Porous carbon material, silicon-carbon negative electrode material, and preparation method and application of porous carbon material and silicon-carbon negative electrode material

By using porous carbon materials to control the coordination of surface functional groups and nanosilicon particles in silicon carbon anode materials, the problem of unsatisfactory electrical performance of silicon carbon materials is solved, and efficient electrochemical performance improvement of lithium-ion batteries is achieved.

CN118877877APending Publication Date: 2024-11-01LIYANG ZICHEN NEW MATERIALS TECH CO LTD +2

Patent Information

Application Number
CN202411377080.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The existing silicon carbon negative electrode materials have poor silicon utilization and poor electrical performance, which leads to rapid attenuation of lithium-ion battery capacity, limiting its industrial application.

Method used

Porous carbon materials are used to control the content and types of surface functional groups, and the conductivity and wettability of silicon carbon materials are improved, and nanosilicon particles are deposited in porous carbon materials through vapor deposition to form an efficient silicon carbon negative electrode material.

Benefits of technology

It significantly improves the conductivity, capacity and circulation performance of silicon-carbon anode materials, extends the cycle life of lithium-ion batteries, and improves the rate performance and safety performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention relates to the technical field of batteries, in particular to a porous carbon material, a silicon-carbon negative electrode material and a preparation method and application of the porous carbon material and the silicon-carbon negative electrode material. The invention relates to a porous carbon material, the porous carbon material has surface functional groups, the surface functional groups comprise basic functional groups, neutral functional groups and acidic functional groups, the content of the surface functional groups is 0.4-1 mmol / g, the content of the basic functional groups is 0.2-0.5 mmol / g, the content of the neutral functional groups is 0.2-0.4 mmol / g, and the content of the acidic functional groups is less than 0.2 mmol / g. The surface of the porous carbon material has functional groups with proper content and types, so that the porous carbon has high conductivity and proper wettability, the silicon utilization rate of the silicon-carbon negative electrode material is improved, and the cycle performance and the rate capability of the silicon-carbon negative electrode material are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of battery technology, and in particular to a porous carbon material, a silicon-carbon negative electrode material, and a preparation method and application thereof. Background Art

[0002] Lithium-ion batteries have been widely used in electric vehicles, mobile devices and other fields. One of the key factors affecting the electrical performance of lithium-ion batteries is the negative electrode material. Existing commercial negative electrode materials include mesophase carbon microspheres and modified graphite, but they have disadvantages such as low theoretical lithium storage capacity and easy co-embedding of organic solvents.

[0003] Among the current lithium storage materials, silicon has the highest theoretical capacity (4200mAh / g), but the huge volume change of silicon negative electrode materials during the battery charging and discharging process causes the electrode active materials to fall off and pulverize, and even causes damage to the electrode structure, resulting in rapid attenuation of battery capacity, which seriously restricts its industrial application. In the prior art, silicon and carbon materials are compounded to obtain silicon-carbon composite materials to alleviate the volume change of silicon during the charging and discharging process. However, the utilization rate of silicon in the preparation process of the current silicon-carbon negative electrode material is poor, and the electrical performance of the silicon-carbon negative electrode material is not ideal.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] One object of the present invention is to provide a porous carbon material to solve the technical problems of poor silicon utilization and unsatisfactory electrical properties of silicon-carbon negative electrode materials in the prior art; the porous carbon of the present invention has surface functional groups with appropriate content and types, which is beneficial to improve the utilization rate of silicon in the silicon-carbon material and improve the electrical properties of the silicon-carbon material.

[0006] Another object of the present invention is to provide a silicon-carbon negative electrode material having high electrical conductivity, high capacity and high cycle performance.

[0007] Another object of the present invention is to provide a method for preparing a silicon-carbon negative electrode material, which is simple and easy to implement, and the obtained silicon-carbon negative electrode material has excellent electrical properties.

[0008] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted: A porous carbon material, the porous carbon material having surface functional groups, the surface functional groups comprising basic functional groups, neutral functional groups and acidic functional groups; the content of the surface functional groups is 0.4-1 mmol / g, the content of the basic functional groups is 0.2-0.5 mmol / g, the content of the neutral functional groups is 0.2-0.4 mmol / g, and the content of the acidic functional groups is less than 0.2 mmol / g. In some embodiments, the content of the surface functional groups is 0.4-0.7 mmol / g, wherein the content of the basic functional groups is 0.2-0.5 mmol / g, the content of the neutral functional groups is 0.2-0.4 mmol / g, and the content of the acidic functional groups is less than 0.1 mmol / g.

[0009] In some embodiments, the basic functional group comprises a carbonyl group, the neutral functional group comprises a phenolic hydroxyl group, and the acidic functional group comprises a hydroxyl group and a carboxyl group.

[0010] In some embodiments, the electrical conductivity of the porous carbon material is 2-5 S / mm.

[0011] In some embodiments, the pH of the porous carbon material is 6.8-8.

[0012] In some embodiments, the particle size Dv50 of the porous carbon material is 3-10 μm.

[0013] In some embodiments, the particle size Dv99 of the porous carbon material is 10-25 μm, and the particle size Dn10 of the porous carbon material is 0.5-5 μm.

[0014] In some embodiments, the specific surface area of ​​the porous carbon material is 1000-2200 m 2 / g.

[0015] In some embodiments, the pore volume of the porous carbon material is 0.6-1.2 cm 3 / g.

[0016] In some embodiments, the microporosity of the porous carbon material is 50% to 100%.

[0017] A silicon-carbon negative electrode material comprises the porous carbon material and nano silicon particles located in the pores of the porous carbon material.

[0018] In some embodiments, the mass content of nano silicon particles in the silicon-carbon negative electrode material is 5% to 85%.

