Space-limited particle foaming method without weld marks and foaming product

By heating and pressurizing in a confined space, the ratio and temperature of particles and mold cavity are controlled, and the problem of poor bonding between particles is solved, and low-density foamed products without welding traces are realized. It is suitable for a variety of industries. application.

CN118876320APending Publication Date: 2024-11-01GUANGDONG UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410972770.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Traditional particle foaming technology can easily lead to poor bonding between particles during low-density foaming, obvious weld marks, and it is difficult to meet the appearance and quality requirements of high-standard products.

Method used

Using a space-limited particle foaming method without welding marks, the particles are placed into the mold cavity with micropores, heated to a preset temperature, injected foaming agent and pressurized, so that the particles are in the The compressed and welded in the confined space is controlled to control the theoretical foaming volume ratio of the mold cavity volume and heating temperature to ensure the tight welded between the particles.

Benefits of technology

It realizes low-density foamed products without welding traces, with higher welding effect and low density, and is suitable for the production of lightweight and precise foamed products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118876320A_ABST
    Figure CN118876320A_ABST
Patent Text Reader

Abstract

The invention relates to the field of microcellular foaming, in particular to a space-limited particle foaming method without weld marks and a foaming product. A space-limited particle foaming method without weld marks specifically comprises the following steps that S1, foaming particles are placed in a mold cavity with micropores, then the mold cavity is placed in a closed space, the temperature of the closed space is increased to a preset temperature, and heat preservation is conducted; s2, heating the closed space to a foaming temperature, and injecting a foaming agent to enable the pressure in the closed space to reach a first preset pressure; s3, carrying out heat preservation and pressure maintaining on the closed space, releasing the pressure of the closed space to environment pressure, and heating to maintain the internal temperature of the closed space at a foaming temperature; and S4, after pressure relief is completed, heating is stopped, and the foaming particles in the mold cavity are cooled and formed. According to the scheme, the ratio of the theoretical foaming volume of the foaming particles to the volume of the mold cavity and the preset foaming temperature of the particles are regulated and controlled, so that the low-density foaming product without welding traces is prepared.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of microporous foaming, and in particular to a space-limited particle foaming method without welding marks and a foamed product. Background Art

[0002] Foaming technology is a technology that generates bubbles through chemical reactions or physical methods to form a porous structure of the material. It can be used to make various foam materials, such as foam plastics, foam rubber, foam ceramics, etc. Compared with chemical foaming, physical foaming has the advantages of being environmentally friendly, stable product performance, simple operation, no chemical residue, and good recyclability, so it has attracted much attention.

[0003] Physical foaming technology includes intermittent foaming, extrusion foaming, and microporous foaming. The foam prepared by intermittent foaming has a closed-cell structure and uniform pores, but it requires a two-step process to form a three-dimensional shape. It is necessary to first prepare a sheet of the corresponding shape and then microporous foaming. The process is long, the equipment is multi-faceted, and the pore structure is not easily controllable. Extrusion foaming to form a three-dimensional shape also requires a two-step process, first extruding the foamed sheet and then cutting it. It is difficult to achieve different pore structures in different areas. Injection foaming can form a three-dimensional shape in one step, but the pores are uneven, the foaming ratio is low, and the pore structure is not easy to control. Compared with continuous extrusion foaming technology, the particle foaming method shows a higher degree of design freedom, and can produce more precise parts and complex three-dimensional structures; at the same time, microporous foam products have shown their unique application potential in the packaging and transportation industries due to their excellent mechanical properties, impact resistance, low thermal conductivity, light weight and sound insulation.

[0004] However, traditional particle foaming is mostly carried out in autoclaves, which are difficult to form low-density products due to their complex molding equipment and processes. In addition, if low-density products are prepared, the interface between particles is prone to poor bonding, resulting in obvious welding marks or gaps between foamed particles, making it difficult for the appearance and quality of the products to meet high standards. In view of this, the market is in urgent need of a low-density particle foaming technology with good welding to overcome the limitations of traditional particle foaming processes. Summary of the invention

[0005] In view of this, the present invention provides a space-constrained particle foaming method and foamed product without welding marks, which is used to solve the technical problem that the existing foaming technology is prone to poor adhesion between particles during the low-density foaming process, resulting in obvious welding marks on the foamed products.

