Anti-drag capsule material as well as preparation method and application thereof

By using the combination of glue-cured plain wet fabric and weather-resistant layer in the floating capsule material, a continuous concave and convex structure is formed, which solves the shortcomings of the drag reduction technology of flexible moving objects and achieves high-performance drag reduction and mechanical strength. Suitable for aerobatics and underwater oil storage capsules.

CN118876532AActive Publication Date: 2024-11-01CHANGCHUN INSTITUTE OF APPLIED CHEMISTRY CHINESE ACADEMY OF SCIENCES
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411242485.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-11-01
Estimated Expiration
2044-09-05

AI Technical Summary

Technical Problem

The prior art mainly focuses on the application of drag reduction of rigid substrates. There are few drag reduction technologies for flexible moving objects, especially in the field of floating capsule materials, which are difficult to meet high performance requirements.

Method used

The capsule material of the weather-resistant layer, the drag-reducing bearing layer and the barrier layer that contacts sequentially. The drag-reducing bearing layer is a plain weave fabric after being cured by glue. It forms a continuous concave-convex structure through the cross-circulation of the weft yarn and warp yarn, and combines with polyurethane resin. , nanotitanium dioxide, light stabilizer and mica sheet weather-resistant layer to achieve drag reduction effect.

Benefits of technology

It achieves excellent drag reduction performance, mechanical strength and weather resistance of the capsule material. It is suitable for aerospace devices and underwater flexible oil storage capsules, and has good application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118876532A_ABST
    Figure CN118876532A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of capsule materials, and particularly relates to a resistance-reducing capsule material as well as a preparation method and application thereof. The resistance-reducing capsule material provided by the invention comprises a weather-proof layer, a resistance-reducing force-bearing layer and a barrier layer which are in contact in sequence, wherein the resistance-reducing force-bearing layer is a plain weave fabric subjected to gum dipping and curing; the number of strands of weft yarns of the plain weave fabric is 1, and the fineness of the weft yarns is 200-300 dtex; warp yarns of the plain weave fabric comprise first warp yarns and second warp yarns, and the first warp yarns and the second warp yarns are sequentially and circularly arranged in a crossed mode. The number of strands of the first warp yarns is 1, and the fineness of the first warp yarns is 200-500 dtex; the number of strands of the second warp yarns is 1, and the fineness of the second warp yarns is 500-1000 dtex; or the number of strands of the second warp yarns is 2-4, and the fineness of the second warp yarns is 200-300 dtex. The capsule material provided by the invention utilizes the natural texture of the fiber fabric to construct the drag reduction microstructure, has a good drag reduction effect, and does not need to add or attach a drag reduction layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of bladder materials, and in particular relates to a drag-reducing bladder material and a preparation method and application thereof. Background Art

[0002] As a kind of flying machine, aerostat has been manufactured and used by human beings for hundreds of years. It uses helium, which has a lower density than air, to provide assistance to the aircraft, so that the aircraft can take off by static lift and fly for a long time. Relying on new capsule materials and advanced control systems and power systems, aerostats have truly entered the practical fields of civil and military use. As the largest and most important part of the aerostat, the capsule material of the aerostat must meet the requirements of high performance. Its quality directly determines the vitality of the airship, and its preparation technology is one of the key technologies restricting the development of airships.

[0003] At present, the research on material surface drag reduction technology at home and abroad is mainly focused on aircraft fuselage surface drag reduction, natural gas transportation drag reduction, long-distance transportation of liquids (water, oil), and drag reduction of underwater weapons and equipment (submarines, torpedoes, etc.). Although the existing surface drag reduction technology has been successfully applied to aircraft and other aircraft structures, they are all based on rigid matrix drag reduction applications, and there are few drag reduction applications for flexible moving objects. Summary of the invention

[0004] In view of this, the object of the present invention is to provide a drag reducing bladder material and a preparation method and application thereof. The bladder material provided by the present invention utilizes the natural texture of the fiber fabric to construct a drag reducing microstructure, has a good drag reducing effect, and does not require the addition or attachment of a drag reducing layer.