[0019] In some embodiments, the particle size Dv50 of the silicon-carbon negative electrode material is 3-10 μm, the particle size Dv99 of the silicon-carbon negative electrode material is 10-25 μm, and the particle size Dn10 of the silicon-carbon negative electrode material is 0.5-5 μm.

[0020] In some embodiments, the specific surface area of ​​the silicon-carbon negative electrode material is less than 3m 2 / g.

[0021] In some embodiments, the electrical conductivity of the silicon-carbon negative electrode material is 0.2~2S / mm.

[0022] In some embodiments, the surface of the silicon-carbon negative electrode material further includes a coating layer; the coating layer contains at least one of amorphous carbon, a fast ion conductor and a high molecular polymer.

[0023] The method for preparing the silicon-carbon negative electrode material comprises the following steps: The porous carbon material is vapor deposited in an atmosphere containing a silicon source to obtain the silicon-carbon negative electrode material.

[0024] In some embodiments, the method further includes: coating the silicon-carbon negative electrode material to obtain a coating layer on the surface of the silicon-carbon negative electrode material, wherein the coating layer contains at least one of amorphous carbon, a fast ion conductor and a high molecular polymer.

[0025] An electrode comprises the silicon-carbon negative electrode material.

[0026] A lithium ion battery comprises the electrode.

[0027] An electrical device comprises the lithium-ion battery.

[0028] Compared with the prior art, the present invention has the following beneficial effects: (1) The present invention controls the surface of the porous carbon material to have an appropriate content and type of functional groups, thereby ensuring high electrical conductivity, wettability and stability of the porous carbon.

[0029] (2) The silicon-carbon negative electrode material of the present invention, the combination of porous carbon and nano-silicon particles, can ensure that it has high conductivity, high capacity and high cycle performance.

[0030] (3) The preparation method of the silicon-carbon negative electrode material of the present invention adopts a specific porous carbon material, which is beneficial to the adsorption effect of the porous carbon on the silicon-containing gas, and can improve the silicon utilization rate of the silicon-containing gas, so that the final silicon-carbon negative electrode material has high electrical conductivity and suitable wettability, thereby improving its capacity and improving its cycle performance.

[0031] (4) The lithium-ion battery obtained from the silicon-carbon negative electrode material of the present invention has excellent cycle performance, rate performance and safety performance. DETAILED DESCRIPTION

[0032] The embodiments of the present invention will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. If no specific conditions are specified in the examples, the conditions are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be obtained commercially.

[0033] According to one invention of the present invention, the present invention relates to a porous carbon material, wherein the porous carbon material has surface functional groups, and the surface functional groups include basic functional groups, neutral functional groups and acidic functional groups; the content of the surface functional groups is 0.4~1mmol / g, the content of the basic functional groups is 0.2~0.5mmol / g, the content of the neutral functional groups is 0.2~0.4mmol / g, and the content of the acidic functional groups is less than 0.2mmol / g.

[0034] The oxygen-containing functional groups on the surface of carbon materials can be divided into acidic functional groups (such as carboxyl groups and carboxylic anhydride), neutral functional groups (also known as weakly acidic functional groups, such as phenolic hydroxyl groups, epoxy groups, ether groups, etc.), and basic functional groups (such as quinones, carbonyl groups, etc.). Surface functional groups have a very important influence on the conductivity, wettability of materials, rate performance, and cycle life. The present invention controls the surface of the porous carbon material to have an appropriate content of functional groups, thereby ensuring the high conductivity, wettability, and stability of the porous carbon material. Since the rate capability of silicon-carbon negative electrode materials is significantly affected by porous carbon, and the rate capability of porous carbon materials depends on the influence of oxygen-containing functional groups on the ion diffusion and conductivity of carbon materials, and the total content of surface functional groups is often inversely proportional to the conductivity (the decrease in conductivity is due to the introduction of oxygen-containing functional groups that increase defects, sp3 carbon and impedance); if there are too many surface functional groups, ion diffusion will be hindered, the rate performance will be reduced, and the first effect of porous carbon materials will be significantly reduced; and complete deoxygenation will reduce the wettability of porous carbon materials; the presence of surface functional groups can not only change the hydrophobicity of the surface of porous carbon materials, but also provide adsorption sites for many reactions. Hydrophilic groups (hydroxyl, carboxyl) can effectively improve the wettability of carbon materials, which is more beneficial to the cycle life of silicon-carbon negative electrode materials. Therefore, the present invention controls the total content of surface functional groups of porous carbon materials within the above-mentioned suitable range to facilitate the performance of silicon-carbon negative electrode materials. In some embodiments, the content of surface functional groups of the porous carbon is 0.4~1mmol / g, for example, it can be but not limited to 0.4mmol / g, 0.45mmol / g, 0.5mmol / g, 0.55mmol / g, 0.6mmol / g, 0.7mmol / g, 0.8mmol / g, 0.9mmol / g, 1mmol / g, etc., or any range value between two thereof.

[0035] Among the above-mentioned functional groups, carboxyl and hydroxyl are unstable functional groups, while carbonyl and phenolic hydroxyl are more stable. The redox reaction of unstable oxygen-containing functional groups is irreversible, which will not only cause the capacity contributed by oxygen-containing functional groups to decay rapidly, but may also block the pore structure of porous carbon materials, resulting in a significant decrease in the overall cycle stability of subsequent silicon-carbon materials. Therefore, unstable groups are removed through high temperature and other processes to make the content of acidic functional groups less than 0.2 mmol / g, and to ensure that the basic functional groups and neutral functional groups have the above-mentioned appropriate contents, so that the content of stable functional groups in the porous carbon material is greater than the content of unstable functional groups, so that the porous carbon has high conductivity and suitable wettability. In some embodiments, the content of basic functional groups can be, for example, but not limited to, 0.2mmol / g, 0.25mmol / g, 0.3mmol / g, 0.35mmol / g, 0.4mmol / g, 0.5mmol / g, etc., or any range value between the two; the content of neutral functional groups can be, for example, but not limited to, 0.2mmol / g, 0.25mmol / g, 0.3mmol / g, 0.35mmol / g, 0.4mmol / g, etc., or any range value between the two; the content of acidic functional groups can be, for example, but not limited to, 0, 0.02mmol / g, 0.05mmol / g, 0.08mmol / g, 0.1mmol / g, 0.12mmol / g, 0.15mmol / g, 0.19mmol / g, etc., or any range value between the two.