[0006] A first aspect of the present invention provides a method for foaming particles with limited space without welding marks, comprising the following steps:

[0007] Step S1, placing foamed particles into a mold cavity with micropores, and then placing the mold cavity containing the foamed particles in a closed space, heating the internal temperature of the closed space to a preset temperature in the range of Tm±10°C, and keeping the temperature for 20 to 30 minutes;

[0008] Step S2, heating the internal temperature of the enclosed space to the foaming temperature of the foaming particles, and then injecting a foaming agent into the enclosed space to increase the pressure inside the enclosed space to a first preset pressure;

[0009] Step S3, after the enclosed space is kept warm and pressurized for a first period of time, the pressure inside the enclosed space is released to ambient pressure, and while the pressure is released, the enclosed space is heated to maintain the temperature inside the enclosed space at the foaming temperature of the foaming particles;

[0010] Step S4, when the pressure in the enclosed space is released to the ambient pressure, heating is stopped, and the foamed particles in the mold cavity are cooled and formed;

[0011] In the step S1, Tm is the melting point of the foamed particles at room temperature; and the ratio of the theoretical foaming volume of the foamed particles to the volume of the mold cavity is 140±5 to 190±5%.

[0012] Preferably, the ratio of the theoretical foaming volume of the foamed particles to the volume of the mold cavity is 140±5%.

[0013] Preferably, the particle size of the foamed particles is 1 to 4 mm.

[0014] Preferably, the foamed particles include one or more of general plastics and engineering plastics.

[0015] Preferably, the general plastic includes one or more of polyethylene, polypropylene, polystyrene, and polyvinyl chloride; the engineering plastic includes one or more of polybutylene adipate / terephthalate, polylactic acid, thermoplastic polyurethane elastomer rubber, polyolefin elastomer, thermoplastic polyester elastomer, and nylon elastomer.

[0016] Preferably, in step S1, the foaming particles are poly(butylene adipate) / poly(butylene terephthalate) particles, and the preset temperature is 115±5°C.

[0017] Preferably, the foaming temperature of the general plastic is Tm-30 to Tm+10°C; the foaming temperature of the engineering plastic is Tm-30 to Tm+10°C.

[0018] Preferably, the foaming agent includes one or more of supercritical carbon dioxide and supercritical nitrogen.

[0019] Preferably, in step S2, the foaming agent is supercritical carbon dioxide, and the first preset pressure is 8-18 MPa; in step S3, the first duration of heat preservation and pressure preservation is 60-120 min.

[0020] Preferably, in step S3, the pressure relief rate is 20-50 MPa / s.

[0021] The present invention provides a space-limited particle foaming method without welding marks. In step S1, the internal temperature of the enclosed space is set to the melting point of the foamed particles at room temperature, and a temperature change space of 5°C is provided. At this heating temperature, the surface of the foamed particles can be softened or melted, and the local area is in a bonding state, which can improve the welding ability between the foamed particles, so that the prepared foamed products have a better welding effect. At the same time, the present invention controls the ratio of the theoretical foaming volume of the foamed particles to the volume of the mold cavity, so that the foamed particles are compressed by the space limitation of the mold cavity during the foaming process, so that the foamed particles are squeezed against each other and the welding is tighter, thereby reducing the gap between the foamed particles. The present invention further improves the welding effect of the foamed particles by controlling the internal temperature of the enclosed space and the ratio of the theoretical foaming volume of the foamed particles to the volume of the mold cavity, prepares low-density products without welding marks, and solves the technical problem that the foamed particles are easily poorly bonded to each other when foamed under low-density conditions, resulting in obvious welding marks in the foamed products.

[0022] The present invention provides a space-limited particle foaming method without welding marks, wherein the surface of the foamed particles is softened and melted, and the foamed particles in an expanded state and with melted surfaces are squeezed and welded to each other by using space limitation to prepare foamed products. The foamed products prepared by the present invention have the characteristics of low density and no welding marks, and can be applied to the production of more lightweight and precise foamed products.

