Preparation method of halogen-free phosphorus-free flame-retardant glass felt laminated board

Halogen-free and phosphorus-free flame-retardant glass mat laminates were prepared by coating g-C3N4 filler with Mg(OH)2 and combining it with phenolphthalein-type benzoxazine and glycidyl ester-type epoxy resin, combined with microwave radiation and aluminum hydroxide treatment. This solved the problems of flame resistance and smoke suppression of laminates under extreme conditions, and achieved high flame retardancy and environmental protection.

CN118876558AActive Publication Date: 2024-11-01JIANGSU FURUNDA NEW MATERIAL TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410913021.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-11-01
Estimated Expiration
2044-07-09

AI Technical Summary

Technical Problem

Existing halogen-free and phosphorus-free laminates have insufficient flame retardancy under extreme conditions, and the limited amount of smoke suppressant added affects the performance of the boards, making it impossible to simultaneously meet the requirements of high flame retardancy and environmental protection.

Method used

Halogen-free and phosphorus-free flame-retardant glass mat laminates were prepared by combining Mg(OH)2-coated g-C3N4 filler with phenolphthalein-type benzoxazine and glycidyl ester-type epoxy resin, mixing by microwave radiation, and then treating glass mat with aluminum hydroxide and boric acid.

Benefits of technology

It improves the flame retardancy and smoke suppression of the laminate, meets the UL94 V0 standard, and has excellent machinability and flame resistance under extreme conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118876558A_ABST
    Figure CN118876558A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of a halogen-free phosphorus-free flame-retardant glass felt laminated board. The preparation method comprises the following steps: mixing a solvent, a curing agent and an accelerant to prepare curing accelerating liquid; then mixing phenolphthalein benzoxazine and glycidyl ester type epoxy resin, then adding the Mg (OH) 2 coated g-C3N4 filler and aluminum hydroxide, mixing to obtain an adhesive, and performing microwave irradiation on the adhesive to obtain a pretreated adhesive; treating the glass mat with boric acid to obtain an activated glass mat; the preparation method comprises the following steps: dipping an activated glass mat in a pretreatment adhesive, baking to obtain a prepreg, and then cutting, stacking and hot-pressing to obtain the halogen-free phosphorus-free flame-retardant glass mat laminated board, the laminated board can meet the halogen-free, phosphorus-free and flame-retardant requirements, the flame retardance reaches the UL94V0 level, and the laminated board is high in environmental protection property and also has excellent machining performance; after normal-temperature and low-temperature freezing treatment, 1200 DEG C melt resistance is good, large-area thermal shock resistance is good, and the smoke suppression effect is good.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a halogen-free and phosphorus-free flame-retardant glass felt laminate, belonging to the technical field of laminates. Background Art

[0002] In the composition of halogen-free material preparations, phosphides are generally selected as flame retardants to replace existing halogen compounds. However, since the phosphorus content cannot be too high, it will cause insufficient heat resistance.

[0003] At present, halogen-free laminates mainly use phosphorus-based flame retardants to replace brominated epoxy resins to achieve flame retardancy. However, phosphorus-based flame retardants can cause oxidation in rivers or lakes due to hydrolysis, which leads to another environmental issue. Therefore, based on environmental protection requirements, halogen-free and phosphorus-free flame-retardant laminates are the mainstream of development.

[0004] For laminated boards, some special applications (melting workshops) and the impact of flame particle flows, such as flame impact of combustibles and physical impact of combustibles, will affect the flame retardancy of the boards under extreme conditions. For some boards that have been in extreme low temperature environments for a long time, their own flame retardancy will be significantly reduced. In addition, the smoke suppression property depends on the added smoke suppressants (such as magnesium hydroxide, aluminum hydroxide, etc.). There is an upper limit to the amount of smoke suppressants added, and excessive addition will affect other properties of the boards.