[0036] In addition, the oxygen-containing functional groups on the surface of porous carbon materials can increase the adsorption sites. The content and distribution of functional groups have a significant effect on the adsorption of porous carbon materials. They usually increase the polarity of the surface of porous carbon materials, thereby enhancing the interaction with silicon material molecules, which is beneficial to promote adsorption and diffusion in the preparation of silicon-carbon negative electrode materials, and is beneficial to the preparation of silicon-carbon negative electrode materials and their performance. In some embodiments, the content of the surface functional groups is 0.4-0.7 mmol / g, wherein the content of the basic functional groups is 0.2-0.5 mmol / g, the content of the neutral functional groups is 0.2-0.4 mmol / g, and the content of the acidic functional groups is less than 0.1 mmol / g. The present invention further optimizes the content range of the total surface functional groups and the content ranges of the basic functional groups, neutral functional groups, and acidic functional groups, thereby being more conducive to the coordinated acquisition of porous carbon materials with high conductivity, suitable wettability, and high stability.

[0037] In some embodiments, the electrical conductivity of the porous carbon material is 2-5S / mm, for example, it can be but not limited to 2S / mm, 2.2S / mm, 2.5S / mm, 2.8S / mm, 3S / mm, 3.2S / mm, 3.5S / mm, 3.8S / mm, 4S / mm, 5S / mm, etc., or any range value therebetween. The porous carbon of the present invention has a high electrical conductivity, which lays a good foundation for the subsequent acquisition of high-conductivity silicon-carbon negative electrode materials to improve the electrical properties of silicon-carbon negative electrode materials.

[0038] In some embodiments, the pH of the porous carbon material is 6.8 to 8, for example, it can be but not limited to 6.8, 6.9, 7, 7.1, 7.2, 7.5, 7.8 or 8, or any range between the two. The surface functional groups of the porous carbon of the present invention mainly contain basic functional groups and neutral functional groups, and the pH of the obtained porous carbon is 6.8 to 8.

[0039] In some embodiments, the particle size Dv50 of the porous carbon material is 3 to 10 μm, for example, it can be but not limited to 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, etc., or any range between the two. The particle size Dv99 of the porous carbon is 10 to 25 μm, for example, it can be but not limited to 10 μm, 12 μm, 15 μm, 18 μm, 20 μm, 22 μm, 25 μm, etc., or any range between the two. The particle size Dn10 of the porous carbon is 0.5 to 5 μm, for example, it can be but not limited to 0.5 μm, 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, etc., or any range between the two. The porous carbon of the present invention has a suitable particle size, which is more conducive to ensuring the electrical properties of the porous carbon.

[0040] In some embodiments, the specific surface area of ​​the porous carbon material is 1000-2200 m 2 / g, for example, but not limited to 1000m 2 / g、1200m 2 / g、1500m 2 / g、1700m 2 / g、1800m 2 / g, 2000m 2 / g, 2100m 2 / g or 2200m 2 / g, etc., or any range between the two. The porous carbon of the present invention has a suitable specific surface area, which is more conducive to ensuring its high conductivity and high capacity.

[0041] In some embodiments, the pore volume of the porous carbon material is 0.6 to 1.2 cm 3 / g, for example, but not limited to 0.6 cm3 / g, 0.7cm 3 / g, 0.8cm 3 / g, 0.9cm 3 / g, 1cm 3 / g or 1.2cm 3 / g, etc., or any range between the two. The porous carbon of the present invention has a suitable pore volume to ensure its mechanical strength and electrical properties, as well as the adsorption effect of the subsequent preparation of silicon-carbon negative electrode materials on silicon materials.

[0042] In some embodiments, the microporosity of the porous carbon material is 50% to 100%, for example, it can be but not limited to 50%, 60%, 70%, 80%, 85%, 90%, 95% or 100%, or any range between the two. The porous carbon of the present invention has a large number of micropores, which is more conducive to ensuring the mechanical strength, adsorption performance and electrical properties of the porous carbon.

[0043] In some embodiments, the porous carbon material includes at least one of biomass-derived carbon, resin-derived carbon, petroleum coke-derived carbon, coal-derived carbon, metal-modified carbon material, and metal oxide-modified carbon material.

[0044] In some embodiments, the porous carbon material can be selected from commercially available products, or prepared by methods known in the art, such as hydrothermal method, solvothermal method, electrochemical deposition method, powder metallurgy method, molten metal method, ion exchange method, activation method, etc.

[0045] In some specific embodiments of the present invention, the method for preparing the porous carbon material comprises the following steps: (1) Microwave carbonization of precursor The alcoholysis lignin is used as a precursor and subjected to microwave carbonization treatment in a humidified nitrogen atmosphere at a temperature of 400-900°C to obtain a carbonized material.

[0046] (2) Chemical activation The carbonized material obtained in step (1) is activated with potassium hydroxide (KOH) to obtain an activated material. The mass ratio of potassium hydroxide to the carbonized material is 1:1 to 3:1, the activation time is 0.5 to 4 hours, and the activation temperature is 600 to 900°C.