[0023] Experimental results show that in step S1 of the present invention, when the internal temperature of the enclosed space is set to 115°C and the ratio of the theoretical foaming volume of the foamed particles to the volume of the mold cavity is 140% to 150%, foamed products with low density and no welding marks can be prepared; and when the ratio of the theoretical foaming volume of the foamed particles to the volume of the mold cavity is 140%, lower density foaming can be achieved without affecting the welding marks of the foamed products. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0025] Figure 1This is an electron microscope image of the interface of the particle foaming sample in Example 1 of the present invention, with a scale of 500 μm;

[0026] Figure 2 This is an electron microscope image of the interface of the particle foaming sample in Example 1 of the present invention, with a scale of 50 μm;

[0027] Figure 3 This is an electron microscope image of the interface of the particle foaming sample in Example 2 of the present invention, with a scale of 500 μm;

[0028] Figure 4 This is an electron microscope image of the interface of the particle foaming sample in Example 2 of the present invention, with a scale of 50 μm;

[0029] Figure 5 This is a sample diagram of particle foaming in Example 3 of the present invention;

[0030] Figure 6 This is a sample diagram of particle foaming in Example 4 of the present invention;

[0031] Figure 7 This is a sample diagram of particle foaming in Comparative Example 1 of the present invention;

[0032] Figure 8 This is a sample diagram of particle foaming in Comparative Example 2 of the present invention;

[0033] Fig. 9 This is a picture of the particle foaming sample in Comparative Example 3 of the present invention. DETAILED DESCRIPTION

[0034] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0035] The sources of all raw materials in the present invention are not particularly limited and can be purchased from the market or prepared according to conventional methods known to those skilled in the art.

[0036] The present invention provides a space-limited particle foaming method without welding marks, and the specific steps are as follows:

[0037] Step S1, placing foamed particles into a mold cavity with micropores, and then placing the mold cavity containing the foamed particles in a closed space, heating the internal temperature of the closed space to a preset temperature in the range of Tm±5°C, and keeping the temperature for 20 to 30 minutes;

[0038] Step S2, heating the internal temperature of the enclosed space to the foaming temperature of the foaming particles, and then injecting a foaming agent into the enclosed space to increase the pressure inside the enclosed space to a first preset pressure;

[0039] Step S3, after the enclosed space is kept warm and pressurized for a first period of time, the pressure inside the enclosed space is released to ambient pressure, and while the pressure is released, the enclosed space is heated to maintain the temperature inside the enclosed space at the foaming temperature of the foaming particles;

[0040] Step S4, when the pressure in the enclosed space is released to the ambient pressure, the heating is stopped, and the foamed particles in the mold cavity are cooled and formed;

[0041] In the step S1, Tm is the melting point of the foamed particles at room temperature; and the ratio of the theoretical foaming volume of the foamed particles to the volume of the mold cavity is 140±5 to 190±5%.

[0042] Specifically, in some embodiments, the particles are heated and insulated in the mold cavity to soften or melt the particle surface, and the local area is in a bonding state. At this time, the particles are in a state where the bonding between weak van der Waals forces turns to a state where the polymer molecular chains cross the boundaries of the particles and are entangled with each other. Then the temperature is adjusted to the foaming temperature and a foaming agent is introduced into the mold cavity to allow the foaming agent to fully infiltrate the particles. When the foaming agent reaches a saturated state in the particles, the particles are foamed by releasing pressure. At the same time, the particles are compressed by the space limitation of the mold cavity during the foaming process, so that the foamed particles are squeezed and welded together until the particles fuse with each other, and finally a well-welded product is obtained.

[0043] In some embodiments, the particle size of the foamed particles is 1 to 4 mm; more preferably, the average particle size of the foamed particles is 2 mm.

[0044] In some embodiments, the foamed particles include one or more of general-purpose plastics and engineering plastics.

[0045] In some embodiments, the general plastic includes one or more of polyethylene, polypropylene, polystyrene, and polyvinyl chloride; the engineering plastic includes one or more of polybutylene adipate / terephthalate, polylactic acid, thermoplastic polyurethane elastomer rubber, polyolefin elastomer, thermoplastic polyester elastomer, and nylon elastomer.

