C, wherein an exhaust system is installed on the top of the sintering furnace to control the outlet temperature; the drying furnace consists of two sections, and the temperature rises in steps. The temperature of the first section is set to 120°C, and the temperature of the second section is set to 180°C, wherein an exhaust system is installed on the top of the drying furnace to control the outlet temperature.

[0104] The etching liquid in the automatic etching system is a sodium naphthalene etching liquid, and an etching stabilizer is added to the etching liquid in an amount of 0.4wt% of the total amount of the etching liquid. The preparation method of the etching stabilizer is as follows:

[0105] T1: 24 g of 2,7-naphthyldithiol, 12 g of allyl-1,1,2,2-tetrafluoroethyl ether, 3 g of triethylamine, and 225 g of N-methylpyrrolidone were placed in a stirred tank, the reaction temperature was controlled at 70°C, and the reaction time was 6 hours;

[0106] T2: Add 15 g of 1-(2-propenyl)-2-benzimidazolone, maintain the temperature at 70° C. and stir the reaction for 2 hours, and distill to remove N-methylpyrrolidone to obtain an etching stabilizer.

[0107] The test results of this example are:

[0108] 1. Process stability and formability: Among 100 catheters, the inner cavity position deviation of 98 catheters was within ±0.02mm, and the forming integrity reached more than 97%, proving that the process is stable and the formability is good.

[0109] 2. Relative position stability of the inner lumens of multi-lumen microcatheters: The relative position deviation of the inner lumens of 49 catheters was within 0.01 mm, proving that this process can still maintain the relative position stability of the inner lumens after multiple coatings and sintering.

[0110] 3. Production efficiency test: The production efficiency of this process is 2.5 times that of the traditional extrusion method, and the downtime is reduced by 60%. Within the same production time, the output of this process is significantly increased, and the production process is more stable.

[0111] Example 3

[0112] A preparation process of an etched PTFE multi-lumen microcatheter, the operation steps of which are as follows:

[0113] S1: 75 kg of PTFE dispersion, 1.4 kg of defoamer, 1.4 kg of wetting agent, 0.85 kg of leveling agent, 0.4 kg of thickener and 25 kg of water are prepared to obtain PTFE emulsion 1, and the PTFE emulsion 1 is added to the emulsion tank 1, and the emulsion 1 in the emulsion tank 1 is transported to the emulsion mold 1 through the automatic control system of the emulsion tank 1, and the emulsion monitor is used to control so that the emulsion 1 in the mold 1 is always maintained at a set height;

[0114] S2: 50 kg of PTFE dispersion, 0.75 kg of defoamer, 0.75 kg of wetting agent, 1.6 kg of leveling agent and 50 kg of water are prepared to obtain PTFE emulsion 2, and the PTFE emulsion 2 is added to the emulsion tank 2, and the emulsion 2 in the emulsion tank 2 is transported to the emulsion mold 2 through the automatic control system of the emulsion tank 2, and the emulsion monitor is used to control so that the emulsion 2 in the mold 2 is always maintained at a set height;

[0115] S3: Select silver-plated copper wires of appropriate specifications, unwind the silver-plated copper wires of various specifications through the unwinding system, and position the silver-plated copper wires of different specifications upward through the guide positioning block. The silver-plated copper wires of various specifications passing through the guide positioning block are arranged in accordance with the spacing requirements and in a directional manner to form an orderly moving silver-plated copper wire combination, and the silver-plated copper wire combination passes through a mold containing PTFE emulsion;

[0116] S4: The silver-plated copper wire combination passing through the silicone pad is coated with the emulsion in the mold 1, and a PTFE emulsion layer is formed on the surface of the silver-plated copper wire and between the silver-plated copper wires. The silver-plated copper wire combination coated with the PTFE emulsion enters the drying-pre-sintering furnace upward for drying and pre-sintering;

[0117] S5: After drying and pre-sintering, a PTFE coating is formed on the surface of the silver-plated copper wire and between the wires. The silver-plated copper wire assembly with the PTFE coating continues to move upward into the emulsion mold 2. The lower end of the emulsion mold 2 is matched with a heating tool, so that the silver-plated copper wire assembly with the PTFE coating is coated with the emulsion 2 when passing through the lower end of the mold to obtain a PTFE multi-lumen microcatheter with optimized roundness;