[0005] Based on this, in the field of halogen-free, phosphorus-free, flame-retardant laminates, developing a laminate that has the above-mentioned properties has certain market prospects. Summary of the invention

[0006] In view of the shortcomings of the prior art, the present invention provides a method for preparing a halogen-free and phosphorus-free flame-retardant glass mat laminate. The specific technical scheme is as follows:

[0007] A method for preparing a halogen-free and phosphorus-free flame-retardant glass felt laminate comprises the following steps:

[0008] Step 1: Mix magnesium hydroxide and acetone in a mass ratio of 1: (2-3), ultrasonically disperse for 10-15 minutes, remove acetone by filtering, and dry at a temperature of 110-120°C to obtain refined magnesium hydroxide; the purpose of refining magnesium hydroxide is mainly to remove crystal water and remove impurities from the surface of magnesium hydroxide. Refined magnesium hydroxide, g-C3N4 powder, and acetone are mixed in a mass ratio of 10: (12-16): (150-200), ultrasonically dispersed, acetone removed, dried at a temperature of 60-65°C, and ground to obtain Mg(OH)2-coated g-C3N4 filler.

[0009] Step 2: Pour 200-250 parts by weight of solvent, 5-8 parts by weight of curing agent and 0.5-1.1 parts by weight of accelerator into a stirring kettle and stir and disperse to obtain a curing accelerator liquid; then pour 100 parts by weight of phenolphthalein type benzoxazine and 20-30 parts by weight of glycidyl ester type epoxy resin into the reaction kettle, stir and disperse to obtain a resin mixture; then add 20-30 parts by weight of Mg(OH)2 coated g-C3N4 filler to the resin mixture in batches and successively, stir and disperse, then add 3-5 parts by weight of aluminum hydroxide, and stir and disperse to obtain an adhesive.

[0010] Step 3: transfer the adhesive to a microwave reactor, react for 25 to 30 minutes at a microwave power of 200 to 260 W, and stir for 20 to 30 minutes to obtain a pretreated adhesive.

[0011] Step 4: immerse the glass felt in a boric acid solution with a mass fraction of 10 to 12%, perform ultrasonic treatment at a temperature of 75 to 80° C. for 30 to 40 minutes, take out the glass felt, and dry it to obtain an activated glass felt.

[0012] Step 5: immerse the activated glass felt in the pre-treated adhesive, then scrape the adhesive, and then put it into an oven and bake it at a temperature of 155-165° C. for 5-6 minutes to obtain a semi-cured sheet.

[0013] Step 6: Cut and stack the prepregs and send them into a hot press for hot pressing.

[0014] Step 7: After the hot pressing is completed, the mixture is cooled to room temperature and taken out to obtain the halogen-free and phosphorus-free flame-retardant glass felt laminate.

[0015] As a further improvement, in step 1, the frequency of ultrasonic dispersion is 20 kHz and the power is 300-500 W.

[0016] In a further improvement, the solvent is one or more of acetone and butanone.

[0017] In a further improvement, the curing agent is dicyandiamide.

[0018] In a further improvement, the accelerator is 2-methylimidazole.

[0019] As a further improvement, in step 4, the frequency of ultrasonic treatment is 22-23 kHz and the power is 120-150 W.

[0020] As a further improvement, in step 6, the temperature in the hot press is increased to 205-215°C by gradient, and the pressure is increased to 0.85-0.9 MPa by gradient, and hot pressing is performed for 2 hours under the conditions of 205-215°C and 0.85-0.9 MPa.

[0021] Beneficial effects of the present invention:

[0022] 1. The present invention effectively solves the problem of uneven distribution of components inside the resin by adding Mg(OH)2-coated g-C3N4 filler to the composite resin of phenolphthalein type benzoxazine and glycidyl ester type epoxy resin and irradiating the resin mixture with microwaves. The distribution of the filler tends to be consistent, and while improving the flame retardancy, the compatibility and reactivity between the filler and the resin are also improved, and the large-area thermal shock resistance of the laminated board to 1200°C melt after room temperature and low-temperature freezing treatment is significantly improved.

[0023] 2. The resin composition (pretreatment adhesive), prepreg and laminate of the present invention can achieve the requirements of halogen-free, phosphorus-free and flame-retardant, with flame retardancy reaching UL94 V0 level, high environmental protection and excellent mechanical processing performance.