[0046] In some embodiments, the foaming temperature of general plastics is Tm-30 to Tm+10°C; the foaming temperature of the engineering plastics is Tm-30 to Tm+10°C.

[0047] Specifically, in some embodiments, different foaming temperatures are selected according to different foaming materials, which can effectively improve the foaming efficiency of the particles and ensure the stability of the foamed particles during the curing process. In addition, the selection of a specific foaming temperature can effectively reduce the energy consumption required to reach the foaming temperature, thereby reducing production costs.

[0048] In some embodiments, the blowing agent includes one or more of supercritical carbon dioxide and supercritical nitrogen, more preferably supercritical carbon dioxide.

[0049] Specifically, in some embodiments, the foaming process only uses supercritical gas that is non-reactive with raw materials and has no environmental pollution as a foaming agent, and does not involve the use of other inorganic or organic polymer foaming agents. Therefore, the method of the present invention is also environmentally friendly.

[0050] In some embodiments, in step S2, the foaming agent is supercritical carbon dioxide, and the first preset pressure is 8-18 MPa.

[0051] Specifically, in some embodiments, the type of foaming agent can accurately control the preset pressure, which can effectively improve the penetration efficiency of the foaming agent in the particles, so that the foaming agent can quickly reach a saturated state in the particles, thereby reducing the time used for the entire foaming process and achieving energy saving and consumption reduction.

[0052] In some embodiments, in step S3, the first duration of heat preservation and pressure preservation is 60 to 120 minutes.

[0053] In some embodiments, in step S3, the pressure relief rate is 20-50 MPa / s.

[0054] Specifically, in some embodiments, by adjusting the pressure relief rate to control the foaming and expansion speed of the particles, the instability of the particles during foaming can be effectively reduced, so that the particles can be foamed uniformly, thereby ensuring the consistency of the foamed products and improving the welding effect of the foamed products.

[0055] Example 1

[0056] This embodiment provides a space-limited particle foaming method without welding marks, and the specific steps are as follows:

[0057] Step S1, placing 1.43 g of foamed particles into a mold cavity with micropores, and then placing the mold cavity containing the foamed particles in a closed space, heating the closed space to a preset temperature in the range of 115° C., and keeping the temperature for 20 to 30 minutes;

[0058] Step S2, cooling the internal temperature of the enclosed space to the foaming temperature of the foamed particles, 95°C, and then injecting supercritical carbon dioxide into the enclosed space to increase the pressure inside the enclosed space to 18Mpa;

[0059] Step S3, heat and pressure-maintaining the enclosed space at a temperature of 95° C. and an internal pressure of 18 MPa for 90 minutes, and after the heat and pressure-maintaining is completed, the internal pressure of the enclosed space is released to the ambient pressure at a pressure release rate of 20 to 50 MPa / s, and the internal temperature of the enclosed space is maintained at 95° C. by heating at the same time during the pressure release;

[0060] Step S4, when the pressure in the enclosed space is released to the ambient pressure, heating is stopped, and the foamed particles in the mold cavity are cooled and formed;

[0061] In some embodiments, in step S1, Tm is the melting point of the foamed particles at room temperature; and the ratio of the theoretical foaming volume of the foamed particles to the volume of the mold cavity is 140±5%.

[0062] Among them, the particles in this embodiment are polybutylene adipate / terephthalate particles (PBAT) particles with an average particle size of 2 mm. The PBAT particles need to be dried at 90° C. for 4 hours before foaming; the mold cavity is a cylinder with a diameter of 30 mm and a height of 9 mm; the ratio of the theoretical foaming volume of the particles to the volume of the mold cavity is 140%.

[0063] Example 2

[0064] The difference between this embodiment and embodiment 1 is that in step S1, the mass of the foamed particles is 1.54 g, and the ratio of the theoretical foaming volume of the particles to the volume of the mold cavity is 150%.

[0065] Example 3

[0066] The difference between this embodiment and embodiment 1 is that in step S1, the mass of the foamed particles is 1.94 g, the preset temperature is 115° C., and the ratio of the theoretical foaming volume of the particles to the volume of the mold cavity is 190%.

