Low-reflection water vapor barrier film
By layering inorganic and organic materials with different refractive indices, a low-reflectivity water vapor barrier film was constructed, which solved the problems of unsatisfactory water-blocking performance and light pollution in high humidity environments, and achieved efficient water vapor and oxygen blocking and reflectivity reduction.
Patent Information
- Application Number
- CN202410952801.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-01
AI Technical Summary
Existing water-blocking membranes do not perform well in high humidity environments and may cause light pollution problems.
The low-reflectivity water vapor barrier film with a layered structure includes a substrate, a first inorganic barrier layer, a hardened layer, a second inorganic barrier layer, a high-refractive-index organic resin layer, a third inorganic barrier layer, and a low-refractive-index hydrophobic layer. It utilizes a combination of materials with different refractive indices to reduce reflectivity and improve water and oxygen barrier efficiency.
This technology effectively blocks water vapor and oxygen under high humidity conditions while reducing the membrane's reflectivity, avoiding light pollution, and improving the overall performance of the membrane.
Smart Images

Figure CN118876550A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of protective films, and in particular relates to a low-reflection water vapor barrier film. Background Art
[0002] Existing water-blocking films have some shortcomings in their applications. That is, water-blocking films can prevent water penetration to a certain extent, but in certain circumstances, their water-blocking effect may not be very ideal. For example, in a high humidity environment, the water-blocking performance may be challenged. In addition, some water-blocking films may have a high reflectivity, which can easily cause light pollution problems and have adverse effects in application scenarios that require high light transmittance.
[0003] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention and should not be regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art. Summary of the invention
[0004] The object of the present invention is to provide a low-reflection water vapor barrier film, which has a low refractive index and good water barrier performance.
[0005] In order to achieve the above-mentioned object, a specific embodiment of the present invention provides a low-reflection water vapor barrier film, comprising a substrate, a first inorganic barrier layer, a hardening layer, a second inorganic barrier layer, a high-refractive organic resin layer, a third inorganic barrier layer and a low-refractive hydrophobic layer stacked in sequence;
[0006] The raw materials of the first inorganic barrier layer, the second inorganic barrier layer and the third inorganic barrier layer all include at least one of aluminum oxide, silicon oxide, silicon nitride and silicon oxynitride;
[0007] The refractive index of the high-refractive organic resin layer is 1.6-1.7; the refractive index of the low-refractive hydrophobic layer is 1.3-1.4; the refractive index of the first inorganic barrier layer, the second inorganic barrier layer and the third inorganic barrier layer are all 1.40-1.76; the refractive index of the hardened layer is 1.5-1.6.
[0008] In one or more embodiments of the present invention, the low-fold hydrophobic layer comprises the following raw material components by mass: 80-120 parts of hardened resin, 3-5 parts of silica particles, 180-220 parts of organic solvent, less than or equal to 1 part of AF additive and less than or equal to 1 part of silane coupling agent.
[0009] In one or more embodiments of the present invention, the high-refractive organic resin layer includes the following raw material components by mass: 40-60 parts of multifunctional acrylate, 1-3 parts of photoinitiator, 10-20 parts of Al2O3 particles and 60-80 parts of organic solvent.
[0010] In one or more embodiments of the present invention, the hardened layer comprises, by mass, 30 to 50 parts of multifunctional acrylate, 8 to 12 parts of polyethylene glycol resin, 1 to 3 parts of photoinitiator and 40 to 60 parts of organic solvent.
[0011] In one or more embodiments of the present invention, the multifunctional acrylate includes one of trimethylolpropane triacrylate, trimethylolpentane trimethacrylate, dipentaerythritol acrylate, 2-ethylpentaerythritol triacrylate, trimethylolpropane triacrylate, pentaerythritol triacrylate, trimethylolpropane trimethacrylate, pentaerythritol tetraacrylate and dipentaerythritol hexaacrylate; and / or,
[0012] The organic solvent is one or more of butanone, methyl isobutyl ketone, acetone, cyclopentanone, propylene glycol methyl ether, ethyl acetate, butyl acetate, amyl acetate, methanol, methyl isobutyl ketone, ethanol, n-propanol, butanol, ethylene glycol ethyl ether, ethylene glycol butyl ether and diethylene glycol ethyl ether.
[0013] In one or more embodiments of the present invention, the thickness of the low-fold hydrophobic layer is 80-120 nm; and / or,
[0014] The thickness of the high-refractive organic resin layer is 50-150 nm.