[0047] (3) Placing the activated material obtained in the above step (2) in a reducing atmosphere, and sequentially performing a first heat treatment and a second heat treatment, wherein the temperature of the first heat treatment is 90-150°C, and the holding time of the first heat treatment is 20-40 min, and the temperature of the second heat treatment is 600-1000°C, and the holding time of the second heat treatment is 2-5 h, to obtain a porous carbon material.

[0048] In the specific embodiment of the present invention, the preparation method of the porous carbon material is described by taking the above-mentioned preparation method of the porous carbon material as an example, but it is not limited thereto, and other preparation methods of the porous carbon are all acceptable.

[0049] In the above step (1), the humidified nitrogen atmosphere can effectively improve the pore-forming efficiency, and microwave carbonization can form a large number of active centers. The temperature of the carbonization treatment includes but is not limited to 400°C, 500°C, 600°C, 700°C, 800°C or 900°C, or any range between the two.

[0050] In the above step (2), the mass ratio of alkali to carbonized material includes but is not limited to 1:1, 2:1 or 3:1. The activation treatment time may be, for example, but is not limited to 0.5 h, 1 h, 2 h, 3 h or 4 h, or any range between the two. The activation treatment temperature may be, for example, but is not limited to 600°C, 650°C, 700°C, 750°C, 800°C or 900°C, or any range between the two.

[0051] In the above step (3), the temperature of the first heat treatment may be, for example, but not limited to, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, etc., or any range between them; the holding time of the first heat treatment may be, for example, but not limited to, 20 min, 25 min, 30 min, 40 min, etc., or any range between them. The temperature of the second heat treatment may be, for example, but not limited to, 600°C, 700°C, 800°C, 900°C, 950°C, 1000°C, etc., or any range between them; the holding time of the second heat treatment may be, for example, but not limited to, 2h, 2.5h, 3h, 3.5h, 4h, 4.5h or 5h, etc., or any range between them. The reducing atmosphere includes hydrogen.

[0052] The number and type of oxygen-containing functional groups on the surface of porous carbon materials are controlled by activation treatment, and different activation processes will lead to different surface functional groups. The present invention uses microwave carbonization, alkaline activation, and then reductive atmosphere passivation treatment on porous carbon raw materials to reduce or remove unstable surface functional groups (acidic functional groups), leaving a suitable content of stable functional groups (neutral functional group phenolic hydroxyl and alkaline functional group carbonyl), thereby ensuring the conductivity and wettability of porous carbon, and ensuring the cycle performance and rate performance of the silicon-carbon negative electrode material prepared therefrom.

[0053] According to another aspect of the present invention, the present invention also relates to a silicon-carbon negative electrode material, comprising the porous carbon material and nano-silicon particles located in the pores of the porous carbon material.

[0054] The silicon-carbon negative electrode material of the present invention has a porous carbon with an appropriate content of oxygen-containing surface functional groups. The rate capability of the silicon-carbon negative electrode material is significantly affected by the porous carbon, and the rate capability of the porous carbon depends on the influence of the oxygen-containing functional groups on the ion diffusion and conductivity of the carbon material. The total content of the surface functional groups is usually inversely proportional to the conductivity (the decrease in conductivity is due to the introduction of oxygen-containing functional groups, which increases defects, sp3 carbon and impedance). However, if the content of the surface functional groups of the porous carbon is too low, its wettability will be poor. In addition, the oxygen-containing functional groups on the surface of the porous carbon can increase the adsorption sites. The concentration and distribution of the surface functional groups have a significant effect on the adsorption properties of the carbon material. The carbon material with more oxygen has a stronger adsorption force for adsorbing polar gases, especially polar silicon-containing gases. The alkaline sites in the porous carbon material have a better chemical adsorption effect on silicon-containing gases. The phenolic hydroxyl functional group is a highly hydrophilic group that can adsorb with silicon-containing gas molecules through hydrogen bond interactions and promote adsorption and diffusion. It usually increases the polarity of the porous carbon material surface, thereby enhancing the interaction with silicon-containing gas molecules to improve the silicon utilization rate of the silicon-containing gas. In summary, to coordinate the conductivity and wettability of silicon-carbon negative electrode materials, it is necessary to control the surface functional groups within an appropriate content range.

[0055] In some embodiments, the mass content of nano silicon particles in the silicon-carbon negative electrode material is 5% to 85%, for example, 5%, 10%, 15%, 20%, 25%, 25%, 30%, 40%, 50%, 60%, 70%, 80%, 85%, etc., or any range between the two. The present invention loads an appropriate amount of silicon in the porous carbon material, thereby improving the conductivity of the negative electrode material and increasing the capacity.

[0056] In some embodiments, the particle size Dv50 of the silicon-carbon negative electrode material is 3 to 10 μm, for example, it can be but not limited to 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 10 μm, etc., or any range between the two. The particle size Dv99 of the silicon-carbon negative electrode material is 10 to 25 μm, for example, it can be but not limited to 10 μm, 12 μm, 15 μm, 20 μm, 25 μm, etc., or any range between the two. The particle size Dn10 of the silicon-carbon negative electrode material is 0.5 to 5 μm, for example, 0.5 μm, 1 μm, 2 μm, 3 μm, 4 μm or 5 μm, etc., or any range between the two. The silicon-carbon negative electrode material of the present invention has a suitable particle size, and small particles of material can be filled in large particles, which helps to increase the compaction density of the pole piece, improve the volume energy density of the battery, and help improve the charge and discharge performance and cycle performance.

[0057] In some embodiments, the specific surface area of ​​the silicon-carbon negative electrode material is less than 3m 2 / g, for example, but not limited to 0.5m 2 / g, 1m2 / g, 1.5m 2 / g, 1.8m 2 / g, 2m 2 / g, 2.5m 2 / g or 2.8m 2 / g, etc., or any range between the two. The silicon-carbon negative electrode material of the present invention has a suitable specific surface area, which is beneficial to improving the electrical performance of the battery.

