Preparation method and application of macroporous spinel type high-entropy oxide oxygen evolution reaction catalyst

Large pore spinel-type high entropy oxides were prepared by sol-gel accompanying phase separation method, which solved the problem of low oxygen evolution reaction efficiency in hydrogen production in water electrolysis, and achieved low cost and efficient catalyst preparation and excellent catalysis Active, suitable for industrial applications.

CN118877948APending Publication Date: 2024-11-01ZHEJIANG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410733006.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-07
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

In the prior art, the anode oxygen evolution reaction of hydrogen produced by electrolyzing water is inefficient due to its complex four-electron transfer mechanism and high reaction barrier. The existing high entropy oxide catalyst preparation method has high equipment cost and energy consumption. The problems of large, low purity, low safety risks and low catalytic activity are difficult to meet industrial needs.

Method used

The macroporous spinel-type high entropy oxide was prepared by sol-gel accompanying phase separation method. By controlling the ratio of metal salts and phase separation inducers, a three-dimensional and continuous macropore structure was formed, and Fe, Ni, Co, Mn, The high entropy oxide composed of Zn element combines the ring opening reaction of propylene oxide to promote sol-gel transformation, and a catalyst with excellent catalytic activity is prepared.

Benefits of technology

It realizes a low-cost, safe and reliable high-efficiency preparation process. The material has a good three-dimensional co-continuous large pore structure and excellent catalytic activity of electrocatalytic oxygen evolution reaction, which is suitable for large-scale industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118877948A_ABST
    Figure CN118877948A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of functional materials, and particularly relates to a macroporous spinel type high-entropy oxide oxygen evolution reaction catalyst and a preparation method thereof. The invention provides a macroporous spinel type high-entropy oxide oxygen evolution reaction catalyst. Metal is composed of a Fe source, a Ni source, a Co source, a Mn source and a Zn source. The macroporous spinel type high-entropy oxide material is prepared by using a sol-gel accompanying phase separation method, the raw materials are cheap and easy to obtain, the preparation process is simple and stable, the repeatability is high, and the method has an extremely high application prospect in industrial large-scale preparation of the macroporous spinel type high-entropy oxide. The spinel type high-entropy oxide with a good three-dimensional co-continuous macroporous structure can be prepared by controlling the dosage of the precursor, the deionized water, the glycerol, the polyacrylic acid and the epoxypropane, and the spinel type high-entropy oxide shows excellent catalytic activity in an electrocatalytic oxygen evolution reaction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of functional materials, and in particular relates to a macroporous spinel-type high-entropy oxide oxygen evolution reaction catalyst and a preparation method thereof. Background Art

[0002] In today's world, serious environmental problems such as rapid population growth, global warming and depletion of fossil fuels are becoming increasingly severe. In order to solve these problems, scientists have turned their attention to new energy sources such as solar energy, wind energy, nuclear energy, geothermal energy and hydrogen energy. Among them, hydrogen energy, as a clean and efficient energy carrier, is widely regarded as a potential solution for future energy security and sustainable development. Hydrogen production by water electrolysis has become an important research direction for hydrogen production due to its advantages of low raw material prices and low carbon emissions. However, its anode oxygen evolution reaction has a high reaction barrier due to its complex four-electron transfer mechanism, involving the adsorption and desorption of a large number of intermediates, which greatly limits the efficiency of water electrolysis. Therefore, finding a suitable catalyst to reduce its reaction barrier is an urgent problem to be solved in today's society.

[0003] High entropy oxides refer to oxide materials in which five or more metal elements are randomly distributed in a single-phase lattice in equimolar or nearly equimolar proportions. They have high entropy effect, lattice distortion effect, slow diffusion effect and "cocktail" effect. At present, the main methods for synthesizing high entropy oxides are solid phase method, mechanical alloying method, hydrothermal method, coprecipitation method, etc. Spinel-type high entropy oxides refer to a type of high entropy oxide with a spinel crystal structure. They have high stability and excellent catalytic performance, and have been gradually applied in the field of catalysis in recent years.