[0005] The present invention provides a drag reduction capsule material, comprising a weather-resistant layer, a drag reduction bearing layer and a barrier layer which are in contact with each other in sequence, wherein the drag reduction bearing layer is a plain woven fabric which has been impregnated and cured; The number of weft yarns of the plain fabric is 1, and the fineness of the weft yarns is 200-300 dtex; the warp yarns of the plain fabric include a first warp yarn and a second warp yarn, and the first warp yarn and the second warp yarn are arranged in a cross-circular manner; the number of plies of the first warp yarn is 1, and the fineness is 200-500 dtex; the number of plies of the second warp yarn is 1, and the fineness is 500-1000 dtex; or, the number of plies of the second warp yarn is 2-4, and the fineness is 200-300 dtex; The plain weave fabric makes the surface of the drag reduction bladder material present a fabric texture with a continuous concave-convex structure by interweaving warp yarns and weft yarns.

[0006] Preferably, the surface density of the plain fabric is 100-150 g / m 2 .

[0007] Preferably, the material of the plain fabric is one or more of nylon fiber, aramid fiber and polyarylate fiber.

[0008] Preferably, in terms of mass percentage, the ingredients of the weather-resistant layer include: 90-94% polyurethane resin, 3-5% nano titanium dioxide, 1-2% light stabilizer, 0.5-2% carbon black, and 1-3% mica flakes.

[0009] Preferably, the surface density of the weather-resistant layer is 70-100 g / m 2 .

[0010] Preferably, the material of the barrier layer is polyester; the surface density of the barrier layer is 10-20 g / m 2 .

[0011] The present invention provides a method for preparing the drag reduction bladder material described in the above technical solution, comprising the following steps: a) applying adhesive to one side of the drag-reducing bearing layer, and then pressing and drying the side coated with adhesive with the barrier layer to obtain a double-layer composite layer; b) hot-pressing the weather-resistant layer and the drag-reducing bearing layer of the double-layer composite layer to obtain a drag-reducing bladder material.

[0012] Preferably, the drag reduction bearing layer is prepared according to the following steps: The plain fabric is subjected to a rubber dipping treatment, dried, and heat-fixed to obtain a rubber-dipping fabric; The dipped fabric is dipped again, dried, and thermally recovered to obtain a drag-reducing load-bearing layer.

[0013] Preferably, before the adhesive is applied to the drag-reducing bearing layer, the surface of the layer pre-coated with the adhesive is first subjected to plasma treatment.

[0014] The present invention provides a capsule, wherein the material of the capsule comprises the drag-reducing capsule material described in the above technical solution or the drag-reducing capsule material prepared by the preparation method described in the above technical solution.

[0015] Compared with the prior art, the present invention provides a drag-reducing capsule material and its preparation method and application. The drag-reducing capsule material provided by the present invention comprises a weather-resistant layer, a drag-reducing bearing layer and a barrier layer in contact with each other in sequence, wherein the drag-reducing bearing layer is a plain fabric after dipping and curing; the number of weft yarns of the plain fabric is 1, and the fineness of the weft yarns is 200-300 dtex; the warp yarns of the plain fabric include a first warp yarn and a second warp yarn, and the first warp yarn and the second warp yarn are arranged in a cross-circular manner in sequence; the number of strands of the first warp yarn is 1, and the fineness is 200-500 dtex; the number of strands of the second warp yarn is 1, and the fineness is 500-1000 dtex; or, the number of strands of the second warp yarn is 2-4, and the fineness is 200-300 dtex; the plain fabric presents a fabric texture with a continuous concave-convex structure on the surface of the drag-reducing capsule material through interlaced warp yarns and weft yarns. The present invention uses a cured fabric as the bearing layer of the bladder material, and optimizes the weaving method and warp and weft yarn specifications of the fabric to form a continuous ridge structure of specific specifications on the fabric surface, and the texture of these continuous ridge structures can still be presented on the surface of the bladder material, thereby giving the bladder material drag reduction performance. The bladder material provided by the present invention has excellent drag reduction performance, mechanical strength and weather-resistant barrier performance, and has good application prospects in the field of bladder materials for aerostat bladders and underwater flexible oil storage bladders. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.

[0017] Figure 1 It is a schematic diagram of a weft section of a fabric provided by an embodiment of the present invention. DETAILED DESCRIPTION

[0018] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0019] The invention provides a drag-reducing capsule material, comprising a weather-resistant layer, a drag-reducing bearing layer and a barrier layer which are contacted in sequence.