[0118] S6: The PTFE multi-lumen microcatheter after roundness optimization continues to move upward through emulsion 2, and then through mold 3, the roundness of the PTFE multi-lumen microcatheter is further optimized, and then after high-temperature sintering, the sintered PTFE multi-lumen microcatheter continues to move upward, and when the PTFE multi-lumen microcatheter is close to the guide positioning block at the upper end, the guide positioning block fixed at the upper end is removed, and the subsequent upper end positioning is performed by the formed PTFE multi-lumen microcatheter itself, and then the PTFE multi-lumen microcatheter passes through a pulley with a smaller angle change and enters the automatic etching system for etching. The etched PTFE multi-lumen microcatheter moves upward and enters the automatic cleaning system and the drying system in turn for cleaning and drying. The etched PTFE multi-lumen microcatheter after drying passes through the tension control system and enters the traction cutting machine for fixed-length cutting or the winding machine for winding. The etched PTFE multi-lumen microcatheter after cutting can be obtained by extracting the core shaft to obtain a PTFE multi-lumen microcatheter with a small size and meeting the functional requirements.

[0119] The solid content of the PTFE dispersion is 60 wt %.

[0120] The defoamer is an organosilicon defoamer selected from BYK-024.

[0121] The wetting agent is a nonionic surfactant selected from Tritont X100.

[0122] The leveling agent is a fluorocarbon leveling agent selected from Capstone FS-3100.

[0123] The thickener is a water-soluble thickener selected from CMC.

[0124] The temperature control range of the emulsion 1 and the emulsion 2 is 25°C.

[0125] The core wire is selected from zinc-copper alloy wire, and the coating thickness of the coated core wire is not less than 2 μm.

[0126] The drying-pre-sintering furnace consists of three sections, and the temperature rises in steps. The temperature of the first section is set to 140°C, the temperature of the second section is set to 180°C, and the temperature of the third section is set to 240°C, wherein an exhaust system is installed on the top of the sintering furnace to control the outlet temperature; the sintering furnace consists of three sections, and the temperature rises in steps. The temperature of the first section is set to 210°C, the temperature of the second section is set to 330°C, and the temperature of the third section is set to 420°C, wherein an exhaust system is installed on the top of the sintering furnace to control the outlet temperature; the drying furnace consists of two sections, and the temperature rises in steps. The temperature of the first section is set to 140°C, and the temperature of the second section is set to 190°C, wherein an exhaust system is installed on the top of the drying furnace to control the outlet temperature.

[0127] The etching liquid in the automatic etching system is sodium naphthalene etching liquid, and an etching stabilizer is added to the etching liquid in an amount of 0.8wt% of the total amount of the etching liquid. The preparation method of the etching stabilizer is:

[0128] T1: 32 g of 2,7-naphthyldithiol, 14 g of allyl-1,1,2,2-tetrafluoroethyl ether, 4 g of triethylamine, and 280 g of N-methylpyrrolidone were placed in a stirred tank, the reaction temperature was controlled at 70°C, and the reaction time was 9 hours;

[0129] T2: 18 g of 1-(2-propenyl)-2-benzimidazolone was added, and the reaction was stirred at 70° C. for 3 hours. N-methylpyrrolidone was removed by distillation to obtain an etching stabilizer.

[0130] The test results of this example are:

[0131] 1. Process stability and formability: Among 100 catheters, the inner cavity position deviation of 99 catheters was within ±0.02mm, and the forming integrity reached more than 99%, proving that the process is stable and the formability is good.

[0132] 2. Relative position stability of the inner lumens of multi-lumen microcatheters: The relative position deviation of the inner lumens of 50 catheters is within 0.01 mm, which proves that this process can still maintain the relative position stability of the inner lumens after multiple coating and sintering.

[0133] 3. Production efficiency test: The production efficiency of this process is 2.5 times that of the traditional extrusion method, and the downtime is reduced by 60%. Within the same production time, the output of this process is significantly increased, and the production process is more stable.