[0058] In some embodiments, the electrical conductivity of the silicon-carbon negative electrode material is 0.2-2S / mm, for example, it can be but not limited to 0.2S / mm, 0.5S / mm, 0.8S / mm, 1S / mm, 1.5S / mm, 2S / mm, etc., or any range value therebetween. The silicon-carbon negative electrode material of the present invention has a higher electrical conductivity through the combination of porous carbon and silicon material, which is more conducive to improving the electrical performance of the battery.

[0059] In some embodiments, the surface of the silicon-carbon negative electrode material further includes a coating layer. The coating layer contains at least one of amorphous carbon, a fast ion conductor (such as LiF, etc.) and a high molecular polymer. The present invention further coats the surface of the silicon-carbon negative electrode material with the above coating layer to further improve the electrical properties of the silicon-carbon negative electrode material.

[0060] According to another aspect of the present invention, the present invention relates to a method for preparing a silicon-carbon negative electrode material, comprising the following steps: The porous carbon material is vapor deposited in an atmosphere containing a silicon source to obtain the silicon-carbon negative electrode material.

[0061] The preparation method of the silicon-carbon negative electrode material of the present invention adopts the above-mentioned specific porous carbon material, thereby ensuring the adsorption performance of the porous carbon to silicon source gas molecules, improving the silicon utilization rate, and improving the conductivity, wettability, and stability of the final silicon-carbon negative electrode material, thereby improving the capacity and cycle performance.

[0062] In some embodiments, the silicon source comprises a conventional siliconizing gas. The silicon source includes but is not limited to monosilane (SiH 4 ), at least one of disilane, trisilane, halogenated silane, polysilane, silole and its derivatives, silane and its derivatives. In some embodiments, the temperature of vapor deposition is 400~550℃, for example, it can be but not limited to 400℃, 450℃, 480℃, 500℃, 510℃, 550℃, etc., or any range between the two. The holding time of vapor deposition is 3~5h, for example, it can be but not limited to 3h, 3.5h, 4h, 4.5h or 5h, etc., or any range between the two. The heating rate is 2~6℃ / min, for example, 2℃ / min, 5℃ / min, 6℃ / min, etc. The flow rate of silicon source gas is 0.2~0.6L / min, for example, 0.2L / min, 0.3L / min, 0.4L / min, 0.5L / min or 0.6L / min, etc., or any range between the two. The atmosphere of vapor deposition is a protective gas condition, such as nitrogen, helium, etc. The present invention adopts suitable vapor deposition conditions to ensure that the silicon source gas is better deposited in the pores of the porous carbon, so as to obtain a silicon-carbon negative electrode material with high conductivity, high capacity and high cycle performance.

[0063] In some embodiments, the method further includes: coating the silicon-carbon negative electrode material to obtain a coating layer on the surface of the silicon-carbon negative electrode material, wherein the coating layer comprises at least one of amorphous carbon, a fast ion conductor and a high molecular polymer. The coating treatment specifically includes: performing a third heat treatment after vapor deposition while continuously introducing a coating source gas. The present invention further coats the surface of the silicon-carbon negative electrode material to improve the comprehensive performance of the final silicon-carbon negative electrode material.

[0064] In some embodiments, the temperature of the third heat treatment is 650-750°C, for example, it can be but not limited to 650°C, 680°C, 700°C, 720°C, 730°C or 750°C, or any range between the two. The holding time of the third heat treatment is 2-4h, for example, it can be but not limited to 2h, 2.5h, 3h, 3.5h or 4h, or any range between the two. The coating source gas includes acetylene, methane, ethane, isopropane, propane, butane, isobutane, ethylene, butene, propylene, acetylene (C 2 H 2 ), vinyl chloride, ethyl chloride, vinyl fluoride, pentachlorofluoroethane, difluoroethane, 1,1-difluoroethylene, fluoromethane, chloromethane, difluoromethane, trifluoromethane or LiF, etc. The heating rate of the third heat treatment is 2~6°C / min, such as 2°C / min, 5°C / min, 6°C / min, etc. The third heat treatment is carried out under protective gas conditions. The present invention adopts suitable third heat treatment conditions to ensure the coating effect, which is conducive to further improving the conductivity of the silicon-carbon negative electrode material, increasing the capacity, and improving the cycle performance.

[0065] According to another aspect of the present invention, the present invention also relates to an electrode, comprising the silicon-carbon negative electrode material.

[0066] The electrode of the present invention comprises a current collector and a negative electrode material layer located on at least one side surface of the current collector, and the negative electrode material layer contains the above-mentioned silicon-carbon negative electrode material.

[0067] According to another aspect of the present invention, the present invention also relates to a lithium ion battery comprising the electrode.

[0068] The lithium ion battery of the present invention comprises the above-mentioned electrode, positive electrode, separator and electrolyte. The battery of the present invention has excellent cycle performance, rate performance and safety performance.

[0069] According to another aspect of the present invention, the present invention also relates to an electrical device, comprising the lithium-ion battery.

[0070] The lithium ion battery of the present invention is applied to electrical equipment to ensure power supply effect and improve safety.

[0071] The following is further explained in conjunction with specific embodiments and comparative examples.

[0072] Example 1 A method for preparing a silicon-carbon negative electrode material comprises the following steps: (a) 1 kg of porous carbon material was placed in a rotary furnace, and nitrogen was introduced for protection. The temperature was then raised to 450 °C at a rate of 5 °C / min. At the same time, monosilane was introduced at a flow rate of 0.5 L / min for 4 h, and the silicon source valve was closed.