[0004] Chinese patent CN201911302087.7 ​​proposes a high entropy oxide type electrocatalytic anode oxygen evolution catalyst material and its preparation method, using a certain proportion of MnO, CoO, NiO, Fe3O4 powder in a ball mill for alloying and ball milling to obtain a high entropy oxide (Co2O3) with a spinel structure. 0.25 Mn 0.25 Ni 0.25 Fe 0.25 )Fe2O4, but its equipment cost is high, energy consumption is large, and purity is low, which cannot meet the needs of large-scale industrial production.

[0005] Chinese patent CN202211418410.9 proposes a method for preparing alginate-based high-entropy metal oxides and their applications. Sodium alginate is used as a raw material to chelate transition metal ions. A hydrothermal reaction and tubular furnace carbonization method are used to prepare alginate-based high-entropy metal oxide electrocatalysts under low temperature conditions. However, it involves the use of a high-pressure reactor, which has certain safety risks.

[0006] Chinese patent CN202110241056.6 proposes a high-entropy perovskite hollow nanotube efficient oxygen evolution reaction catalytic material and its preparation method, which uses lanthanum salt, strontium salt, iron salt, cobalt salt, nickel salt and nanofiber precursor dispersed in an organic solvent to prepare a spinning solution, and then electrospinning is used to prepare a nanofiber membrane. After calcination, high-entropy perovskite hollow nanotubes are prepared, but its catalytic activity in oxygen evolution reaction is low and needs to be further improved.

[0007] Chinese patent CN116949487A adopts an ultrathin nanosheet induction method to prepare a three-dimensional high specific surface area high entropy metal oxide oxygen evolution catalyst, which contains elements such as Me, Co, Ni, Fe, Mn, etc., and Me is Cu, Cr or Zn. However, its preparation process is cumbersome and the catalytic activity of the oxygen evolution reaction is low. Summary of the invention

[0008] The problem to be solved by the present invention is to provide a macroporous spinel-type high entropy oxide oxygen evolution reaction catalyst material and a preparation method thereof, which has excellent catalytic activity for oxygen evolution reaction.

[0009] In order to solve the above technical problems, the present invention provides a macroporous spinel high entropy oxide oxygen evolution reaction catalyst, wherein the metal is composed of Fe source, Ni source, Co source, Mn source and Zn source (i.e., the total molar ratio is 100%);

[0010] The molar proportion of the Fe source in the metal is 15% to 25%, the molar proportion of the Ni source is 15% to 25%, the molar proportion of the Co source is 15% to 25%, the molar proportion of the Mn source is 15% to 25%, and the rest is the Zn source.

[0011] Description: It has a three-dimensional co-continuous macroporous structure, and the crystal structure is a single-phase spinel structure.

[0012] As an improvement of the macroporous spinel high entropy oxide oxygen evolution reaction catalyst of the present invention: the molar ratio of Fe source, Ni source, Co source, Mn source and Zn source is 20%.

[0013] The present invention also provides a method for preparing the above-mentioned macroporous spinel-type high entropy oxide oxygen evolution reaction catalyst, comprising the following steps:

[0014] Step 1: 0.1-3.6 mL of deionized water, 0.1-3.6 mL of glycerol and 1.5-4.5 g of polyacrylic acid aqueous solution are mixed, and after stirring and mixing evenly, a solution A is obtained;

[0015] Step 2: Add ferric chloride, nickel chloride, cobalt chloride, manganese chloride and zinc chloride to solution A, and mix them vigorously to obtain solution B;

[0016] The dosage of the ferric chloride is 300-450 mg;

[0017] Step 3: Slowly add 1-4 mL of propylene oxide to solution B under vigorous stirring (addition time is 4-6 min), and then ultrasonically degas (violently stir for 1-2 min and then ultrasonically degas for 30-90 s), then transfer to an oven at a temperature of 40-80 ° C and age for 12-72 h in a sealed state, and then dry at 40-80 ° C for 48±4 hours to obtain a dry gel (product C);

[0018] As a preferred method, starting from 12 hours of aging, ethanol is used to replace the solvent every 12 hours;

[0019] Step 4: calcine the dry gel (product C) obtained in step 3 at 450-950° C. for 1-4 h, and then cool to room temperature to obtain a macroporous spinel high entropy oxide oxygen evolution reaction catalyst.