[0134] Example 4

[0135] A preparation process of an etched PTFE multi-lumen microcatheter, the operation steps of which are as follows:

[0136] S1: 80 kg of PTFE dispersion, 2 kg of defoamer, 2 kg of wetting agent, 1 kg of leveling agent, 0.5 kg of thickener and 30 kg of water are prepared to obtain PTFE emulsion 1, and the PTFE emulsion 1 is added to an emulsion tank 1, and the emulsion 1 in the emulsion tank 1 is transported to an emulsion mold 1 through an automatic control system of the emulsion tank 1, and the emulsion monitor is used to control so that the emulsion 1 in the mold 1 is always maintained at a set height;

[0137] S2: 55 kg of PTFE dispersion, 1 kg of defoamer, 1 kg of wetting agent, 2 kg of leveling agent and 50 kg of water are prepared to obtain PTFE emulsion 2, and the PTFE emulsion 2 is added to the emulsion tank 2, and the emulsion 2 in the emulsion tank 2 is transported to the emulsion mold 2 through the automatic control system of the emulsion tank 2, and the emulsion monitor is used to control so that the emulsion 2 in the mold 2 is always maintained at a set height;

[0138] S3: Select silver-plated copper wires of appropriate specifications, unwind the silver-plated copper wires of various specifications through the unwinding system, and position the silver-plated copper wires of different specifications upward through the guide positioning block. The silver-plated copper wires of various specifications passing through the guide positioning block are arranged in accordance with the spacing requirements and in a directional manner to form an orderly moving silver-plated copper wire combination, and the silver-plated copper wire combination passes through a mold containing PTFE emulsion;

[0139] S4: The silver-plated copper wire combination passing through the silicone pad is coated with the emulsion in the mold 1, and a PTFE emulsion layer is formed on the surface of the silver-plated copper wire and between the silver-plated copper wires. The silver-plated copper wire combination coated with the PTFE emulsion enters the drying-pre-sintering furnace upward for drying and pre-sintering;

[0140] S5: After drying and pre-sintering, a PTFE coating is formed on the surface of the silver-plated copper wire and between the wires. The silver-plated copper wire assembly with the PTFE coating continues to move upward into the emulsion mold 2. The lower end of the emulsion mold 2 is matched with a heating tool, so that the silver-plated copper wire assembly with the PTFE coating is coated with the emulsion 2 when passing through the lower end of the mold to obtain a PTFE multi-lumen microcatheter with optimized roundness;

[0141] S6: The PTFE multi-lumen microcatheter after roundness optimization continues to move upward through emulsion 2, and then through mold 3, the roundness of the PTFE multi-lumen microcatheter is further optimized, and then after high-temperature sintering, the sintered PTFE multi-lumen microcatheter continues to move upward, and when the PTFE multi-lumen microcatheter is close to the guide positioning block at the upper end, the guide positioning block fixed at the upper end is removed, and the subsequent upper end positioning is performed by the formed PTFE multi-lumen microcatheter itself, and then the PTFE multi-lumen microcatheter passes through a pulley with a smaller angle change and enters the automatic etching system for etching. The etched PTFE multi-lumen microcatheter moves upward and enters the automatic cleaning system and the drying system in turn for cleaning and drying. The etched PTFE multi-lumen microcatheter after drying passes through the tension control system and enters the traction cutting machine for fixed-length cutting or the winding machine for winding. The etched PTFE multi-lumen microcatheter after cutting can be obtained by extracting the core shaft to obtain a PTFE multi-lumen microcatheter with a small size and meeting the functional requirements.

[0142] The solid content of the PTFE dispersion is 70 wt %.

[0143] The defoamer is an organosilicon defoamer selected from BYK-024.

[0144] The wetting agent is a nonionic surfactant selected from Tritont X100.

[0145] The leveling agent is a fluorocarbon leveling agent selected from Capstone FS-3100.

[0146] The thickener is a water-soluble thickener selected from CMC.

[0147] The temperature control range of the emulsion 1 and the emulsion 2 is 30°C.