[0015] In one or more embodiments of the present invention, the thickness of the hardened layer is 3.5-4.5 μm.
[0016] In one or more embodiments of the present invention, the thickness of the first inorganic barrier layer, the second inorganic barrier layer and the third inorganic barrier layer are all less than or equal to 80 nm.
[0017] In one or more embodiments of the present invention, the thickness of the substrate is 50-100 μm, and the refractive index of the substrate is 1.5-1.6.
[0018] In one or more embodiments of the present invention, the substrate includes a substrate body and a primer layer disposed on the substrate body, the primer layer is bonded to the first inorganic barrier layer, and the substrate body is a PET substrate.
[0019] Compared with the prior art, the low-reflective water vapor barrier film of the present invention plays a role in reducing the reflectivity of the entire film by stacking a multilayer structure with different refractive indices, wherein the first inorganic barrier layer, the second inorganic barrier layer and the third inorganic barrier layer can not only reduce the reflectivity of the entire film, but also improve the water and oxygen barrier rate of the entire film, that is, improve the water vapor barrier rate. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the prior art descriptions are briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0021] Figure 1 Schematic diagram of the structure of a low-reflection water vapor barrier film in one embodiment of the present invention.
[0022] Description of main reference numerals:
[0023] 1. Substrate; 11. Substrate body; 12. Primer layer; 2. First inorganic barrier layer; 3. Hardening layer; 4. Second inorganic barrier layer; 5. High-refractive organic resin layer; 6. Third inorganic barrier layer; 7. Low-refractive hydrophobic layer. DETAILED DESCRIPTION
[0024] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0025] like Figure 1 As shown, a low-reflection water vapor barrier film in an embodiment of the present invention comprises a substrate 1, a first inorganic barrier layer 2, a hardening layer 3, a second inorganic barrier layer 4, a high-refractive organic resin layer 5, a third inorganic barrier layer 6 and a low-refractive hydrophobic layer 7 which are stacked in sequence;
[0026] The raw materials of the first inorganic barrier layer 2, the second inorganic barrier layer 4 and the third inorganic barrier layer 6 all include at least one of aluminum oxide, silicon oxide, silicon nitride and silicon oxynitride;
[0027] The refractive index of the high-refractive organic resin layer 5 is 1.6-1.7; the refractive index of the low-refractive hydrophobic layer 7 is 1.3-1.4; the refractive index of the first inorganic barrier layer 2, the second inorganic barrier layer 4 and the third inorganic barrier layer 6 are all 1.40-1.76; the refractive index of the hardened layer 3 is 1.5-1.6.
[0028] It can be understood that the low-reflection water vapor barrier film of the present invention plays a role in reducing the reflectivity of the entire film by stacking a multilayer structure with different refractive indices, wherein the first inorganic barrier layer 2, the second inorganic barrier layer 4 and the third inorganic barrier layer 6 can not only reduce the reflectivity of the entire film, but also improve the water and oxygen barrier rate of the entire film, that is, improve the water vapor barrier rate. Among them, the hardening layer 3 and the high-refractive organic resin layer 5 can be considered as organic coatings.
[0029] Specifically, the low-fold hydrophobic layer 7 includes the following raw material components by mass: 80-120 parts of hardened resin, 3-5 parts of silica particles, 180-220 parts of organic solvent, less than or equal to 1 part of AF additive and less than or equal to 1 part of silane coupling agent.
[0030] Among them, in order to facilitate subsequent coating and control of film thickness after curing, common organic solvents can be used to mix with the above raw materials, and then the mixed raw materials can be evenly transferred to the surface of the film material by micro-concave coating and the like, followed by oven thermal curing and UV light curing to form a low-refractive hydrophobic layer 7.
[0031] Preferably, the hardening resin can be selected from one or more of Shanghai Lien Chemical Model A-2505LR, Arakawa Chemical Co., Ltd. Model SL045, and Kyoeisha Chemical Model KC-1600.
[0032] Preferably, the AF auxiliary agent may be Shin-Etsu KY-1203. The silane coupling agent may be Shin-Etsu KBM-503.
[0033] Preferably, the average particle size of the silicon dioxide particles may be 40 to 50 nm. The silicon dioxide particles may be Nissan Chemical PGM-AC-4130Y.
[0034] Specifically, the high-refractive organic resin layer 5 includes the following raw material components by weight: 40-60 parts of multifunctional acrylate, 1-3 parts of photoinitiator, 10-20 parts of Al2O3 particles and organic solvent. After the above raw materials are evenly mixed, the mixed raw materials can be evenly transferred to the surface of the film material by micro-concave coating and the like, and then oven heat curing and UV light curing are performed to form the high-refractive organic resin layer 5.