[0067] Example 4

[0068] The difference between this embodiment and embodiment 1 is that in step S1, the mass of the foamed particles is 1.94 g, the preset temperature is 110° C., and the ratio of the theoretical foaming volume of the particles to the volume of the mold cavity is 190%.

[0069] Comparative Example 1

[0070] The difference between this embodiment and embodiment 1 is that in step S1, the mass of the foamed particles is 1.74 g, the preset temperature is 105° C., and the ratio of the theoretical foaming volume of the particles to the volume of the mold cavity is 170%.

[0071] Comparative Example 2

[0072] The difference between this embodiment and embodiment 1 is that in step S1, the mass of the foamed particles is 1.54 g, the preset temperature is 105° C., and the ratio of the theoretical foaming volume of the particles to the volume of the mold cavity is 150%.

[0073] Comparative Example 3

[0074] The difference between this embodiment and embodiment 1 is that in step S1, the mass of the foamed particles is 1.94 g, the preset temperature is 105° C., and the ratio of the theoretical foaming volume of the particles to the volume of the mold cavity is 190%.

[0075] Please refer to Table 1 for the results of the above examples and comparative examples.

[0076] Table 1. Test results of Examples 1 to 4 and Comparative Examples 1 to 3

[0077] Test items Welding effect detection Example 1 No welding marks Example 2 No welding marks Example 3 No welding marks Example 4 No welding marks Comparative Example 1 There are obvious welding marks between particles Comparative Example 2 There are obvious gaps between particles Comparative Example 3 The particles are tightly welded but there are slight welding marks

[0078] Note: The effect descriptions of the embodiments and comparative examples in Table 1 refer to the accompanying drawings.

[0079] According to the test results in this embodiment,

[0080] In Examples 1 to 4, the particle dosage is adjusted to control the ratio of the theoretical foaming volume of the particles to the mold cavity volume. In Examples 1 to 2, the ratio of the theoretical foaming volume of the particles to the mold cavity volume is controlled to 140% and 150%, and the preset temperature is controlled at 115°C. The foamed products prepared under the above conditions of the theoretical foaming volume of the particles to the mold cavity volume ratio have no obvious welding marks, and there are no obvious boundaries between the particles. In Examples 3 to 4, the ratio of the theoretical foaming volume of the particles to the mold cavity volume is controlled to 190%, and the preset temperatures are controlled at 115°C and 105°C, respectively, and the prepared foamed products have no obvious welding marks.

[0081] In Comparative Examples 1 and 2, the particle dosage is adjusted to regulate the ratio of the theoretical foaming volume of the particles to the mold cavity volume. In Comparative Examples 1 and 2, the ratio of the theoretical foaming volume of the particles to the mold cavity volume is controlled to 170% and 150%. In the product prepared in Comparative Example 1, obvious welding marks can be observed; in the product prepared in Comparative Example 2, obvious welding gaps can be observed between the particles. In Comparative Example 3, the ratio of the theoretical foaming volume of the particles to the mold cavity volume is controlled to 190%, and the preset temperature is set to 105°C. The prepared foamed product has slight welding marks.

[0082] Example 2 and Comparative Example 2 adjust the heating temperature of the particles before foaming. The heating temperatures before foaming in Example 2 and Comparative Example 2 are 115°C and 105°C. The particles of the product prepared in Example 2 are tightly welded, with no obvious welding marks. In the product prepared in Comparative Example 2, it can be observed that there are obvious welding gaps between the particles.

[0083] It can be known from the experimental data that the various properties of Examples 1 to 4 in this embodiment are significantly better than those of the comparative example, and Examples 1 to 4 realize the preparation of a space-limited particle foaming method without welding marks. It is explained that the present invention has developed a low-density particle foaming technology without welding marks by regulating the ratio of the theoretical foaming volume of the particles to the mold cavity volume, and the heating temperature of the particles before foaming, and solves the technical problem that the conventional foaming technology has obvious welding marks in the foamed products due to poor bonding between particles during the low-density foaming process. At the same time, Examples 1 to 2 in this embodiment also adopted different ratios of the theoretical foaming volume of the particles to the mold cavity volume, and the prepared foamed products had no obvious welding marks, indicating that Example 1 can also achieve lower density foaming under the condition of no welding marks. Therefore, the foamed products prepared by the method of the present invention have the characteristics of low density and good welding effect, and can be applied to more industrial fields.