[0020] As an improvement of the preparation method of the macroporous spinel high entropy oxide oxygen evolution reaction catalyst of the present invention, the step 2 is: adding 300-450 mg of ferric chloride, 350-550 mg of nickel chloride, 350-550 mg of cobalt chloride, 300-450 mg of manganese chloride, and 200-300 mg of zinc chloride to solution A.

[0021] As a further improvement of the preparation method of the macroporous spinel high entropy oxide oxygen evolution reaction catalyst of the present invention, in step 1: the concentration of the polyacrylic acid aqueous solution is (35±3) wt%, and the average molecular weight of the polyacrylic acid is 100,000.

[0022] As a further improvement to the preparation method of the macroporous spinel high entropy oxide oxygen evolution reaction catalyst of the present invention: the gas used for calcination in step 4 is any one of air and oxygen.

[0023] As a further improvement to the method for preparing the macroporous spinel high entropy oxide oxygen evolution reaction catalyst of the present invention: the heating rate in the step 4 is 2 to 10°C / min.

[0024] As a further improvement of the preparation method of the macroporous spinel high entropy oxide oxygen evolution reaction catalyst of the present invention:

[0025] The stirring speed is 700±50r / min;

[0026] The speed of vigorous stirring is 1100±100r / min.

[0027] As a further improvement of the preparation method of the macroporous spinel high entropy oxide oxygen evolution reaction catalyst of the present invention:

[0028] In the step 1, the amount of the polyacrylic acid aqueous solution is 4.3±0.2 g; the total amount of deionized water and glycerol is 3±1 mL, and the volume ratio of deionized water to glycerol is 1.4:(0.4±0.1);

[0029] In the step 2: the molar ratio of ferric chloride, nickel chloride, cobalt chloride, manganese chloride and zinc chloride is 1:1:1:1:1;

[0030] In the step 3: the amount of propylene oxide is 2.3±0.2 mL, the aging temperature is 60±5° C., and the aging time is 48±2 h;

[0031] In the step 4: the calcination temperature is 750±20°C, the calcination time is 2±0.1h, and the heating rate is 5±0.5°C / min.

[0032] In the present invention, step 1 and step 2 are both completed at room temperature;

[0033] The present invention also provides a macroporous spinel high entropy oxide prepared by any of the above methods and its use - an electrocatalytic oxygen evolution reaction catalyst.

[0034] The present invention is a method for preparing macroporous spinel high entropy oxide based on a sol-gel accompanying phase separation system; in the present invention:

[0035] Step 1: a mixed solution of deionized water and glycerol is used as a solvent, and polyacrylic acid is used as a phase separation inducer to induce phase separation in the system;

[0036] Step 2: iron chloride, nickel chloride, cobalt chloride, manganese chloride and zinc chloride are reaction precursors for generating macroporous spinel high entropy oxide;

[0037] In step three, propylene oxide is used as a gel accelerator, which increases the pH of the system through a ring-opening reaction, thereby completing the sol-gel transition.

[0038] The present invention uses a sol-gel phase separation method to prepare a macroporous spinel high entropy oxide material. The raw materials are cheap and readily available, the preparation process is simple and stable, and the repeatability is high. It has a very high application prospect for industrial large-scale preparation of macroporous spinel high entropy oxides. By controlling the amount of precursor, deionized water, glycerol, polyacrylic acid and propylene oxide, a spinel high entropy oxide with a good three-dimensional co-continuous macroporous structure can be prepared, and it exhibits excellent catalytic activity in the electrocatalytic oxygen evolution reaction.

[0039] The present invention organically combines a porous material (three-dimensional co-continuous macroporous structure) with a high entropy oxide material (spinel high entropy oxide synthesized from five elements, namely, iron, cobalt, nickel, manganese and zinc) through a sol-gel phase separation method, which has the advantages of rich active sites of high entropy oxide and the ability of the porous material to fully contact with the electrolyte, thereby greatly enhancing the catalytic activity of the material in the electrocatalytic oxygen evolution reaction.