[0035] Preferably, the photoinitiator may be Efka photoinitiator No. 1173. The Al2O3 particles may be UVH-D-AL-24 produced by Harima Chemicals Co., Ltd.
[0036] Specifically, the hardened layer 3 comprises, by weight, 30 to 50 parts of multifunctional acrylate, 8 to 12 parts of polyethylene glycol resin, 1 to 3 parts of photoinitiator and 40 to 60 parts of organic solvent.
[0037] After the above raw materials are evenly mixed, the mixed raw materials can be evenly transferred to the surface of the film material by micro-concave coating or the like, and then thermally cured in an oven and UV-cured to form a hardened layer 3.
[0038] Preferably, the photoinitiator may be Efka No. 1173 photoinitiator.
[0039] Specifically, the multifunctional acrylate includes one of trimethylolpropane triacrylate, trimethylolpentane trimethacrylate, dipentaerythritol acrylate, 2-ethylpentaerythritol triacrylate, trimethylolpropane triacrylate, pentaerythritol triacrylate, propylene glycol methyl ether, trimethylolpropane trimethacrylate, pentaerythritol tetraacrylate and dipentaerythritol hexaacrylate; and / or,
[0040] The organic solvent is one or more of butanone, methyl isobutyl ketone, acetone, cyclopentanone, propylene glycol methyl ether, ethyl acetate, butyl acetate, amyl acetate, methanol, methyl isobutyl ketone, ethanol, n-propanol, butanol, ethylene glycol ethyl ether, ethylene glycol butyl ether and diethylene glycol ethyl ether.
[0041] Specifically, the thickness of the low-refractive hydrophobic layer 7 is 80-120 nm; the thickness of the high-refractive organic resin layer 5 is 50-150 nm.
[0042] Specifically, the thickness of the hardened layer 3 is 3.5-4.5 μm.
[0043] Specifically, the thickness of the first inorganic barrier layer 2 , the second inorganic barrier layer 4 , and the third inorganic barrier layer 6 are all less than or equal to 80 nm.
[0044] Specifically, the substrate 1 includes a substrate body 11 and a primer layer 12 disposed on the substrate body 11, the primer layer 12 is bonded to the first inorganic barrier layer 2, and the substrate body 11 is a PET substrate; the thickness of the substrate 1 is 50 to 100 μm, and the refractive index of the substrate 1 is 1.5 to 1.6.
[0045] Preferably, the substrate 1 is a PET optical film produced by Toray Industries, Ltd. of Japan, and the PET optical film includes a substrate body 11 and a primer layer 12 .
[0046] The low-reflection water vapor barrier film of the present invention will be described in detail below in conjunction with specific embodiments and comparative examples:
[0047] Example 1
[0048] On a 50μm thick PET optical film produced by Japan's Toray Corporation, SiO2 was evenly plated on the surface of the substrate primer layer through a magnetron sputtering process, a single Si target, a vehicle speed of 2.0m / min, and a power of 4.8kw, to form a first inorganic barrier layer with a thickness of 5nm.
[0049] The hardening layer is composed of 30 parts of multifunctional acrylate trimethylolpropane triacrylate, 8 parts of polyethylene glycol resin, 1 part of Efka No. 1173 photoinitiator, 20 parts of butanone, and 20 parts of propylene glycol methyl ether. The coating is evenly transferred to the surface of the first inorganic barrier layer by micro-concave coating, and then oven thermal curing and UV light curing are performed to form a hardening layer with a thickness of 4μm.
[0050] Through the magnetron sputtering process, single Si target, vehicle speed 2.0m / min, power 4.8kw, SiO2 is evenly plated on the surface of the hardened layer to form a second inorganic barrier layer with a thickness of 5nm.
[0051] After 40 parts of multifunctional acrylate trimethylolpropane triacrylate, 2 parts of Efka No. 1173 photoinitiator, 30 parts of butanone, 30 parts of propylene glycol methyl ether, and 10 parts of Al2O3 particles (Halimah Chemicals Co., Ltd. UVH-D-AL-24) are mixed evenly, the coating is evenly transferred to the surface of the second inorganic barrier layer by micro-concave coating, and then oven thermal curing and UV light curing are performed to form a high-refractive organic resin layer with a thickness of 130nm.