[0084] In summary, the solution of the present invention has the following beneficial effects:

[0085] (i) The present invention optimizes the ratio of the theoretical foaming volume of particles to the volume of the mold cavity, as well as the heating temperature before foaming, and utilizes particle foaming expansion and spatial confinement to prepare foamed products without welding marks, and achieves low-density foaming.

[0086] (ii) The present invention optimizes the particle size so that the particles can adapt to the foaming mold cavity, has a higher degree of freedom to control the pore morphology, helps to prepare three-dimensional products with more precise structures, and can be applied to more industrial fields.

[0087] (III) The present invention optimizes the pressure and foaming time of the foaming agent infiltrating the particles, so that the foaming agent can quickly penetrate into the particles, improve the penetration efficiency, shorten the time for the foaming agent to infiltrate the particles, and achieve the effect of energy saving and consumption reduction.

[0088] (iv) The present invention only uses supercritical gas which is non-reactive with raw materials and has no environmental pollution as a foaming agent during the foaming process, and does not involve the use of other inorganic or organic polymer foaming agents. Therefore, the method of the present invention is also environmentally friendly.

[0089] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A space-limited particle foaming method without weld marks, It is characterized in that The following steps are involved: Step S1, placing foamed particles into a mold cavity with micropores, and then placing the mold cavity containing the foamed particles in a closed space, heating the internal temperature of the closed space to a preset temperature in the range of Tm±5°C, and keeping the temperature for 20 to 30 minutes; Step S2, heating the internal temperature of the enclosed space to the foaming temperature of the foaming particles, and then injecting a foaming agent into the enclosed space to increase the pressure inside the enclosed space to a first preset pressure; Step S3, after the enclosed space is kept warm and pressurized for a first period of time, the pressure inside the enclosed space is released to ambient pressure, and while the pressure is released, the enclosed space is heated to maintain the temperature inside the enclosed space at the foaming temperature of the foaming particles; Step S4, when the pressure in the enclosed space is released to the ambient pressure, heating is stopped, and the foamed particles in the mold cavity are cooled and formed; In the step S1, Tm is the melting point of the foamed particles at room temperature; and the ratio of the theoretical foaming volume of the foamed particles to the volume of the mold cavity is 140±5 to 190±5%.

2. The method for foaming particles with limited space without weld marks according to claim 1, Features: The ratio of the theoretical foaming volume of the foamed particles to the volume of the mold cavity is 140±5%.

3. The method for foaming particles with limited space without weld marks according to claim 1, Features: The particle size of the foamed particles is 1 to 4 mm.

4. The method for foaming particles with limited space without weld marks according to claim 1, Features: The foamed particles include one or more of general plastics and engineering plastics.

5. The method for foaming particles with limited space without weld marks according to claim 4, Features: The general plastics include one or more of polyethylene, polypropylene, polystyrene, and polyvinyl chloride; the engineering plastics include one or more of polybutylene adipate / terephthalate, polylactic acid, thermoplastic polyurethane elastomer rubber, polyolefin elastomer, thermoplastic polyester elastomer, and nylon elastomer.

6. The method for foaming particles with limited space without weld marks according to claim 1, Features: The foaming particles are poly(butylene adipate) / terephthalate particles, and the preset temperature is 115±5°C.

7. The method for foaming particles with limited space without weld marks according to claim 5, Features: The foaming temperature of the general plastic is Tm-30 to Tm+10°C; the foaming temperature of the engineering plastic is Tm-30 to Tm+10°C.

8. The method for foaming particles with limited space without weld marks according to claim 1, Features: The foaming agent includes one or more of supercritical carbon dioxide and supercritical nitrogen.

9. The method for foaming particles with limited space without weld marks according to claim 1, Features: In the step S2, the foaming agent is supercritical carbon dioxide, and the first preset pressure is 8-18 MPa; in the step S3, the first duration of heat preservation and pressure preservation is 60-120 minutes.

10. A foamed product, Features: The particle foaming method according to any one of claims 1 to 9 is used for preparation.