[0148] The core wire is selected from tin-copper alloy wire, and the coating thickness of the coated core wire is not less than 2 μm.

[0149] The drying-pre-sintering furnace consists of three sections, and the temperature rises in steps. The temperature of the first section is set to 150°C, the temperature of the second section is set to 200°C, and the temperature of the third section is set to 260°C, wherein an exhaust system is installed on the top of the sintering furnace to control the outlet temperature; the sintering furnace consists of three sections, and the temperature rises in steps. The temperature of the first section is set to 250°C, the temperature of the second section is set to 360°C, and the temperature of the third section is set to 450°C, wherein an exhaust system is installed on the top of the sintering furnace to control the outlet temperature; the drying furnace consists of two sections, and the temperature rises in steps. The temperature of the first section is set to 150°C, and the temperature of the second section is set to 200°C, wherein an exhaust system is installed on the top of the drying furnace to control the outlet temperature.

[0150] The etching liquid in the automatic etching system is a sodium naphthalene etching liquid, and an etching stabilizer is added to the etching liquid, and the added amount is 1wt% of the total amount of the etching liquid. The preparation method of the etching stabilizer is:

[0151] T1: 38 g of 2,7-naphthyldithiol, 16 g of allyl-1,1,2,2-tetrafluoroethyl ether, 5 g of triethylamine, and 300 g of N-methylpyrrolidone were placed in a stirring tank, the reaction temperature was controlled at 75°C, and the reaction time was 12 hours;

[0152] T2: Add 20 g of 1-(2-propenyl)-2-benzimidazolone, maintain the temperature at 75° C. and stir the reaction for 4 hours, and distill to remove N-methylpyrrolidone to obtain an etching stabilizer.

[0153] The test results of this example are:

[0154] 1. Process stability and formability: Among 100 catheters, the inner cavity position deviation of all 100 catheters was within ±0.02mm, and the forming integrity reached more than 99%, proving that the process was stable and the formability was good.

[0155] 2. Relative position stability of the inner lumens of multi-lumen microcatheters: The relative position deviation of the inner lumens of 50 catheters is within 0.01 mm, which proves that this process can still maintain the relative position stability of the inner lumens after multiple coating and sintering.

[0156] 3. Production efficiency test: The production efficiency of this process is 2.5 times that of the traditional extrusion method, and the downtime is reduced by 60%. Within the same production time, the output of this process is significantly increased, and the production process is more stable.

[0157] Comparative Example 1

[0158] This example is used as a comparative example of Example 1, except that no etching stabilizer is added to the etching solution of the etching system. The rest is the same as Example 1 and will not be described again here.

[0159] The test results of this example are:

[0160] 1. Process stability and formability: Among the 100 catheters, the inner cavity position deviation of 93 catheters was within ±0.02mm, and the forming integrity reached more than 92%, proving that the process was stable and the formability was good.

[0161] 2. Relative position stability of the inner lumens of multi-lumen microcatheters: The relative position deviation of the inner lumens of 46 catheters is within 0.01 mm, which proves that this process can still maintain the relative position stability of the inner lumens after multiple coating and sintering.

[0162] 3. Production efficiency test: The production efficiency of this process is 2.5 times that of the traditional extrusion method, and the downtime is reduced by 60%. Within the same production time, the output of this process is significantly increased, and the production process is more stable.

[0163] Comparative Example 2

[0164] This example is used as a comparative example of Example 1, except that allyl-1,1,2,2-tetrafluoroethyl ether is not added during the preparation of the etching stabilizer. The rest is the same as Example 1 and will not be repeated here.

[0165] The test results of this example are:

[0166] 1. Process stability and formability: Among 100 catheters, the inner cavity position deviation of 96 catheters was within ±0.02mm, and the forming integrity reached more than 95%, proving that the process is stable and the formability is good.

[0167] 2. Relative position stability of the inner lumens of multi-lumen microcatheters: The relative position deviation of the inner lumens of 48 catheters is within 0.01 mm, which proves that this process can still maintain the relative position stability of the inner lumens after multiple coating and sintering.