[0020] In the capsule material provided by the present invention, the components of the weather-resistant layer include: polyurethane resin, nano titanium dioxide, light stabilizer, carbon black and mica flakes; wherein the number average molecular weight of the polyurethane resin is preferably 50000-150000, more preferably 80000-100000; the particle size of the nano titanium dioxide is preferably 1-50nm, more preferably 20-30nm; the light stabilizer is preferably a hindered amine light stabilizer, more preferably light stabilizer 791; the particle size of the mica flakes is preferably 500-1000 mesh, more preferably 700-800 mesh; the mass content of the polyurethane resin in the weather-resistant layer is preferably 90-94%, specifically It can be 90%, 90.5%, 91%, 91.5%, 92%, 92.5%, 93%, 93.5% or 94%; the mass content of the nano titanium dioxide in the weather-resistant layer is preferably 3-5%, specifically 3%, 3.5%, 4%, 4.5% or 5%; the mass content of the light stabilizer in the weather-resistant layer is preferably 1-2%, specifically 1%, 1.5% or 2%; the mass content of the carbon black in the weather-resistant layer is preferably 0.5-2%, specifically 0.5%, 1%, 1.5% or 2%; the mass content of the mica flakes in the weather-resistant layer is preferably 1-3%, specifically 1%, 1.5%, 2%, 2.5% or 3%.

[0021] In the capsule material provided by the present invention, the surface density of the weather-resistant layer is preferably 70-100 g / m 2 , specifically 70g / m 2 , 72g / m 2 , 75g / m 2 , 77g / m 2 , 80g / m 2 , 85g / m 2 , 88g / m 2 , 90g / m 2 , 92g / m 2 , 95g / m 2 or 100g / m 2 .

[0022] In the bladder material provided by the present invention, the drag reduction bearing layer is a plain woven fabric after dipping and curing; wherein, the number of weft yarns of the plain woven fabric is 1, and the weft yarn fineness is 200~300dtex, more specifically 220dtex; the warp yarns of the plain woven fabric include a first warp yarn and a second warp yarn, and the first warp yarn and the second warp yarn are arranged in a cross-cyclic manner; the number of strands of the first warp yarn is 1, and the fineness is 200~500dtex, more specifically 220dtex or 440dtex; the number of strands of the second warp yarn is 1, and the fineness is 500~1000dtex, more specifically 660dtex or 880dtex; or, the number of strands of the second warp yarn is 2~4, more specifically 2, 3 or 4, and the fineness is 200~300dtex, more specifically 220dtex.

[0023] In the bladder material provided by the present invention, the material of the plain fabric in the drag-reducing load-bearing layer is preferably one or more of nylon fiber, aramid fiber and polyarylate fiber.

[0024] In the bladder material provided by the present invention, the surface density of the plain fabric in the drag reduction bearing layer is preferably 100-150 g / m 2 , specifically 100g / m 2 , 105g / m 2 , 110g / m 2 , 115g / m 2 , 120g / m 2 , 125g / m 2 , 130g / m 2 , 135g / m 2 , 140g / m 2 , 145g / m 2 or 150g / m 2 .

[0025] In the bladder material provided by the present invention, the plain fabric in the drag-reducing bearing layer is subjected to a dipping and curing treatment, and the number of the dipping and curing treatment is preferably 1 to 5 times, and more preferably 2 times. In the specific embodiment provided by the present invention, the glue used in the first dipping and curing treatment is preferably an acrylic glue, and the dipping amount (dry glue amount) is preferably 15 to 20 g / m 2 , specifically 15g / m 2 , 16g / m 2 , 17g / m 2 , 18g / m 2 , 19g / m 2 or 20g / m 2 The glue used in the second dipping and curing treatment is preferably epoxy resin glue, and the dipping amount (dry glue amount) is preferably 10~15g / m 2 , specifically 10g / m2 , 11g / m 2 , 12g / m 2 , 13g / m 2 , 14g / m 2 or 15g / m 2 .

[0026] In the bladder material provided by the present invention, the interwoven warp yarns and weft yarns in the drag-reducing load-bearing layer can make the surface of the bladder material present a fabric texture with a continuous concave-convex structure, thereby giving the bladder material drag-reducing performance.

[0027] In the capsule material provided by the present invention, the material of the barrier layer is preferably polyester.