[0052] Through the magnetron sputtering process, single Si target, vehicle speed 2.0m / min, power 4.8kw, SiO2 is evenly plated on the surface of the high-refractive organic resin layer to form a third inorganic barrier layer with a thickness of 5nm.
[0053] After mixing 80 parts of hardening resin (Shanghai Lien Chemical Model A-2505LR), 3 parts of silica particles (Nissan Chemical PGM-AC-4130Y), 180 parts of organic solvent (methyl isobutyl ketone), 1 part of AF additive (Shin-Etsu KY-1203) and 1 part of silane coupling agent (Shin-Etsu KBM-503) evenly, the coating was evenly transferred to the surface of the third inorganic barrier layer by micro-concave coating, and then oven thermal curing and UV light curing were performed to form a low-refractive hydrophobic layer with a thickness of 100 nm. Finally, the low-reflection water vapor barrier film of the present invention was obtained.
[0054] Example 2
[0055] On a 50μm thick PET optical film produced by Japan's Toray Corporation, SiO2 was evenly plated on the surface of the substrate primer layer through a magnetron sputtering process, a single Si target, a vehicle speed of 1.0m / min, and a power of 4.8kw, to form a first inorganic barrier layer with a thickness of 10nm.
[0056] The hardening layer is composed of 50 parts of multifunctional acrylate trimethylolpropane triacrylate, 12 parts of polyethylene glycol resin, 3 parts of Efka No. 1173 photoinitiator, 30 parts of butanone, and 30 parts of propylene glycol methyl ether. The coating is evenly transferred to the surface of the first inorganic barrier layer by micro-concave coating, and then oven thermal curing and UV light curing are performed to form a hardening layer with a thickness of 4μm.
[0057] Through the magnetron sputtering process, single Si target, vehicle speed 1.0m / min, power 4.8kw, SiO2 is evenly plated on the surface of the hardened layer to form a second inorganic barrier layer with a thickness of 10nm.
[0058] 60 parts of multifunctional acrylate trimethylolpropane triacrylate, 3 parts of Efka No. 1173 photoinitiator, 80 parts of organic solvent (butanone and propylene glycol methyl ether), and 20 parts of Al2O3 particles (Halimah Chemicals Co., Ltd. UVH-D-AL-24) are mixed evenly, and the coating is evenly transferred to the surface of the second inorganic barrier layer by micro-concave coating, followed by oven thermal curing and UV light curing to form a high-refractive organic resin layer with a thickness of 130nm.
[0059] Through the magnetron sputtering process, single Si target, vehicle speed 1.0m / min, power 4.8kw, SiO2 is evenly plated on the surface of the high-refractive organic resin layer to form a third inorganic barrier layer with a thickness of 10nm.
[0060] After mixing 120 parts of hardening resin (Shanghai Lien Chemical Model A-2505LR), 5 parts of silica particles (Nissan Chemical PGM-AC-4130Y), 220 parts of organic solvent (methyl isobutyl ketone), 1 part of AF additive (Shin-Etsu KY-1203) and 1 part of silane coupling agent (Shin-Etsu KBM-503) evenly, the coating was evenly transferred to the surface of the third inorganic barrier layer by micro-concave coating, and then oven thermal curing and UV light curing were performed to form a low-reflection hydrophobic layer with a thickness of 100 nm. Finally, the low-reflection water vapor barrier film of the present invention was obtained.
[0061] Example 3
[0062] On a 50μm thick PET optical film produced by Japan's Toray Corporation, SiO2 was evenly plated on the surface of the substrate primer layer through a magnetron sputtering process, a single Si target, a vehicle speed of 1.0m / min, and a power of 9.6kw, to form a first inorganic barrier layer with a thickness of 20nm.
[0063] The hardening layer is composed of 40 parts of multifunctional acrylate trimethylolpropane triacrylate, 10 parts of polyethylene glycol resin, 2 parts of Efka No. 1173 photoinitiator, 25 parts of butanone and 25 parts of propylene glycol methyl ether. The coating is evenly transferred to the surface of the first inorganic barrier layer by micro-concave coating, and then oven thermal curing and UV light curing are performed to form a hardening layer with a thickness of 4μm.
[0064] Through the magnetron sputtering process, single Si target, vehicle speed 1.0m / min, power 9.6kw, SiO2 is evenly plated on the surface of the hardened layer to form a second inorganic barrier layer with a thickness of 20nm.