[0168] 3. Production efficiency test: The production efficiency of this process is 2.5 times that of the traditional extrusion method, and the downtime is reduced by 60%. Within the same production time, the output of this process is significantly increased, and the production process is more stable.

[0169] Comparative Example 3

[0170] This example is used as a comparative example of Example 1, except that 1-(2-propenyl)-2-benzimidazolone is not added during the preparation of the etching stabilizer. The rest is the same as Example 1 and will not be repeated here.

[0171] The test results of this example are:

[0172] 1. Process stability and formability: Among 100 catheters, the inner cavity position deviation of 95 catheters was within ±0.02mm, and the forming integrity reached more than 94%, proving that the process is stable and the formability is good.

[0173] 2. Relative position stability of the inner lumens of multi-lumen microcatheters: The relative position deviation of the inner lumens of 47 catheters was within 0.01 mm, proving that this process can still maintain the relative position stability of the inner lumens after multiple coatings and sintering.

[0174] 3. Production efficiency test: The production efficiency of this process is 2.5 times that of the traditional extrusion method, and the downtime is reduced by 60%. Within the same production time, the output of this process is significantly increased, and the production process is more stable.

[0175] The above test results confirm that the PTFE multi-lumen microcatheter preparation process of the present invention has the advantages of simple process, convenient operation, good formability, high production efficiency and low safety risk, and can quickly realize mass production and meet the functional requirements of the microcatheter.

[0176] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A preparation process of an etched PTFE multi-lumen microcatheter, the operation steps of which are: S1: According to weight proportions, 70-80 parts of PTFE dispersion, 0.1-2.0 parts of defoamer, 0.1-2.0 parts of wetting agent, 0.1-1.0 parts of leveling agent, 0.1-0.5 parts of thickener and 20-30 parts of water are prepared to obtain PTFE emulsion 1, and the PTFE emulsion 1 is added to an emulsion tank 1, and the emulsion 1 in the emulsion tank 1 is transported to an emulsion mold 1 through an automatic control system of the emulsion tank 1, and the emulsion monitor is used to control the emulsion 1 in the mold 1 so that the emulsion 1 is always kept at a set height; S2: 45-55 parts of PTFE dispersion, 0.1-1.0 parts of defoaming agent, 0.1-1.0 parts of wetting agent, 0.1-2.0 parts of leveling agent and 45-50 parts of water are prepared to obtain PTFE emulsion 2, and the PTFE emulsion 2 is added to the emulsion tank 2, and the emulsion 2 in the emulsion tank 2 is transported to the emulsion mold 2 through the automatic control system of the emulsion tank 2, and the emulsion monitor is used to control so that the emulsion 2 in the mold 2 is always maintained at a set height; S3: Select silver-plated copper wires of appropriate specifications, unwind the silver-plated copper wires of various specifications through the unwinding system, and position the silver-plated copper wires of different specifications upward through the guide positioning block. The silver-plated copper wires of various specifications passing through the guide positioning block are arranged in accordance with the spacing requirements and in a directional manner to form an orderly moving silver-plated copper wire combination, and the silver-plated copper wire combination passes through a mold containing PTFE emulsion; S4: The silver-plated copper wire combination passing through the silicone pad is coated with the emulsion in the mold 1, and a PTFE emulsion layer is formed on the surface of the silver-plated copper wire and between the silver-plated copper wires. The silver-plated copper wire combination coated with the PTFE emulsion enters the drying-pre-sintering furnace upward for drying and pre-sintering; S5: After drying and pre-sintering, a PTFE coating is formed on the surface of the silver-plated copper wire and between the wires. The silver-plated copper wire assembly with the PTFE coating continues to move upward into the emulsion mold 2. The lower end of the emulsion mold 2 is matched with a heating tool, so that the silver-plated copper wire assembly with the PTFE coating is coated with the emulsion 2 when passing through the lower end of the mold to obtain a PTFE multi-lumen microcatheter with optimized roundness; S6: The PTFE multi-lumen microcatheter after roundness optimization continues to move upward through emulsion 2, and then through mold 3, the roundness of the PTFE multi-lumen microcatheter is further optimized, and then after high-temperature sintering, the sintered PTFE multi-lumen microcatheter continues to move upward, and when the PTFE multi-lumen microcatheter is close to the guide positioning block at the upper end, the guide positioning block fixed at the upper end is removed, and the subsequent upper end positioning is performed by the formed PTFE multi-lumen microcatheter itself, and then the PTFE multi-lumen microcatheter passes through a pulley with a smaller angle change and enters the automatic etching system for etching. The etched PTFE multi-lumen microcatheter moves upward and enters the automatic cleaning system and the drying system in turn for cleaning and drying. The etched PTFE multi-lumen microcatheter after drying passes through the tension control system and enters the traction cutting machine for fixed-length cutting or the winding machine for winding. The etched PTFE multi-lumen microcatheter after cutting can be obtained by extracting the core shaft to obtain a PTFE multi-lumen microcatheter with a small size and meeting the functional requirements.