[0024] 3. The resin composition (pretreated adhesive) of the present invention has good smoke suppression effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a photo of the halogen-free and phosphorus-free flame-retardant glass felt laminated board described in Example 1;

[0026] Figure 2 This is a photo of the halogen-free and phosphorus-free flame-retardant glass mat laminate described in Example 2;

[0027] Figure 3 This is a physical photograph of the halogen-free and phosphorus-free flame-retardant glass felt laminate described in Example 3. DETAILED DESCRIPTION

[0028] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0029] Example 1

[0030] Step 1, after magnesium hydroxide and acetone are mixed in a mass ratio of 1:2, ultrasonic dispersion is performed for 10 minutes, the frequency of ultrasonic dispersion is 20kHz, and the power is 300W; remove acetone, and dry at a temperature of 120°C to obtain refined magnesium hydroxide; refine magnesium hydroxide, g-C3N4 powder, and acetone are mixed in a mass ratio of 10:12:150, ultrasonic dispersion is performed, acetone is removed, drying is performed at a temperature of 60°C, and grinding is performed to obtain Mg(OH)2-coated g-C3N4 filler.

[0031] Step 2: Pour 250 kg of acetone, 8 kg of dicyandiamide and 1.1 kg of 2-methylimidazole into a stirring kettle and stir and disperse them to obtain a curing promoting liquid; then pour 100 kg of phenolphthalein type benzoxazine and 30 kg of glycidyl ester type epoxy resin into the reaction kettle, stir and disperse them to obtain a resin mixture; then add 30 kg of Mg(OH)2-coated g-C3N4 filler to the resin mixture in batches and successively, stir and disperse them, then add 5 kg of aluminum hydroxide, and stir and disperse them to obtain an adhesive.

[0032] Step 3: transfer the adhesive to a microwave reactor, react for 30 min at a microwave power of 260 W, and stir for 30 min to obtain a pretreated adhesive.

[0033] Step 4, immersing the glass felt in a boric acid solution with a mass fraction of 12%, ultrasonically treating it at a temperature of 80° C. for 40 minutes, taking out the glass felt, and drying it to obtain an activated glass felt; the frequency of the ultrasonic treatment is 23 kHz, and the power is 150 W.

[0034] Step 5: immerse the activated glass felt in the pre-treated adhesive, scrape the adhesive, and then put it into an oven and bake it at 165° C. for 6 minutes to obtain a semi-cured sheet.

[0035] Step 6: Cut and stack the prepregs and send them into a hot press for hot pressing. The temperature in the hot press is increased to 205° C. and the pressure is increased to 0.85 MPa by a gradient, and hot pressing is performed for 2 hours at 205° C. and 0.85 MPa.

[0036] Step 7: After the hot pressing is completed, the mixture is cooled to room temperature and taken out to obtain the halogen-free and phosphorus-free flame-retardant glass felt laminate. See the actual photo for details. Figure 1 .

[0037] Example 2

[0038] Step 1, after magnesium hydroxide and acetone are mixed in a mass ratio of 1:2.6, ultrasonic dispersion is performed for 13 minutes, the frequency of ultrasonic dispersion is 20kHz, and the power is 350W; remove acetone, and dry at a temperature of 105°C to obtain refined magnesium hydroxide; refine magnesium hydroxide, g-C3N4 powder, and acetone are mixed in a mass ratio of 10:15:150, ultrasonic dispersion is performed, acetone is removed, drying is performed at a temperature of 60°C, and grinding is performed to obtain Mg(OH)2-coated g-C3N4 filler.

[0039] Step 2: Pour 220 kg of acetone, 7 kg of dicyandiamide and 1 kg of 2-methylimidazole into a stirring kettle and stir and disperse them to obtain a curing promoting liquid; then pour 100 kg of phenolphthalein type benzoxazine and 25 kg of glycidyl ester type epoxy resin into the reaction kettle, stir and disperse them to obtain a resin mixture; then add 28 kg of Mg(OH)2-coated g-C3N4 filler to the resin mixture in batches and successively, stir and disperse them, then add 5 kg of aluminum hydroxide, and stir and disperse them to obtain an adhesive.

[0040] Step 3: transfer the adhesive to a microwave reactor, react for 30 min at a microwave power of 230 W, and stir for 20 min to obtain a pretreated adhesive.

[0041] Step 4, immersing the glass felt in a boric acid solution with a mass fraction of 11%, ultrasonically treating the glass felt at a temperature of 80° C. for 30 minutes, taking out the glass felt, and drying the glass felt to obtain an activated glass felt; the frequency of the ultrasonic treatment is 22 kHz, and the power is 150 W.