[0040] In summary, the present invention uses inexpensive and easily available metal salts as raw materials and adopts the sol-gel phase separation method to prepare a spinel-type high-entropy oxide with a three-dimensional co-continuous macroporous structure. The preparation process is safe and reliable, with low energy consumption and a simple flow. It has extremely high application prospects for the large-scale industrial preparation of macroporous spinel-type high-entropy oxides, and the material has excellent catalytic activity in oxygen evolution reaction. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] The specific implementation modes of the present invention are further described in detail below with reference to the accompanying drawings.

[0042] Figure 1 is a SEM photograph of the xerogel (product C) prepared in Example 1;

[0043] Figure 2 is a SEM photograph of the macroporous spinel high entropy oxide prepared in Example 1;

[0044] Figure 3 is a SEM photograph of the macroporous spinel high entropy oxide prepared in Example 2;

[0045] Figure 4 is a SEM photograph of the macroporous spinel high entropy oxide prepared in Example 3;

[0046] Figure 5 is a SEM photograph of the macroporous spinel high entropy oxide prepared in Example 4;

[0047] Figure 6 It is a linear voltammetric scanning test result diagram of the electrocatalytic electrode prepared from the samples of the embodiment and the comparative example;

[0048] Figure 7 is a SEM photograph of the xerogel (product C) prepared in Comparative Example 3-1;

[0049] Figure 8 is a SEM photograph of the xerogel (product C) prepared in Comparative Example 3-2;

[0050] Fig. 9 This is a SEM photograph of the dry gel (product C) prepared in Comparative Example 4-1. DETAILED DESCRIPTION

[0051] The present invention is further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto:

[0052] The stirring speed is 700±50r / min;

[0053] The vigorous stirring speed is 1100±100r / min.

[0054] Example 1: A method for preparing a macroporous spinel high entropy oxide material using ferric chloride, nickel chloride, cobalt chloride, manganese chloride, and zinc chloride as reaction precursors, a polyacrylic acid aqueous solution with a mass fraction of 35wt% and a molecular weight of 100,000 as a phase separation inducer, and propylene oxide as a gel accelerator, comprising the following steps in sequence:

[0055] Step 1: At room temperature, add 2.8 mL of deionized water, 0.8 mL of glycerol and 4.5 g of polyacrylic acid aqueous solution into a glass bottle, stir and mix evenly to obtain solution A.

[0056] Step 2: At room temperature, weigh 398 mg (0.002 mol) of ferric chloride, 475 mg (0.002 mol) of nickel chloride, 475 mg (0.002 mol) of cobalt chloride, 396 mg (0.002 mol) of manganese chloride, and 273 mg (0.002 mol) of zinc chloride, add them to solution A, stir vigorously and mix well to obtain solution B.

[0057] Step 3: At room temperature, add 2.4 mL of propylene oxide slowly (addition time is 5 minutes) to solution B with a syringe under vigorous stirring. After the addition is completed, stir vigorously for 1 minute and then ultrasonically degas for 60 seconds. Then transfer to a 60°C oven and age for 48 hours in a sealed state. Starting from 12 hours of aging, use ethanol to replace the solvent once every 12 hours, for a total of 3 times. Then dry at 60°C for 48 hours to obtain a dry gel (product C).

[0058] Note: The first anhydrous ethanol replacement refers to opening the container and adding anhydrous ethanol until the entire container is filled; the subsequent anhydrous ethanol replacement refers to opening the container, pouring out the original anhydrous ethanol, replacing it with new anhydrous ethanol, and resealing the container.

[0059] Step 4: calcine the dry gel (product C) obtained in step 3 at 750°C in air for 2h with a heating rate of 5°C / min. After cooling to room temperature, a macroporous spinel-type high entropy oxide oxygen evolution reaction catalyst is obtained.

[0060] The SEM image of the obtained dry gel (product C) is as follows: Figure 1 , with a smooth and uniform three-dimensional co-continuous macroporous structure; the SEM photos of macroporous spinel high entropy oxide materials are shown in Figure 2 The prepared macroporous spinel high-entropy oxide material is black and has a uniform three-dimensional co-continuous macroporous structure.