[0028] In the capsule material provided by the present invention, the surface density of the barrier layer is preferably 10-20 g / m 2 , specifically 10g / m 2 , 11g / m 2 , 12g / m 2 , 13g / m 2 , 14g / m 2 , 15g / m 2 , 16g / m 2 , 17g / m 2 , 18g / m 2 , 19g / m 2 or 20g / m 2 .

[0029] In the capsule material provided by the present invention, the thickness of the barrier layer is 50-100 μm, specifically 50 μm, 55 μm, 60 μm, 65 μm, 70 μm, 75 μm, 80 μm, 85 μm, 90 μm, 95 μm or 100 μm.

[0030] In the bladder material provided by the present invention, the weather-resistant layer and the drag-reducing load-bearing layer are preferably hot-pressed composite, and the drag-reducing load-bearing layer and the barrier layer are preferably glued.

[0031] In the bladder material provided by the present invention, the surface of the drag-reducing bearing layer on the side in contact with the barrier layer is preferably plasma treated.

[0032] In the capsule material provided by the present invention, the overall surface density of the capsule material is preferably 200-250 g / m 2 , specifically 200g / m 2 , 205g / m 2 , 210g / m 2 , 215g / m 2 , 220g / m 2 , 225g / m2 , 230g / m 2 , 235g / m 2 , 240g / m 2 , 245g / m 2 or 250g / m 2 .

[0033] The present invention also provides a method for preparing the drag reduction capsule material described in the above technical solution, comprising the following steps: a) applying adhesive to one side of the drag-reducing bearing layer, and then pressing and drying the side coated with adhesive with the barrier layer to obtain a double-layer composite layer; b) hot-pressing the weather-resistant layer and the drag-reducing bearing layer of the double-layer composite layer to obtain a drag-reducing bladder material.

[0034] In the preparation method provided by the present invention, in step a), the drag reduction bearing layer is preferably prepared according to the following steps: i) the plain fabric is subjected to a dipping treatment, dried, and heat-fixed to obtain a dipping fabric; ii) The dipped fabric is dipped again, dried, and heat-recovered to obtain a drag-reducing load-bearing layer.

[0035] In the above-mentioned steps for preparing the drag-reducing bearing layer provided by the present invention, in step i), the glue solution (also called sizing agent) used in the dipping treatment is preferably an acrylic glue solution; the dipping amount (dry glue amount) of the dipping treatment is preferably 15-20 g / m 2 , specifically 15g / m 2 , 16g / m 2 , 17g / m 2 , 18g / m 2 , 19g / m 2 or 20g / m 2 ; The drying temperature is preferably 100-120°C, specifically 100°C, 105°C, 110°C, 115°C or 120°C; the drying time is preferably 1-3h, specifically 3h, 2.5h, 2h, 1.5h or 1h; the heat fixing temperature is preferably 180-200°C, specifically 180°C, 185°C, 190°C, 195°C or 200°C; the heat fixing tension draw ratio is preferably 95-99%, specifically 95%, 96%, 97%, 98% or 99%; the heat fixing time is preferably 25-50s, specifically 50s, 45s, 38s, 35s or 25s.

[0036] In the above-mentioned steps for preparing the drag-reducing bearing layer provided by the present invention, in step ii), the glue used in the dipping treatment is preferably an epoxy resin glue; the dipping amount (dry glue amount) of the dipping treatment is preferably 10-15 g / m2 , specifically 10g / m 2 , 11g / m 2 , 12g / m 2 , 13g / m 2 , 14g / m 2 or 15g / m 2 ; The drying temperature is preferably 140-160°C, specifically 140°C, 145°C, 150°C, 155°C or 160°C; the drying time is preferably 1-1.5h, specifically 1.5h, 1.2h or 1h; the thermal recovery temperature is preferably 120-130°C, specifically 120°C, 125°C or 130°C; the thermal recovery tension draw ratio is preferably 95-99%, specifically 95%, 96%, 97%, 98% or 99%; the thermal recovery time is preferably 15-40s, specifically 40s, 35s, 30s, 25s or 15s.

[0037] In the above-mentioned drag-reducing bearing layer preparation step provided by the present invention, the plain fabric is dipped in glue to improve the wear resistance, bundling and weaving properties of the fiber, while enhancing the adhesion between the fiber and the adhesive and improving the interface bonding ability between the bearing layer fabric and other functional layers.