[0042] Step 5: immerse the activated glass felt in the pre-treated adhesive, then scrape the adhesive, and then put it into an oven and bake it at 160° C. for 5 minutes to obtain a semi-cured sheet.

[0043] Step 6: Cut and stack the prepregs and send them into a hot press for hot pressing. The temperature in the hot press is increased to 210° C. and the pressure is increased to 0.87 MPa by a gradient, and hot pressing is performed for 2 hours at 210° C. and 0.87 MPa.

[0044] Step 7: After the hot pressing is completed, the mixture is cooled to room temperature and taken out to obtain the halogen-free and phosphorus-free flame-retardant glass felt laminate. See the actual photo for details. Figure 2 .

[0045] Example 3

[0046] Step 1, after magnesium hydroxide and acetone are mixed in a mass ratio of 1:3, ultrasonic dispersion is performed for 15 minutes, the frequency of ultrasonic dispersion is 20kHz, and the power is 500W; remove acetone, and dry at a temperature of 110°C to obtain refined magnesium hydroxide; refine magnesium hydroxide, g-C3N4 powder, and acetone are mixed in a mass ratio of 10:16:200, ultrasonic dispersion is performed, acetone is removed, drying is performed at a temperature of 65°C, and grinding is performed to obtain Mg(OH)2-coated g-C3N4 filler.

[0047] Step 2: Pour 200 kg of acetone, 5 kg of dicyandiamide and 0.5 kg of 2-methylimidazole into a stirring kettle, stir and disperse, and obtain a curing promoting liquid; then pour 100 kg of phenolphthalein type benzoxazine and 20 kg of glycidyl ester type epoxy resin into the reaction kettle, stir and disperse, and obtain a resin mixture; then add 20 kg of Mg(OH)2 coated g-C3N4 filler to the resin mixture in batches and successively, stir and disperse, and then add 3 kg of aluminum hydroxide, and stir and disperse to obtain an adhesive.

[0048] Step 3: transfer the adhesive to a microwave reactor, react for 25 min at a microwave power of 200 W, and stir for 20 min to obtain a pretreated adhesive.

[0049] Step 4, immersing the glass felt in a boric acid solution with a mass fraction of 10%, ultrasonically treating it at a temperature of 75°C for 30 minutes, taking out the glass felt, and drying it to obtain an activated glass felt; the frequency of the ultrasonic treatment is 22kHz, and the power is 120W.

[0050] Step 5: immerse the activated glass felt in the pre-treated adhesive, then scrape the adhesive, and then put it into an oven and bake it at 155° C. for 5 minutes to obtain a semi-cured sheet.

[0051] Step 6: Cut and stack the prepregs, and send them into a hot press for hot pressing. The temperature in the hot press is increased to 215° C. and the pressure is increased to 0.9 MPa by a gradient, and hot pressing is performed for 2 hours at 215° C. and 0.9 MPa.

[0052] Step 7: After the hot pressing is completed, the mixture is cooled to room temperature and taken out to obtain the halogen-free and phosphorus-free flame-retardant glass felt laminate. See the actual photo for details. Figure 3 .

[0053] Comparative Example 1

[0054] Compared with Example 1, in this example, the Mg(OH)2-coated g-C3N4 filler used in Step 2 is replaced with refined magnesium hydroxide, and the rest remains unchanged; finally, a control plate 1 is obtained.

[0055] Comparative Example 2

[0056] Compared with Example 1, in this example, the Mg(OH)2-coated g-C3N4 filler used in Step 2 is replaced with refined magnesium hydroxide and g-C3N4 powder grinding material (refined magnesium hydroxide and g-C3N4 powder are mixed in a mass ratio of 10:12 and then ground), and the rest remains unchanged; finally, the control plate 2 is obtained.

[0057] Comparative Example 3

[0058] Compared with Example 1, in this example, the Mg(OH)2-coated g-C3N4 filler used in Step 2 is replaced with g-C3N4 powder, and the rest remains unchanged; finally, a control plate 3 is obtained.