[0065] 50 parts of multifunctional acrylate trimethylolpropane triacrylate, 2 parts of Efka No. 1173 photoinitiator, 35 parts of butanone, 35 parts of propylene glycol methyl ether, and 15 parts of Al2O3 particles (Halimah Chemicals Co., Ltd. UVH-D-AL-24) were mixed evenly, and the coating was evenly transferred to the surface of the second inorganic barrier layer by micro-concave coating, followed by oven thermal curing and UV light curing to form a high-refractive organic resin layer with a thickness of 130nm.
[0066] Through the magnetron sputtering process, single Si target, vehicle speed 1.0m / min, power 9.6kw, SiO2 is evenly plated on the surface of the high-refractive organic resin layer to form a third inorganic barrier layer with a thickness of 20nm.
[0067] After mixing 100 parts of hardening resin (Shanghai Lien Chemical Model A-2505LR), 4 parts of silica particles (Nissan Chemical PGM-AC-4130Y), 200 parts of organic solvent (methyl isobutyl ketone), 1 part of AF additive (Shin-Etsu KY-1203) and 1 part of silane coupling agent (Shin-Etsu KBM-503) evenly, the coating was evenly transferred to the surface of the third inorganic barrier layer by micro-concave coating, and then oven thermal curing and UV light curing were performed to form a low-reflection hydrophobic layer with a thickness of 100 nm. Finally, the low-reflection water vapor barrier film of the present invention was obtained.
[0068] Example 4
[0069] On a 50μm thick PET optical film produced by Japan's Toray Corporation, SiO2 was evenly plated on the surface of the substrate primer layer through a magnetron sputtering process, a single Si target, a vehicle speed of 1.0m / min, and a power of 19.2kw, forming a first inorganic barrier layer with a thickness of 40nm.
[0070] The hardening layer is composed of 40 parts of multifunctional acrylate trimethylolpropane triacrylate, 10 parts of polyethylene glycol resin, 2 parts of Efka No. 1173 photoinitiator, 25 parts of butanone, and 25 parts of propylene glycol methyl ether. The coating is evenly transferred to the surface of the first inorganic barrier layer by micro-concave coating, and then oven thermal curing and UV light curing are performed to form a hardening layer with a thickness of 4μm.
[0071] Through the magnetron sputtering process, single Si target, vehicle speed 1.0m / min, power 19.2kw, SiO2 is evenly plated on the surface of the hardened layer to form a second inorganic barrier layer with a thickness of 40nm.
[0072] 50 parts of multifunctional acrylate trimethylolpropane triacrylate, 2 parts of Efka No. 1173 photoinitiator, 35 parts of butanone, 35 parts of propylene glycol methyl ether, and 15 parts of Al2O3 particles (Halimah Chemicals Co., Ltd. UVH-D-AL-24) are mixed evenly, and the coating is evenly transferred to the surface of the second inorganic barrier layer by micro-concave coating, followed by oven thermal curing and UV light curing to form a high-refractive organic resin layer with a thickness of 130nm.
[0073] Through the magnetron sputtering process, single Si target, vehicle speed 1.0m / min, power 19.2kw, SiO2 is evenly plated on the surface of the high-refractive organic resin layer to form a third inorganic barrier layer with a thickness of 40nm.
[0074] After mixing 100 parts of hardening resin (Shanghai Lien Chemical Model A-2505LR), 4 parts of silica particles (Nissan Chemical PGM-AC-4130Y), 200 parts of organic solvent (methyl isobutyl ketone), 1 part of AF additive (Shin-Etsu KY-1203) and 1 part of silane coupling agent (Shin-Etsu KBM-503) evenly, the coating was evenly transferred to the surface of the third inorganic barrier layer by micro-concave coating, and then oven thermal curing and UV light curing were performed to form a low-reflection hydrophobic layer with a thickness of 100 nm. Finally, the low-reflection water vapor barrier film of the present invention was obtained.
[0075] Example 5
[0076] On a 50μm thick PET optical film produced by Japan's Toray Corporation, SiO2 was evenly plated on the surface of the substrate primer layer through magnetron sputtering technology, dual Si targets, a vehicle speed of 1.0m / min, and powers of 9.6kw and 19.2kw respectively, to form a first inorganic barrier layer with a thickness of 20nm.
[0077] The hardening layer is composed of 40 parts of multifunctional acrylate trimethylolpropane triacrylate, 10 parts of polyethylene glycol resin, 2 parts of Efka No. 1173 photoinitiator, 35 parts of butanone, and 35 parts of propylene glycol methyl ether. The coating is evenly transferred to the surface of the first inorganic barrier layer by micro-concave coating, and then oven thermal curing and UV light curing are performed to form a hardening layer with a thickness of 4μm.