[0038] In the preparation method provided by the present invention, in step a), before the drag-reducing bearing layer is coated with the adhesive, it is preferred to first subject the surface pre-coated with the adhesive to a plasma treatment. The discharge power of the plasma treatment is preferably 1.2-2.5 kW, specifically 1.2 kW, 1.5 kW, 1.7 kW, 2 kW, 2.3 kW or 2.5 kW; the time of the plasma treatment is preferably 0.1-1 s, specifically 0.1 s, 0.2 s, 0.3 s, 0.4 s, 0.5 s, 0.6 s, 0.7 s, 0.8 s, 0.9 s or 1 s. In the present invention, polar groups can be introduced onto the surface of the fiber fabric through the action of high-energy particles in the plasma, thereby improving the wetting ability of the fiber fabric and improving the interfacial bonding strength for subsequent composite with adhesives or other functional layer fibers.

[0039] In the preparation method provided by the present invention, in step a), the adhesive is preferably a polyurethane adhesive; the coating amount of the adhesive is preferably 5-10 g / m 2 , specifically 5g / m 2 , 6g / m 2 , 7g / m 2 , 8g / m 2 , 9g / m 2 or 10g / m 2 .

[0040] In the preparation method provided by the present invention, in step a), the pressure of the pressing and drying is preferably 0.5-1 MPa, specifically 0.5 MPa, 1 MPa, 1.5 MPa, 2 MPa, 2.5 MPa, 3 MPa, 3.5 MPa, 4 MPa, 4.5 MPa or 5 MPa; the temperature of the pressing and drying is preferably 60-80°C, specifically 60°C, 65°C, 70°C, 75°C or 80°C; the time of the pressing and drying is preferably 2-5 h, specifically 2 h, 2.5 h, 3 h, 3.5 h, 4 h, 4.5 h or 5 h.

[0041] In the preparation method provided by the present invention, in step b), the temperature of the hot pressing compound is preferably 120-160°C, specifically 120°C, 125°C, 130°C, 135°C, 140°C, 145°C, 150°C, 155°C or 160°C; the pressure of the hot pressing compound is preferably 0.5-1.5 MPa, specifically 0.5 MPa, 0.6 MPa, 0.7 MPa, 0.8 MPa, 0.9 MPa, 1 MPa, 1.1 MPa, 1.2 MPa, 1.3 MPa, 1.4 MPa or 1.5 MPa; the time of the hot pressing compound is preferably 2-4 s, specifically 2 s, 2.5 s, 3 s, 3.5 s or 4 s.

[0042] The present invention also provides a capsule, wherein the material of the capsule includes the drag-reducing capsule material described in the above technical solution or the drag-reducing capsule material prepared by the preparation method described in the above technical solution.

[0043] In the capsule provided by the present invention, the barrier layer of the drag-reducing capsule material is the inner layer, and the weather-resistant layer is the outer layer.

[0044] The technical solution provided by the present invention uses a cured fabric as the bearing layer of the bladder material, and optimizes the weaving method and warp and weft yarn specifications of the fabric to form a continuous ridge structure of specific specifications on the fabric surface, and the texture of these continuous ridge structures can still be presented on the surface of the bladder material, thereby giving the bladder material drag reduction performance. The bladder material provided by the present invention has excellent drag reduction performance, mechanical strength and weather-resistant barrier performance, and has good application prospects in the field of bladder materials for aerostat bladders and underwater flexible oil storage bladders.

[0045] For the purpose of greater clarity, the invention is described in detail through the following examples.

[0046] Example 1 Screening of weather-resistant layer ingredients: The polyurethane resin, nano titanium dioxide, light stabilizer, carbon black and mica flakes were added into an internal mixer according to the ratio in Table 1. The internal mixing temperature was 130°C, the internal mixing time was 8 minutes, and the rotor speed was 100 rpm. The obtained internally mixed polyurethane material was cut into pieces while hot, and then subjected to a hot pressing molding process at a hot pressing temperature of 120°C and a pressure of 1.2 MPa to obtain a polyurethane film weather-resistant layer. The surface density of the weather-resistant layer was 70-100 g / m 2 .