[0059] Comparative Example 4

[0060] Compared with Example 1, in this example, the Mg(OH)2-coated g-C3N4 filler used in step 2 is replaced by Al(OH)3-coated g-C3N4 filler, and the rest remains unchanged; finally, a control plate 4 is obtained. Among them, the magnesium hydroxide in step 1 is replaced by aluminum hydroxide, and finally the Al(OH)3-coated g-C3N4 filler is obtained.

[0061] Comparative Example 5

[0062] Compared with Example 1, in this example, step 3 is not performed, that is, the adhesive is not reacted under microwaves, and the activated glass felt is directly immersed in the adhesive in step 5, and the rest remains unchanged; finally, a control board 5 is obtained.

[0063] Comparative Example 6

[0064] Compared with Example 1, in this example, step 4 is not performed, that is, the glass felt is not ultrasonically treated in the boric acid solution, and the glass felt is directly immersed in the pretreated adhesive in step 5, and the rest remains unchanged; finally, a control board 6 is obtained.

[0065] The properties of the laminates corresponding to Examples 1 to 3 and Comparative Examples 1 to 6 are shown in Table 1:

[0066] Table 1

[0067]

[0068] It can be seen from Table 1 that g-C3N4 is a lightweight material and is not easy to be added alone into the resin glue. For example, in Control Example 2, direct addition can easily lead to uneven distribution of fillers, which not only fails to exert the relevant performance of the filler, but also causes interference. After g-C3N4 and magnesium hydroxide are treated, magnesium hydroxide is coated around g-C3N4 to form a composite powder, thereby solving the large-area agglomeration of fillers; in addition, the addition of Mg(OH)2-coated g-C3N4 filler can significantly improve the large-area thermal shock resistance of the laminate, and even if the laminate is treated at extremely low temperatures, it still has excellent large-area thermal shock resistance.

[0069] 《Large Area Melt Thermal Shock Investigation》

[0070] 1. Cut the laminates corresponding to Examples 1 to 3 and Comparative Examples 1 to 6 into 50 cm×50 cm sample plates, and then put iron bars around the sample plates and tighten them. The purpose of the iron bars is to prevent the subsequent tin-copper alloy melt from flowing out.

[0071] 2. Liquid carbon dioxide untreated group: Pour 1200℃ tin-copper alloy melt on the front of the sample plate and cover the front of the sample plate. The thickness of the tin-copper alloy melt layer on the surface of the sample plate is 3±0.5mm. After 10 minutes, throw the sample plate into water to cool and clean it, and observe whether there is back burn-through on the back of the sample plate. If there is burn-through, use the grid method to calculate the total area of ​​burn-through. Burn-through rate = total area of ​​burn-through / area of ​​sample plate.

[0072] 3. Immerse the sample plate with the iron bar in liquid carbon dioxide for 1 hour, take it out, and place it at room temperature for 30 minutes. Then pour 1200℃ tin-copper alloy melt on the front of the sample plate and cover the front of the sample plate. The thickness of the tin-copper alloy melt layer on the surface of the sample plate is 3±0.5mm. After 10 minutes, throw the sample plate into water to cool and clean it, and observe whether there is back burn-through on the back of the sample plate. If there is burn-through, use the grid method to calculate the total area of ​​burn-through. Burn-through rate = total area of ​​burn-through / area of ​​sample plate.

[0073] 《Study on the Smoke Suppression of Resins》

[0074] The smoke suppression properties of the pretreated adhesive in Example 1, the adhesive, and the corresponding pretreated adhesives in Comparative Examples 1 to 4 were investigated, and the smoke density Ds4 was tested according to ISO 5659 standard. The results are shown in Table 2:

[0075] Table 2

[0076]

[0077]

[0078] It can be seen from Table 2 that the smoke suppression effect brought about by adding Mg(OH)2-coated g-C3N4 filler is better than that brought about by adding g-C3N4 or magnesium hydroxide alone.

[0079] In the above examples, the phenolphthalein type benzoxazine was purchased from Jinan Shengquan Group Co., Ltd.; the glycidyl ester type epoxy resin was purchased from Jinan Shengquan Group Co., Ltd., which is a halogen-free and phosphorus-free resin. g-C3N4 is a graphite-like carbon nitride, which was purchased from Guangdong Shengke Biochemical Technology Co., Ltd.