[0078] Through the magnetron sputtering process, dual Si targets, a vehicle speed of 1.0m / min, and powers of 9.6kw and 19.2kw respectively, SiO2 is evenly plated on the surface of the hardened layer to form a second inorganic barrier layer with a thickness of 20nm.
[0079] 50 parts of multifunctional acrylate trimethylolpropane triacrylate, 2 parts of Efka No. 1173 photoinitiator, 35 parts of organic solvent (35 parts of butanone, 35 parts of propylene glycol methyl ether, 15 parts of Al2O3 particles (Halimah Chemicals Co., Ltd. UVH-D-AL-24) were mixed evenly, and the coating was evenly transferred to the surface of the second inorganic barrier layer by micro-concave coating, followed by oven thermal curing and UV light curing to form a high-refractive organic resin layer with a thickness of 130nm.
[0080] Through the magnetron sputtering process, double Si target material, vehicle speed 1.0m / min, power 9.6kw and 19.2kw respectively, SiO2 is evenly plated on the surface of the high-refractive organic resin layer to form a third inorganic barrier layer with a thickness of 20nm.
[0081] After mixing 100 parts of hardening resin (Shanghai Lien Chemical Model A-2505LR), 4 parts of silica particles (Nissan Chemical PGM-AC-4130Y), 200 parts of organic solvent (methyl isobutyl ketone), 1 part of AF additive (Shin-Etsu KY-1203) and 1 part of silane coupling agent (Shin-Etsu KBM-503) evenly, the coating was evenly transferred to the surface of the third inorganic barrier layer by micro-concave coating, and then oven thermal curing and UV light curing were performed to form a low-reflection hydrophobic layer with a thickness of 100 nm. Finally, the low-reflection water vapor barrier film of the present invention was obtained.
[0082] Example 6
[0083] On a 50μm thick PET optical film produced by Japan's Toray Corporation, SiO2 was evenly plated on the surface of the substrate primer layer through a magnetron sputtering process, dual Si targets, a vehicle speed of 1.0m / min, and powers of 19.2kw and 19.2kw respectively, to form a first inorganic barrier layer with a thickness of 5nm.
[0084] The hardening layer is composed of 40 parts of multifunctional acrylate trimethylolpropane triacrylate, 10 parts of polyethylene glycol resin, 2 parts of Efka No. 1173 photoinitiator, 25 parts of butanone, and 25 parts of propylene glycol methyl ether. The coating is evenly transferred to the surface of the first inorganic barrier layer by micro-concave coating, and then oven thermal curing and UV light curing are performed to form a hardening layer with a thickness of 4μm.
[0085] Through the magnetron sputtering process, single Si target, vehicle speed 1.0m / min, power 4.8kw, SiO2 is evenly plated on the surface of the hardened layer to form a second inorganic barrier layer with a thickness of 5nm.
[0086] 50 parts of multifunctional acrylate trimethylolpropane triacrylate, 2 parts of Efka No. 1173 photoinitiator, 35 parts of butanone, 35 parts of propylene glycol methyl ether, and 15 parts of Al2O3 particles (Halimah Chemicals Co., Ltd. UVH-D-AL-24) were mixed evenly, and the coating was evenly transferred to the surface of the second inorganic barrier layer by micro-concave coating, followed by oven thermal curing and UV light curing to form a high-refractive organic resin layer with a thickness of 130nm.
[0087] Through the magnetron sputtering process, single Si target, vehicle speed 1.0m / min, power 4.8kw, SiO2 is evenly plated on the surface of the high-refractive organic resin layer to form a third inorganic barrier layer with a thickness of 5nm.
[0088] After mixing 100 parts of hardening resin (Shanghai Lien Chemical Model A-2505LR), 4 parts of silica particles (Nissan Chemical PGM-AC-4130Y), 200 parts of organic solvent (methyl isobutyl ketone), 1 part of AF additive (Shin-Etsu KY-1203) and 1 part of silane coupling agent (Shin-Etsu KBM-503) evenly, the coating was evenly transferred to the surface of the third inorganic barrier layer by micro-concave coating, and then oven thermal curing and UV light curing were performed to form a low-reflection hydrophobic layer with a thickness of 100 nm. Finally, the low-reflection water vapor barrier film of the present invention was obtained.