2. A process for preparing an etched PTFE multi-lumen microcatheter according to claim 1, Features: The solid content of the PTFE dispersion is 50-70wt%.

3. A process for preparing an etched PTFE multi-lumen microcatheter according to claim 1, Features: The defoamer is an organosilicon defoamer, and is selected from at least one of BYK-094 and BYK-024.

4. A process for preparing an etched PTFE multi-lumen microcatheter according to claim 1, Features: The wetting agent is a nonionic surfactant, selected from at least one of Synperonic OP-10 and Tritont X 100.

5. A process for preparing an etched PTFE multi-lumen microcatheter according to claim 1, Features: The leveling agent is a fluorocarbon leveling agent, selected from at least one of Capstone FS-3000 and Capstone FS-3100.

6. A process for preparing an etched PTFE multi-lumen microcatheter according to claim 1, Features: The thickener is a water-soluble thickener selected from CMC.

7. A process for preparing an etched PTFE multi-lumen microcatheter according to claim 1, Features: The temperature control range of the emulsion 1 and the emulsion 2 is 15-30°C.

8. A process for preparing an etched PTFE multi-lumen microcatheter according to claim 1, Features: The core wire is selected from any one of copper wire, aluminum wire, silver wire, zinc-copper alloy wire, tin-copper alloy wire, silver-plated copper wire, and chrome-plated copper wire, and the coating thickness of the coated core wire is not less than 2 μm.

9. The process for preparing an etched PTFE multi-lumen microcatheter according to claim 1, Features: The drying-pre-sintering furnace consists of three sections, and the temperature rises in steps. The temperature of the first section is set at 100-150°C, the temperature of the second section is set at 160-200°C, and the temperature of the third section is set at 210-260°C, wherein an exhaust system is installed on the top of the sintering furnace to control the outlet temperature; the sintering furnace consists of three sections, and the temperature rises in steps. The temperature of the first section is set at 150-250°C, the temperature of the second section is set at 300-360°C, and the temperature of the third section is set at 380-450°C, wherein an exhaust system is installed on the top of the sintering furnace to control the outlet temperature; the drying furnace consists of two sections, and the temperature rises in steps. The temperature of the first section is set at 100-150°C, and the temperature of the second section is set at 160-200°C, wherein an exhaust system is installed on the top of the drying furnace to control the outlet temperature.

10. A process for preparing an etched PTFE multi-lumen microcatheter according to claim 1, Features: The etching liquid in the automatic etching system is a sodium naphthalene etching liquid, and an etching stabilizer is added to the etching liquid in an amount of 0.1-1wt% of the total amount of the etching liquid. The preparation method of the etching stabilizer is: T1: 19-38 parts by weight of 2,7-naphthyldithiol, 8-16 parts of allyl-1,1,2,2-tetrafluoroethyl ether, 2-5 parts of triethylamine, and 200-300 parts of N-methylpyrrolidone are placed in a stirring tank, the reaction temperature is controlled at 65-75°C, and the reaction time is 3-12 hours; T2: Add 10-20 parts of 1-(2-propenyl)-2-benzimidazolone, maintain the temperature at 65-75°C and stir the reaction for 1-4 hours, and distill to remove N-methylpyrrolidone to obtain an etching stabilizer.