[0080] "Large Area Melt Thermal Shock Investigation" mainly examines the plate's resistance to flame particle flow impact (such as the impact of burning materials).

[0081] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a halogen-free and phosphorus-free flame-retardant glass mat laminate, characterized in that: The following steps are involved: Step 1, after magnesium hydroxide and acetone are mixed in a mass ratio of 1: (2-3), ultrasonic dispersion is performed for 10-15 minutes, acetone is removed, and drying is performed at a temperature of 110-120° C. to obtain refined magnesium hydroxide; refined magnesium hydroxide, g-C3N4 powder, and acetone are mixed in a mass ratio of 10: (12-16): (150-200), ultrasonic dispersion is performed, acetone is removed, drying is performed at a temperature of 60-65° C., and grinding is performed to obtain Mg(OH)2-coated g-C3N4 filler; Step 2, pour 200-250 parts by mass of solvent, 5-8 parts by mass of curing agent, and 0.5-1.1 parts by mass of accelerator into a stirring kettle, stir and disperse, and obtain a curing accelerator liquid; then pour 100 parts by mass of phenolphthalein type benzoxazine and 20-30 parts by mass of glycidyl ester type epoxy resin into the reaction kettle, stir and disperse, and obtain a resin mixture; then add 20-30 parts by mass of Mg(OH)2 coated g-C3N4 filler to the resin mixture in batches and successively, stir and disperse, and then add 3-5 parts by mass of aluminum hydroxide, stir and disperse to obtain an adhesive; Step 3, transferring the adhesive to a microwave reactor, reacting for 25 to 30 minutes under a microwave power of 200 to 260 W, and stirring for 20 to 30 minutes to obtain a pretreated adhesive; Step 4, immersing the glass felt in a boric acid solution with a mass fraction of 10 to 12%, ultrasonically treating the glass felt at a temperature of 75 to 80° C. for 30 to 40 minutes, taking out the glass felt, and drying the glass felt to obtain an activated glass felt; Step 5, immersing the activated glass felt in the pre-treated adhesive, and then scraping the adhesive, and then putting it into an oven and baking it at a temperature of 155-165° C. for 5-6 minutes to obtain a prepreg; Step 6: Cut and stack the prepregs and send them into a hot press for hot pressing; Step 7: After the hot pressing is completed, the mixture is cooled to room temperature and taken out to obtain the halogen-free and phosphorus-free flame-retardant glass felt laminate.

2. The method for preparing a halogen-free and phosphorus-free flame-retardant glass mat laminate according to claim 1, characterized in that: In step 1, the frequency of ultrasonic dispersion is 20 kHz and the power is 300-500 W.

3. The method for preparing a halogen-free and phosphorus-free flame-retardant glass mat laminate according to claim 1, characterized in that: The solvent is one or more of acetone and butanone.

4. The method for preparing a halogen-free and phosphorus-free flame-retardant glass mat laminate according to claim 1, characterized in that: The curing agent is dicyandiamide.

5. The method for preparing a halogen-free and phosphorus-free flame-retardant glass mat laminate according to claim 1, characterized in that: The accelerator is 2-methylimidazole.

6. The method for preparing a halogen-free and phosphorus-free flame-retardant glass mat laminate according to claim 1, characterized in that: In step 4, the frequency of ultrasonic treatment is 22-23 kHz and the power is 120-150 W.

7. The method for preparing a halogen-free and phosphorus-free flame-retardant glass mat laminate according to claim 1, characterized in that: In step 6, the temperature in the hot press is increased to 205-215° C. by gradient, and the pressure is increased to 0.85-0.9 MPa by gradient, and hot pressing is performed for 2 hours at 205-215° C. and 0.85-0.9 MPa.

Citation Information

Patent Citations

  • Carbon nitride-coated superconductive graphene electrode material and preparation method thereof

    CN106328242A

  • Low-smoke high-oxygen-index composition, flame-retardant rubber and preparation method of flame-retardant rubber

    CN115109319A

  • Cyanic acid ester compound, method for producing same, resin composition, cured product, prepreg, material for encapsulation, fiber-reinforced composite material, adhesive, metal foil-clad laminate, resin sheet, and printed circuit board

    US20190112410A1

  • Catalyst for decarbonylation reaction, and preparation method for catalyst and use thereof

    WO2023093492A1