[0061] Experiment 1: Preparation of electrocatalytic electrodes

[0062] The nickel foam with a thickness of 0.5 mm was trimmed into a lower half square with an area of ​​1 × 1 cm 2 The convex shape was then immersed in a 1 mol / L hydrochloric acid solution and ultrasonically treated for 30 min. After being repeatedly cleaned with water and ethanol (until the eluent after washing with water is neutral), it was placed in a vacuum oven at 80°C and dried for 1 h and sealed for storage as a carrier for subsequent electrocatalytic materials.

[0063] The macroporous spinel high entropy oxide material obtained in Example 1 was crushed to pass through a 200-mesh sieve as a catalyst material, and then the catalyst material, carbon black and PVDF were dispersed in a certain volume of N-methylpyrrolidone in a mass ratio of 7:2:1, and ultrasonically treated for 1.5 hours to obtain a uniform catalyst solution; the mass concentration of the catalyst material in the catalyst solution was 10 mg / mL.

[0064] 200 μL of the catalyst solution was evenly applied to the 1×1 cm area below the convex nickel foam in 4 drops. 2 area and dried in a vacuum oven at 110 °C for 12 h to obtain an electrocatalytic working electrode, named FNCMZ-2.

[0065] The experiment was carried out according to the following electrochemical test method: at room temperature, a linear voltammetric scan (LSV) was performed in a three-electrode system using an electrochemical workstation (Shanghai Chenhua CHI660E), the electrolyte was 1 M KOH solution, the working electrode was the electrocatalytic working electrode prepared as above, the reference electrode was a mercury / mercury oxide electrode (Hg / HgO), and the counter electrode was a graphite electrode.

[0066] The electrocatalytic electrode exhibits excellent catalytic activity for oxygen evolution reaction, 100 mA / cm 2 The overpotential at a current density of 333 mV.

[0067] Note: The overpotential of the catalytic electrode at a certain current density is the potential corresponding to a certain current density in the linear voltammetry scan result minus the theoretical decomposition potential of the reaction (1.23V). The smaller the overpotential, the smaller the voltage value required to achieve the current density in actual production, that is, the stronger the catalytic activity of the catalyst.

[0068] Example 2: The amount of deionized water in Example 1 is changed to 3.4 mL, the amount of glycerol is changed to 0.2 mL, and the rest is the same as Example 1.

[0069] SEM images of macroporous spinel high entropy oxide materials are shown in Figure 2. Figure 3 , and also has a good three-dimensional co-continuous macroporous structure.

[0070] Perform the test according to the method described in Experiment 1 above:

[0071] The prepared electrocatalytic electrode was named FNCMZ-1, and its catalytic activity for oxygen evolution reaction was lower than that in Example 1, 100 mA / cm 2 The overpotential at a current density of 408 mV.

[0072] Example 3: The amount of deionized water in Example 1 is changed to 2.2 mL, the amount of glycerol is changed to 1.4 mL, and the rest is the same as Example 1.

[0073] SEM images of macroporous spinel high entropy oxide materials are shown in Figure 2. Figure 4 , and also has a good three-dimensional co-continuous macroporous structure.

[0074] Perform the test according to the method described in Experiment 1 above:

[0075] The prepared electrocatalytic electrode was named FNCMZ-3, and its catalytic activity for oxygen evolution reaction was lower than that in Example 1, 100 mA / cm 2 The overpotential at a current density of 385 mV.

[0076] Example 4: The amount of deionized water in Example 1 is changed to 1.6 mL, the amount of glycerol is changed to 2.0 mL, and the rest is the same as Example 1.

[0077] SEM images of macroporous spinel high entropy oxide materials are shown in Figure 2. Figure 5 , with a good three-dimensional co-continuous macroporous structure.

[0078] Perform the test according to the method described in Experiment 1 above:

[0079] The prepared electrocatalytic electrode was named FNCMZ-4, and its catalytic activity for oxygen evolution reaction was lower than that in Example 1, 100 mA / cm 2 The overpotential at a current density of 404 mV.