[0089] Comparative Example 1
[0090] The hardening layer is composed of 40 parts of multifunctional acrylate trimethylolpropane triacrylate, 10 parts of polyethylene glycol resin, 2 parts of Efka No. 1173 photoinitiator, 25 parts of butanone, and 25 parts of propylene glycol methyl ether. The coating is evenly transferred to the upper surface of a 50μm thick PET optical film produced by Toray Industries, Japan by micro-concave coating, and then oven thermal curing and UV light curing are performed to form a hardening layer with a thickness of 4μm.
[0091] 50 parts of multifunctional acrylate trimethylolpropane triacrylate, 2 parts of Efka No. 1173 photoinitiator, 35 parts of butanone, 35 parts of propylene glycol methyl ether, and 15 parts of Al2O3 particles (Harima Chemicals UVH-D-AL-24) were mixed evenly, and the coating was evenly transferred to the surface of the hardened layer by micro-concave coating, followed by oven thermal curing and UV light curing to form a high-refractive organic resin layer with a thickness of 130nm.
[0092] After mixing 100 parts of hardening resin (Shanghai Lien Chemical Model A-2505LR), 4 parts of silica particles (Nissan Chemical PGM-AC-4130Y), 200 parts of organic solvent (methyl isobutyl ketone), 1 part of AF additive (Shin-Etsu KY-1203) and 1 part of silane coupling agent (Shin-Etsu KBM-503) evenly, the coating was evenly transferred to the surface of the high-refractive organic resin layer by micro-concave coating, followed by oven thermal curing and UV light curing to form a low-refractive hydrophobic layer with a thickness of 100nm. Finally, a low-reflection water vapor barrier film was obtained.
[0093] Comparative Example 2
[0094] The hardening layer is composed of 40 parts of multifunctional acrylate trimethylolpropane triacrylate, 10 parts of polyethylene glycol resin, 2 parts of Efka No. 1173 photoinitiator, 25 parts of butanone, and 25 parts of propylene glycol methyl ether. The coating is evenly transferred to the upper surface of a 50μm thick PET optical film produced by Toray Industries, Japan by micro-concave coating, and then oven thermal curing and UV light curing are performed to form a hardening layer with a thickness of 4μm.
[0095] 50 parts of multifunctional acrylate trimethylolpropane triacrylate, 2 parts of Efka No. 1173 photoinitiator, 35 parts of butanone, 35 parts of propylene glycol methyl ether, and 15 parts of Al2O3 particles (Harima Chemicals UVH-D-AL-24) were mixed evenly, and the coating was evenly transferred to the surface of the hardened layer by micro-concave coating, followed by oven thermal curing and UV light curing to form a high-refractive organic resin layer with a thickness of 130nm.
[0096] After mixing 100 parts of hardening resin (Shanghai Lien Chemical Model A-2505LR), 4 parts of silica particles (Nissan Chemical PGM-AC-4130Y), and 200 parts of organic solvent (methyl isobutyl ketone) evenly, the coating was evenly transferred to the surface of the high-refractive organic resin layer by micro-concave coating, followed by oven thermal curing and UV light curing to form a low-refractive hydrophobic layer with a thickness of 100nm. Finally, a low-reflection water vapor barrier film was obtained.
[0097] The following performance tests were performed on the water-blocking films obtained in Examples 1 to 6 and Comparative Examples 1 and 2:
[0098] (1) Adhesion: 100-grid test.
[0099] (2) Water vapor transmission rate: According to the requirements of GB / T 1037, the test sample is placed in a water vapor transmission rate tester for testing.
[0100] (3) Reflectivity: tested by Olympus reflectometer.
[0101] (4) Top drop angle: Drop the liquid to be tested on the surface: Use a dropper or syringe to carefully drop the drop on the solid surface. Observe and measure: Use a microscope or camera to record the morphology of the drop on the surface and measure the angle between the drop and the surface contact line.
[0102] The data shown in the following table is obtained:
[0103]
[0104] From the performance test data of Examples 1 to 6 and Comparative Examples 1 and 2, it can be found that the low-reflection water vapor barrier film of the present invention can achieve low reflection and high water and oxygen barrier effects. Adding an inorganic barrier layer will increase the water and oxygen barrier rate while reducing the reflectivity.
[0105] Under the same conditions, a hydrophobic layer is formed on the surface by introducing a combination of AF additive (Shin-Etsu KY-1203) and silane coupling agent (Shin-Etsu KBM-503) (Shin-Etsu KBM-503), which can effectively improve the water and oxygen barrier rate.