[0073] The porous carbon has surface functional groups, which include alkaline functional groups and acidic functional groups. The alkaline functional groups include carbonyl and phenolic hydroxyl groups, and the acidic functional groups include hydroxyl and carboxyl groups. The carbonyl content is 0.4 mmol / g, the phenolic hydroxyl content is 0.2 mmol / g, and the carboxyl and hydroxyl contents are 0. The conductivity of the porous carbon is 3.41 S / mm, PH=7.86, the particle size Dv50 of the porous carbon is 6.6 μm, Dv99 is 16.2 μm, Dn10 is 3.3 μm, and the specific surface area is 1800 m 2 / g, pore volume is 0.82cm 3 / g.

[0074] (b) The temperature was then raised to 700° C. for a third heat treatment, and acetylene and argon were introduced for 3 hours to obtain a silicon-carbon negative electrode material with a silicon content of 48% by mass.

[0075] Example 2 A method for preparing a silicon-carbon negative electrode material comprises the following steps: (a) 1 kg of porous carbon material was placed in a rotary furnace, and nitrogen was introduced for protection. The temperature was then raised to 450 °C at a rate of 5 °C / min. At the same time, monosilane was introduced at a flow rate of 0.5 L / min for 4 h, and the silicon source valve was closed.

[0076] The porous carbon has surface functional groups, including alkaline functional groups and acidic functional groups. The alkaline functional groups include carbonyl and phenolic hydroxyl groups, and the acidic functional groups include hydroxyl and carboxyl groups. The carbonyl content is 0.5 mmol / g, the phenolic hydroxyl content is 0.2 mmol / g, and the carboxyl and hydroxyl contents are 0. The conductivity of the porous carbon is 3.34 S / mm, and the pH is 7.30. The particle size of the porous carbon is Dv50 of 8.5 μm, Dv99 of 14.5 μm, Dn10 of 3.5 μm, and the specific surface area is 2100 m 2 / g, pore volume is 0.88cm 3 / g.

[0077] (b) The temperature is then raised to 700° C. for a third heat treatment, and acetylene and argon are introduced for 3 hours to obtain a silicon-carbon negative electrode material with a silicon content of 50% by mass.

[0078] Example 3 A method for preparing a silicon-carbon negative electrode material, which differs from Example 1 in that: The carbonyl content of porous carbon is 0.5mmol / g, the phenolic hydroxyl content is 0.4mmol / g, and the carboxyl and hydroxyl content is 0.08mmol / g. The conductivity of porous carbon is 2.98S / mm, PH=7.81; the particle size of porous carbon is Dv50 is 10μm, Dv99 is 17.5μm, Dn10 is 2.8μm, and the specific surface area is 2090m 2 / g, pore volume is 0.95cm 3 / g.

[0079] The mass content of silicon in the obtained silicon-carbon negative electrode material is 51%.

[0080] Example 4 A method for preparing a silicon-carbon negative electrode material, which differs from Example 1 in that: The carbonyl content of porous carbon is 0.45%, the phenolic hydroxyl content is 0.3mmol / g, and the carboxyl and hydroxyl contents are 0.18mmol / g respectively. The conductivity of porous carbon is 2.91S / mm, PH=7.37; the particle size of porous carbon is Dv50 is 5.1μm, Dv99 is 10.2μm, Dn10 is 1.2μm, and the specific surface area is 1937m 2 / g, pore volume is 0.86cm 3 / g.

[0081] The mass content of silicon in the obtained silicon-carbon negative electrode material is 46.6%.

[0082] Example 5 A method for preparing a silicon-carbon negative electrode material comprises the following steps: (a) 1 kg of porous carbon material was placed in a rotary kiln, and then nitrogen was introduced for protection, and then the temperature was raised to 550°C at a rate of 6°C / min, and monosilane was introduced at a flow rate of 0.6 L / min for 3 hours, and the silicon source valve was closed. The porous carbon was the same as in Example 1.

[0083] (b) The temperature was then raised to 750° C. for a third heat treatment, and acetylene and argon were introduced for 2 h to obtain a silicon-carbon negative electrode material with a silicon content of 47% by mass.

[0084] Example 6 A method for preparing a silicon-carbon negative electrode material comprises the following steps: (a) 1 kg of porous carbon material was placed in a rotary kiln, and then nitrogen was introduced for protection, and then the temperature was raised to 400°C at a rate of 4°C / min, and monosilane was introduced at a flow rate of 0.6 L / min for 4 hours, and the silicon source valve was closed. The porous carbon was the same as in Example 1.

[0085] (b) The temperature was then raised to 650° C. for a third heat treatment, and acetylene and argon were introduced for 4 hours to obtain a silicon-carbon negative electrode material with a silicon content of 48% by mass.

[0086] Comparative Example 1 A method for preparing a silicon-carbon negative electrode material, which differs from Example 1 in that: The surface functional groups of porous carbon include carbonyl content of 1.2mmol / g, phenolic hydroxyl content of 0.6mmol / g, carboxyl and hydroxyl content of 0.5mmol / g respectively. The conductivity of porous carbon is 0.02S / mm, PH=8.94; the particle size of porous carbon is Dv50 of 8.2μm, Dv99 of 15.5μm, Dn10 of 3.0μm, and specific surface area of ​​1900m 2 / g, pore volume is 0.73cm 3 / g.

[0087] Comparative Example 2 A method for preparing a silicon-carbon negative electrode material, which differs from Example 1 in that: Among the surface functional groups of porous carbon, carbonyl accounts for 0.1mmol / g, phenolic hydroxyl accounts for 0.1mmol / g, and carboxyl and hydroxyl accounts for 0. The conductivity of porous carbon is 1.13S / mm, PH=7.51; the particle size of porous carbon is Dv50 is 8.8μm, Dv99 is 18.5μm, Dn10 is 3.6μm, and the specific surface area is 2020m 2 / g, pore volume is 0.83cm 3 / g.