[0080] Comparative Example 1: An electrocatalytic electrode was prepared using ruthenium oxide (RuO2), a precious metal oxygen evolution reaction catalyst currently widely used in the commercial industry, according to the method described in Experiment 1.

[0081] Perform the test according to the method described in Experiment 1 above:

[0082] The obtained electrocatalytic electrode is named RuO2, and its catalytic activity for oxygen evolution reaction is lower than that in Example 1, 100 mA / cm 2 The overpotential at a current density of 391 mV.

[0083] In summary, the macroporous spinel high entropy oxide material prepared by the formula corresponding to Example 1 has a good three-dimensional co-continuous macroporous structure, and the electrocatalytic electrode prepared on this basis exhibits excellent catalytic activity in the oxygen evolution reaction.

[0084] Comparative Example 2: Compared with Example 1, ferric chloride, nickel chloride, cobalt chloride, manganese chloride and zinc chloride are replaced by:

[0085] 0.002 mol of ferric nitrate, 0.002 mol of nickel nitrate, 0.002 mol of cobalt nitrate, 0.002 mol of manganese nitrate, 0.002 mol of zinc nitrate; the rest is the same as in Example 1.

[0086] Finally, it was found that the reaction solution could not undergo sol-gel transition. This is because the principle of the method used in the present invention is to react the added propylene oxide (PO) with the Cl in the solution. - The ring-opening reaction occurs, consuming hydrogen ions in the solution, raising the pH of the solution, and thus completing the sol-gel transition. - , The affinity order of H2O is: If nitrate is used, PO will preferentially react with water in the solution to form 1,2-propylene glycol. This reaction cannot consume hydrogen ions in the solution and cannot increase the pH of the solution, so the sol-gel transition cannot occur.

[0087] Comparative Example 3-1: With respect to Example 1, "4.5 g polyacrylic acid aqueous solution" is changed to "5.5 g polyacrylic acid aqueous solution", and the rest is the same as Example 1.

[0088] The SEM image of the obtained dry gel (product C) is as follows: Figure 7 The morphology is clustered precipitation, and there is no three-dimensional co-continuous porous structure.

[0089] Description: Product C is the dry gel obtained before calcination. The three-dimensional co-continuous macroporous structure obtained in the present invention is inherited from its structure. Only when it has a three-dimensional co-continuous macroporous structure, the high entropy oxide obtained by calcination will present a three-dimensional co-continuous macroporous structure.

[0090] Comparative Example 3-2: Compared with Example 1, the amount of the polyacrylic acid aqueous solution was changed from "4.5 g" to "3.5 g", and the rest was the same as Example 1.

[0091] The SEM image of the obtained dry gel (product C) is as follows: Figure 8 The morphology is nanosheet spherical precipitation, and there is no three-dimensional co-continuous macroporous structure.

[0092] Comparative Example 4-1: Compared with Example 1, the amount of propylene oxide was changed from "2.4 mL" to "3.5 mL", and the rest was the same as Example 1.

[0093] The SEM image of the obtained dry gel (product C) is as follows: Fig. 9 The morphology is shown as isolated holes, and there is no three-dimensional continuous macroporous structure.

[0094] Comparative Example 4-2: Relative to Example 1, the amount of propylene oxide was changed from "2.4 mL" to "1 mL", and the rest was the same as Example 1.

[0095] Finally, it was found that the reaction solution could not undergo sol-gel transformation. This was because the principle of the method used in the present invention is that the added propylene oxide (PO) undergoes a ring-opening reaction with the chloride ions in the solution, consumes the hydrogen ions in the solution, and increases the pH of the solution, thereby completing the sol-gel transformation. If the amount of PO added is too small, the pH of the solution cannot be increased to the required level, and thus the sol-gel transformation cannot occur.

[0096] Finally, it should be noted that the above examples are only some specific embodiments of the present invention. Obviously, the present invention is not limited to the above embodiments, and there are many variations. All variations that can be directly derived or associated with the content disclosed by a person skilled in the art should be considered as the protection scope of the present invention.