[0106] In summary, the low-reflection water vapor barrier film of the present invention can effectively block water vapor and oxygen while reducing the reflectivity of the water vapor barrier film by stacking multiple organic barrier layers (hardening layer, high-refractive organic resin layer and low-refractive hydrophobic layer) and inorganic barrier layers with different refractive indices. Secondly, the low-refractive hydrophobic layer on the top layer can prevent it from falling off due to external forces, while allowing water molecules to naturally fall on the surface of the film layer under high humidity conditions, further improving the water vapor barrier performance.
[0107] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.
[0108] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A low-reflection water vapor barrier film, characterized in that: The substrate comprises a first inorganic barrier layer, a hardening layer, a second inorganic barrier layer, a high-fold organic resin layer, a third inorganic barrier layer and a low-fold hydrophobic layer which are sequentially stacked; The raw materials of the first inorganic barrier layer, the second inorganic barrier layer and the third inorganic barrier layer all include at least one of aluminum oxide, silicon oxide, silicon nitride and silicon oxynitride; The refractive index of the high-refractive organic resin layer is 1.6-1.7; the refractive index of the low-refractive hydrophobic layer is 1.3-1.4; the refractive index of the first inorganic barrier layer, the second inorganic barrier layer and the third inorganic barrier layer are all 1.40-1.76; the refractive index of the hardened layer is 1.5-1.
6.
2. The low-reflection water vapor barrier film according to claim 1, characterized in that: The low-fold hydrophobic layer comprises the following raw material components by weight: 80-120 parts of hardened resin, 3-5 parts of silicon dioxide particles, 180-220 parts of organic solvent, less than or equal to 1 part of AF auxiliary agent and less than or equal to 1 part of silane coupling agent.
3. The low-reflection water vapor barrier film according to claim 1, characterized in that: The high-refractive organic resin layer comprises the following raw material components by weight: 40-60 parts of multifunctional acrylate, 1-3 parts of photoinitiator, 10-20 parts of Al2O3 particles and 60-80 parts of organic solvent.
4. The low-reflection water vapor barrier film according to claim 1, characterized in that: The hardened layer comprises, by weight, 30 to 50 parts of multifunctional acrylate, 8 to 12 parts of polyethylene glycol resin, 1 to 3 parts of photoinitiator and 40 to 60 parts of organic solvent.
5. The low-reflection water vapor barrier film according to claim 3 or 4, characterized in that: The multifunctional acrylate includes one of trimethylolpropane triacrylate, trimethylolpentane trimethacrylate, dipentaerythritol acrylate, 2-ethylpentaerythritol triacrylate, trimethylolpropane triacrylate, pentaerythritol triacrylate, trimethylolpropane trimethacrylate, pentaerythritol tetraacrylate and dipentaerythritol hexaacrylate; and / or, The organic solvent is one or more of butanone, methyl isobutyl ketone, acetone, cyclopentanone, propylene glycol methyl ether, ethyl acetate, butyl acetate, amyl acetate, methanol, methyl isobutyl ketone, n-propanol, butanol, ethylene glycol ethyl ether, ethylene glycol butyl ether and diethylene glycol ethyl ether.
6. The low-reflection water vapor barrier film according to claim 1, characterized in that: The thickness of the low-fold hydrophobic layer is 80 to 120 nm; and / or, The thickness of the high-refractive organic resin layer is 50-150 nm.
7. The low-reflection water vapor barrier film according to claim 1, characterized in that: The thickness of the hardened layer is 3.5-4.5 μm.
8. The low-reflection water vapor barrier film according to claim 1, characterized in that: The thickness of the first inorganic barrier layer, the second inorganic barrier layer and the third inorganic barrier layer are all less than or equal to 80 nm.
9. The low-reflection water vapor barrier film according to claim 1, characterized in that: The thickness of the substrate is 50 to 100 μm, and the refractive index of the substrate is 1.5 to 1.
6.
10. The low-reflection water vapor barrier film according to claim 1, characterized in that: The substrate comprises a substrate body and a primer layer arranged on the substrate body, the primer layer is adhered to the first inorganic barrier layer, and the substrate body is a PET substrate.
Citation Information
Patent Citations
Water vapor barrier film
CN117565486A
Wet antireflection film
CN117567945A
Anti-reflection film and flexible display device
CN118276200A
Antireflection film and antireflection layer-affixed plastic substrate
CN1463367A
Antireflection film and its manufacturing process
JP2008207477A