[0047] Table 1 Composition formula of weather-resistant layer (unit: mass parts)

[0048] The weather-resistant layer material of the above formula was tested for solar reflectivity and transmittance to evaluate the weather-resistant effect of the material, and its gas permeability was tested at the same time. The results are shown in Table 2: Table 2 Performance comparison of weather-resistant layers with different components

[0049] According to the test on the performance of the weather-resistant layer material, Formula 2 with excellent comprehensive performance is selected as the weather-resistant layer material for subsequent embodiments.

[0050] Example 2 The specific process of preparing drag reduction capsule materials of different specifications is as follows: (1) Prepare fabrics of different specifications: The fabrics used in this embodiment are all plain weave fabrics woven from polyarylate fibers, with a surface density of 110-125 g / m 2 ; The weft cross-sectional structure of plain weave fabric is as follows Figure 1 As shown, Figure 1 In the fabric, the x-axis direction is the weft direction, with continuous weft fibers; the y-axis direction is the warp direction, with the elliptical cross section being the warp fibers; there is no continuous fiber in the z-axis direction, that is, the fabric only has the height in the warp and weft directions. Figure 1 As shown in Figure 2, by adjusting the number and arrangement of warp fibers, different specifications of "ridge" structures can be constructed on the fabric surface, where h + is the highest height of the fabric, i.e. the height of the furrow; s + is the distance between the two highest heights, that is, the spacing of the ridges; d is the width of the ridges.

[0051] In this embodiment, the weft yarn fineness of fabrics of different specifications is consistent, which is 220 dtex, and the number of strands is 1; the number of strands and arrangement of the warp yarns of the fabric, as well as the ridge sizes of fabrics of different specifications are detailed in Table 3: Table 3 Information table of fabrics of different specifications

[0052] (2) Preparation of drag-reducing bearing layer: The fabric materials of different specifications are subjected to the first dipping treatment, and then subjected to the first drying and heat fixing to obtain a one-bath dipping fabric; wherein the sizing agent used in the first dipping treatment is acrylic ester glue, and the dipping amount (dry) is 15g / m 2 The first drying temperature is 110℃, the time is 2h, the heat fixation temperature is 195℃, the tension drawing rate is 98%, and the time is 35s; The first bath dipped fabric is dipped for the second time, and then dried and heat-recovered to obtain the drag-reducing bearing layer material. The sizing agent used in the second dip treatment is epoxy resin glue, and the dip amount (dry) is 10g / m 2 The second drying temperature is 150℃, the time is 1.2h, the thermal recovery temperature is 120℃, the tension drawing rate is 98%, and the time is 25s.

[0053] (3) Composite of drag-reducing bearing layer and barrier layer: One side of the drag-reducing bearing layer material prepared in the above step was treated with plasma, with a plasma discharge power of 2.0 kW and a time of 0.5 s; the plasma-treated surface layer was facing upwards, and 7 g / m2 of polyurethane adhesive was applied. 2 , and then apply the barrier layer material (polyester film, thickness 75μm, surface density 15g / m 2 ), applying a pressure of 1.0 MPa, and drying in a blast oven at 80°C for 4 hours to obtain a double-layer composite structure of a drag-reducing bearing layer and a barrier layer.

[0054] (4) Composite of drag-reducing bearing layer and weather-resistant layer: The weather-resistant layer material of Formulation 2 of Example 1 and the drag-reducing bearing layer of the above-mentioned double-layer composite structure were hot-pressed and composited using a laminating and composite device. The hot-pressing temperature was 150° C., the hot-pressing pressure was 1.2 MPa, and the hot-pressing time was 3.5 s to obtain a drag-reducing bladder material.

[0055] The drag reduction rate, surface density, tensile strength, interlayer peel strength and gas permeability of the drag reduction bladder materials made of fabrics of different specifications were tested; the test description of the drag reduction rate is as follows: The drag reduction performance of the material is tested in a small DC wind tunnel; the length of the wind tunnel is 4m and the diameter is 0.8m; the wind speed is continuously adjustable in the range of 0~30.0m / s; the test resistance balance has a range of 300N and a load resolution of 0.1; the drag reduction rate is calculated by comparing it with the wind resistance value of the smooth polyurethane capsule material; the drag reduction rate is equal to the wind resistance shear force of the smooth TPU material minus the wind resistance shear force of the embodiment material multiplied by 100% of the wind resistance shear force of the smooth TPU material; if the result is a negative value, it indicates that the material has a drag-increasing effect; if the result is 1, it indicates that the material neither increases nor reduces drag; if the result is greater than 1, it indicates that the material has a drag-reducing effect.