[0088] Experimental example 1. Performance test of silicon-carbon negative electrode materials The conductivity, pH and silane utilization rate of the silicon-carbon negative electrode materials obtained in the examples and comparative examples were tested, and the test results are shown in Table 1.

[0089] Test method for surface functional groups: According to the national standard GBT-38114-2019, the Boehm acid-base titration method was used for determination.

[0090] The principle is that NaHCO 3 , Na 2 CO 3 , NaOH and CH 3 CH 2 In the aqueous solutions of four alkalis with increasing alkalinity strength, NaHCO 3 It can only neutralize the relatively acidic functional groups (type I functional groups) on the surface of activated carbon, such as carboxyl groups; Na 2 CO 3 The acidic functional groups on the surface of activated carbon that can be neutralized include carboxyl and hydroxyl groups in the form of lactone (I+II functional groups); the acidic functional groups on the surface of activated carbon that can be neutralized by NaOH include carboxyl, hydroxyl groups in the form of lactone and phenolic hydroxyl groups (I+II+III functional groups); 3 CH 2 ONa has the strongest alkalinity and can neutralize most of the acidic functional groups (type I+II+III+IV functional groups) on the surface of activated carbon. 3 CH 2 The content of type IV functional groups can be calculated by subtracting the consumption of ONa for neutralization of acidic surface functional groups from the consumption of NaOH for neutralization. The content of type III, II, and I functional groups can be calculated by analogy. The unit is mmol / g.

[0091] Conductivity test method: Use a resistivity tester (Ningbo Ruike FT-301B automatic conductor powder resistivity tester), take the negative electrode, use an electronic press to press it to 5000kg±2kg, maintain it for 15s to 25s, place the sample between the electrodes of the tester, sample height h (cm), voltage U at both ends, current I, resistance R (KΩ) The area after powder pressing is S=3.14cm 2 The electronic conductivity of the powder is calculated according to the formula δ = h / (S×R) / 1000, and the unit is S / mm.

[0092] Testing method for silane utilization: Silane utilization (%) = [received material (g) × silicon content (%)] / [volume of silane introduced (L) × silane density (g / L)].

[0093] Test method for silicon content: The silicon content is measured by calcining at 1000℃ in air for 1 hour using a thermogravimetric analyzer to completely oxidize the carbon and make it lose weight, and to completely convert the silicon into silicon dioxide. The weight of the added oxygen is then used to calculate the silicon content in the silicon-carbon material. The details are as follows: (1) Weigh about 2 g of silicon-carbon material and record the actual mass as m0; place it in a crucible with a mass of m1.

[0094] (2) Place the crucible in a tube furnace or muffle furnace, continuously pass compressed air, raise the temperature to 600°C at 10°C / min, hold for 1 h, then raise the temperature to 1000°C at the same rate and hold for 1 h.

[0095] (3) After cooling naturally to room temperature, take out the crucible and weigh its mass as m2.

[0096] (4) Calculation of Si content (%) = (m2-m0) × MSi / MSiO 2 / m1×100%; among which, MSiO 2 SiO 2 Relative molecular mass, 60.084 g / mol; MSi is the relative molecular mass of Si, 28.0855 g / mol.

[0097] Table 1 Test results of silicon-carbon negative electrode materials

[0098] As can be seen from Table 1, the present invention uses porous carbon with an appropriate content of functional groups to prepare silicon-carbon negative electrode materials, and the obtained silicon-carbon negative electrode materials have high electrical conductivity, appropriate pH, high silane utilization, and better electrical properties of the silicon-carbon negative electrode materials.

[0099] In the porous carbon of Comparative Example 1, the contents of carbonyl, phenolic hydroxyl, hydroxyl and carboxyl are all too high, that is, the total content of the surface functional groups of the porous carbon is too high, the conductivity of the obtained silicon-carbon negative electrode material is low, the pH is too high, and the silane utilization rate is low. In the porous carbon of Comparative Example 2, the contents of carbonyl and phenolic hydroxyl are all too low, that is, the total content of the surface functional groups of the porous carbon is too low, the conductivity of the obtained silicon-carbon negative electrode material is low, and the silane utilization rate is low.

[0100] 2. Battery electrical performance test The silicon-carbon negative electrode materials obtained in each embodiment and comparative example are respectively prepared into batteries, and the preparation method of the battery comprises: Silicon-carbon negative electrode material (negative electrode active material), polyacrylic acid resin (PAA), single carbon nanotube (CNT) and conductive carbon black (SP) were mixed in a mass ratio of 82:7:1:10, made into slurry with deionized water, evenly coated on copper foil, and vacuum dried at 80°C for 24h to obtain the battery electrode for the experiment; lithium sheet was used as the counter electrode; 1.1 mol / L LiPF 6 The electrolyte is a four-component mixed solvent, ethylene carbonate (EC): vinylene carbonate (VC): dimethyl carbonate (DMC): fluoroethylene carbonate (FEC) = 1:1:1:1 (mass ratio); a polypropylene microporous film is used as a separator; and a CR2025 button half-cell is assembled in a vacuum glove box.

[0101] The rate performance and cycle performance were tested using a battery testing system (Arbin multi-channel battery testing system from the United States for half-battery testing and Labstar (1200 / 780) glove box from Braun, Germany).

[0102] Rate performance test: Under room temperature conditions, cycle at a current of 0.1C for 5 weeks, then cycle at a current of 0.2C for 5 weeks, cycle at a current of 0.5C for 5 weeks, cycle at a current of 1C for 5 weeks, cycle at a current of 2C for 5 weeks, and finally cycle at a current of 0.1C for 5 weeks.