Claims

1. A macroporous spinel high entropy oxide catalyst for oxygen evolution reaction, characterized in that: The metal consists of Fe source, Ni source, Co source, Mn source and Zn source; The molar proportion of the Fe source in the metal is 15% to 25%, the molar proportion of the Ni source is 15% to 25%, the molar proportion of the Co source is 15% to 25%, the molar proportion of the Mn source is 15% to 25%, and the rest is the Zn source.

2. The macroporous spinel high entropy oxide oxygen evolution reaction catalyst according to claim 1, characterized in that: The molar ratio of the Fe source, the Ni source, the Co source, the Mn source, and the Zn source is 20%.

3. The method for preparing a macroporous spinel high entropy oxide oxygen evolution reaction catalyst according to claim 1 or 2, characterized in that The following steps are involved: Step 1: Mix 0.1-3.6 mL of deionized water, 0.1-3.6 mL of glycerol and 1.5-4.5 g of polyacrylic acid aqueous solution, and stir to mix evenly to obtain solution A; Step 2: Add ferric chloride, nickel chloride, cobalt chloride, manganese chloride and zinc chloride to solution A, and mix them vigorously to obtain solution B; The dosage of the ferric chloride is 300-450 mg; Step 3: Slowly add 1-4 mL of propylene oxide to solution B under vigorous stirring, then ultrasonically degas, and then transfer to an oven at a temperature of 40-80° C. for aging for 12-72 hours; then dry at 40-80° C. for 48±4 hours to obtain a dry gel; Step 4: calcine the dry gel obtained in step 3 at 450-950° C. for 1-4 hours, and then cool to room temperature to obtain a macroporous spinel high entropy oxide oxygen evolution reaction catalyst.

4. The method for preparing the macroporous spinel high entropy oxide oxygen evolution reaction catalyst according to claim 3, characterized in that Step 2: Add 300-450 mg of ferric chloride, 350-550 mg of nickel chloride, 350-550 mg of cobalt chloride, 300-450 mg of manganese chloride, and 200-300 mg of zinc chloride into solution A.

5. The method for preparing the macroporous spinel high entropy oxide oxygen evolution reaction catalyst according to claim 3 or 4, characterized in that In the step 1, the concentration of the polyacrylic acid aqueous solution is (35±3) wt %, and the average molecular weight of the polyacrylic acid is 100,000.

6. The method for preparing the macroporous spinel high entropy oxide catalyst for oxygen evolution reaction according to any one of claims 3 to 5, characterized in that: During the aging process of step 3, solvent replacement is set, specifically: starting from 12 hours of aging, solvent replacement is performed using ethanol every 12 hours.

7. The method for preparing the macroporous spinel high entropy oxide oxygen evolution reaction catalyst according to claim 6, characterized in that: The gas used for calcination in step 4 is any one of air and oxygen.

8. The method for preparing the macroporous spinel high entropy oxide oxygen evolution reaction catalyst according to claim 7, characterized in that: The heating rate in step 4 is 2-10°C / min.

9. The method for preparing a macroporous spinel high entropy oxide catalyst for oxygen evolution reaction according to any one of claims 3 to 8, characterized in that: The stirring speed is 700±50r / min; The speed of vigorous stirring is 1100±100r / min.

10. The method for preparing a macroporous spinel high entropy oxide catalyst for oxygen evolution reaction according to claim 9, characterized in that: In the step 1, the amount of the polyacrylic acid aqueous solution is 4.3±0.2 g; the total amount of deionized water and glycerol is 3±1 mL, and the volume ratio of deionized water to glycerol is 1.4:(0.4±0.1); In the step 2: the molar ratio of ferric chloride, nickel chloride, cobalt chloride, manganese chloride and zinc chloride is 1:1:1:1:1; In the step 3: the amount of propylene oxide is 2.3±0.2 mL, the aging temperature is 60±5° C., and the aging time is 48±2 h; In the step 4: the calcination temperature is 750±20°C, the calcination time is 2±0.1h, and the heating rate is 5±0.5°C / min.