[0056] The test results are shown in Table 4: Table 4 Performance test results of drag reduction bladder materials of different specifications

[0057] It can be seen from Table 4 that the microstructure "ridge" height is 30-90 μm, the interval is 70-155 μm, the width is 20-73 μm, and the capsule material has a drag reduction rate of 1.3-6.2%. The surface density of the capsule material prepared in this embodiment is 200-250 g / m 2 , tensile strength is 834~946N / cm, interlayer peel strength is 3.2~5.4kN / m; gas permeability is 1.29~1.67L / m 2 ·24h.

[0058] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A drag reduction capsule material, characterized in that: It comprises a weather-resistant layer, a drag-reducing bearing layer and a barrier layer which are in contact with each other in sequence, wherein the drag-reducing bearing layer is a plain woven fabric which has been impregnated and cured; The number of weft yarns of the plain fabric is 1, and the fineness of the weft yarns is 200-300 dtex; the warp yarns of the plain fabric include a first warp yarn and a second warp yarn, and the first warp yarn and the second warp yarn are arranged in a cross-circular manner; the number of plies of the first warp yarn is 1, and the fineness is 200-500 dtex; the number of plies of the second warp yarn is 1, and the fineness is 500-1000 dtex; or, the number of plies of the second warp yarn is 2-4, and the fineness is 200-300 dtex; The plain weave fabric makes the surface of the drag reduction bladder material present a fabric texture with a continuous concave-convex structure by interweaving warp yarns and weft yarns.

2. The drag reduction bladder material according to claim 1, characterized in that: The surface density of the plain fabric is 100-150 g / m 2 .

3. The drag reduction bladder material according to claim 1, characterized in that: The material of the plain fabric is one or more of nylon fiber, aramid fiber and polyarylate fiber.

4. The drag reduction bladder material according to claim 1, characterized in that: Calculated by mass percentage, the components of the weather-resistant layer include: 90-94% polyurethane resin, 3-5% nano titanium dioxide, 1-2% light stabilizer, 0.5-2% carbon black, and 1-3% mica flakes.

5. The drag reduction bladder material according to claim 1, characterized in that: The surface density of the weather-resistant layer is 70-100 g / m 2 .

6. The drag reduction bladder material according to claim 1, characterized in that: The material of the barrier layer is polyester; the surface density of the barrier layer is 10-20 g / m 2 .

7. A method for preparing the drag reduction capsule material according to any one of claims 1 to 6, characterized in that: The following steps are involved: a) applying adhesive to one side of the drag-reducing bearing layer, and then pressing and drying the side coated with adhesive with the barrier layer to obtain a double-layer composite layer; b) hot-pressing the weather-resistant layer and the drag-reducing bearing layer of the double-layer composite layer to obtain a drag-reducing bladder material.

8. The preparation method according to claim 7, characterized in that: The drag reduction bearing layer is prepared according to the following steps: The plain fabric is subjected to a rubber dipping treatment, dried, and heat-fixed to obtain a rubber-dipping fabric; The dipped fabric is dipped again, dried, and thermally recovered to obtain a drag-reducing load-bearing layer.

9. The preparation method according to claim 7, characterized in that: Before the adhesive is applied to the drag-reducing bearing layer, the surface of the layer pre-applied with the adhesive is firstly subjected to plasma treatment.

10. A capsule, characterized in that: The material of the capsule includes the drag-reducing capsule material described in any one of claims 1 to 6 or the drag-reducing capsule material prepared by the preparation method described in any one of claims 7 to 9.

Citation Information

Patent Citations

  • Poly urethane (PU) or thermal receiver unit (TPU) film with anti-drag micro-groove structure for airship skin

    CN102673772A

  • Envelope material composite layer, preparation method of envelope material composite layer, envelope and aerostat

    CN107651157A

  • Fabric for swimwear and swimwear using same

    CN114729477A

  • Underwater polyurethane oil storage bag body material, preparation method thereof and flexible oil bag

    CN115593066A

  • High-strength wear-resistant nylon fabric and preparation method thereof

    CN116377643A