[0103] Cyclic performance test: Under normal temperature conditions, 1C constant current charge and discharge to 0.01V, then 0.05C constant current discharge to 0.005V, and finally 1C constant current charge to 1.5V to obtain the de-lithiation specific capacity. This cycle is repeated 300 times, and the capacity retention rate after 300 cycles is calculated. The 300-week capacity retention rate is the ratio of the de-lithiation specific capacity in the 300th week to the de-lithiation specific capacity in the first week.

[0104] The battery electrical performance test results are shown in Table 2.

[0105] Table 2 Battery electrical performance test results

[0106] As can be seen from Table 2, the present invention prepares silicon-carbon negative electrode materials by using porous carbon with suitable types and contents of functional groups, and further prepares batteries. The batteries have excellent cycle performance and rate performance, with a capacity retention rate of more than 90%, and a capacity retention rate of 80% with a cycle number of 50 weeks or more.

[0107] The surface functional group content of the porous carbon in Comparative Example 1 is too high, and the obtained negative electrode material will hinder ion diffusion, so that the cycle performance and rate performance of the obtained battery are reduced. The surface functional group content of the porous carbon in Comparative Example 2 is too low, the wettability of the material is poor, and the utilization rate of the silicon material is low, which reduces the cycle performance and rate performance of the battery.

[0108] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A porous carbon material, characterized in that: The porous carbon material has surface functional groups, and the surface functional groups include basic functional groups, neutral functional groups and acidic functional groups; The content of the surface functional groups is 0.4-1 mmol / g, wherein the content of the basic functional groups is 0.2-0.5 mmol / g, the content of the neutral functional groups is 0.2-0.4 mmol / g, and the content of the acidic functional groups is less than 0.2 mmol / g.

2. The porous carbon material according to claim 1, characterized in that The invention comprises at least one of the following features (1) to (2): (1) The content of the surface functional groups is 0.4-0.7 mmol / g, wherein the content of the basic functional groups is 0.2-0.5 mmol / g, the content of the neutral functional groups is 0.2-0.4 mmol / g, and the content of the acidic functional groups is less than 0.1 mmol / g; (2) The basic functional group comprises a carbonyl group, the neutral functional group comprises a phenolic hydroxyl group, and the acidic functional group comprises a hydroxyl group and / or a carboxyl group.

3. The porous carbon material according to any one of claims 1 to 2, characterized in that The invention comprises at least one of the following features (1) to (7): (1) The electrical conductivity of the porous carbon material is 2-5 S / mm; (2) The pH of the porous carbon material is 6.8 to 8; (3) The particle size Dv50 of the porous carbon material is 3-10 μm; (4) The particle size Dv99 of the porous carbon material is 10-25 μm, and the particle size Dn10 of the porous carbon material is 0.5-5 μm; (5) The specific surface area of ​​the porous carbon material is 1000~2200m 2 / g; (6) The pore volume of the porous carbon material is 0.6~1.2cm 3 / g; (7) The microporosity of the porous carbon material is 50% to 100%.

4. A silicon-carbon negative electrode material, characterized in that: The porous carbon material comprises the porous carbon material according to any one of claims 1 to 3 and nano silicon particles located in the pores of the porous carbon material.

5. The silicon-carbon negative electrode material according to claim 4, characterized in that: Contains at least one of the following features (1) to (5): (1) In the silicon-carbon negative electrode material, the mass content of nano silicon particles is 5% to 85%; (2) The particle size Dv50 of the silicon-carbon negative electrode material is 3-10 μm, the particle size Dv99 of the silicon-carbon negative electrode material is 10-25 μm, and the particle size Dn10 of the silicon-carbon negative electrode material is 0.5-5 μm; (3) The specific surface area of ​​the silicon-carbon negative electrode material is less than 3m 2 / g; (4) The electrical conductivity of the silicon-carbon negative electrode material is 0.2~2S / mm; (5) The surface of the silicon-carbon negative electrode material also includes a coating layer; the coating layer contains at least one of amorphous carbon, a fast ion conductor and a high molecular polymer.

6. The method for preparing the silicon-carbon negative electrode material according to claim 4 or 5, characterized in that: The following steps are involved: The porous carbon material is vapor deposited in an atmosphere containing a silicon source to obtain the silicon-carbon negative electrode material.

7. The method for preparing the silicon-carbon negative electrode material according to claim 6, characterized in that: Also includes: The silicon-carbon negative electrode material is subjected to coating treatment to obtain a coating layer on the surface of the silicon-carbon negative electrode material, wherein the coating layer contains at least one of amorphous carbon, a fast ion conductor and a high molecular polymer.

8. An electrode, characterized in that: Including the silicon-carbon negative electrode material as described in claim 4 or 5.

9. A lithium ion battery, characterized in that: Comprising the electrode according to claim 8.

10. An electrical device, characterized in that: Includes the lithium ion battery as claimed in claim 9.

Citation Information

Patent Citations

  • Carbon material for electric dual-layer capacitor, electric dual-layer capacitor, and carbon material manufacturing method

    CN101198545A

  • Low-alkali activated preparation method and application of pitch-based activated carbon

    CN105174260A

  • Chemical activated porous carbon pore depth regulation and control method based on mechanical ball milling and tight energy storage application

    CN114275783A

  • Preparation of oxygen-doped modified three-dimensional porous carbon and application of oxygen-doped modified three-dimensional porous carbon in advanced treatment of phenolic organic wastewater

    CN116281944A

  • Fluidized bed system and method for simultaneous preparation of porous carbon and silicon carbon negative electrode material

    CN117691063A

Cited By

  • Preparation method of composite silicon-carbon negative electrode material

    CN121849968A

  • Porous carbon material, silicon-carbon negative electrode material and preparation method therefor and use thereof

    WO2026067787A1