Polyaluminum chloride-based water purifying agent and preparation method thereof

By adding nano iron oxide, magnesium salt, modified starch, modified chitosan and activated kaolin to the polymer aluminum chloride water purifier, the formation of high-efficiency flocs and adsorbents, the poor sewage treatment effect in the prior art is solved. The problem of this method is to efficiently remove ammonia nitrogen, total phosphorus and heavy metal ions in sewage, reduce the treatment cost, and the water purifier is environmentally friendly, non-toxic, and easy to separate and regenerate.

CN118878033AActive Publication Date: 2024-11-01LIAONING BAIWEI TECH CO LTD

Patent Information

Application Number
CN202410922417.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-11-01
Estimated Expiration
2044-07-10

AI Technical Summary

Technical Problem

When the existing polyaluminum chloride water purifier treats industrial and urban sewage, high concentrations of ammonia nitrogen, total phosphorus and heavy metal ions lead to poor water purification results, and additional equipment is required, which increases the cost of sewage treatment.

Method used

Using a water purifier based on polymer aluminum chloride, nano iron oxide, magnesium salt, modified starch, modified chitosan and activated kaolin, the high-efficiency flocs and adsorbents are formed through ultrasonic dispersion and low-temperature plasma irradiation. Improve settlement effect and adsorption capacity.

Benefits of technology

The removal rate of high concentrations of ammonia nitrogen, total phosphorus and heavy metal ions in the sewage is significantly improved, the water purification effect is enhanced, and the wastewater treatment cost is reduced. The water purification agent is environmentally friendly, non-toxic, and easy to separate and regenerate.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of polyaluminum chloride water purifying agents, and particularly discloses a polyaluminum chloride-based water purifying agent and a preparation method thereof.The water purifying agent is prepared by mixing, stirring, ultrasonic dispersing, curing and drying a polyaluminum chloride-magnesium silicate composite solution, a modified starch-modified chitosan composite solution and magnetized active kaolin; wherein the polyaluminum chloride-magnesium silicate composite solution is prepared from aluminum chloride, magnesium chloride hexahydrate and trichloroethyl silane; the modified starch-modified chitosan composite solution is prepared by modifying starch with dimethyl diallyl ammonium chloride and acrylamide and modifying chitosan with diethyl triamine pentaacetic acid; the magnetized active kaolin is prepared from ferric chloride hexahydrate, sodium silicate and acidified kaolin. The water purifying agent disclosed by the invention contains various efficient flocculation and adsorption components, not only has the sweeping function of traditional polyaluminum chloride mesh cloth, but also can synchronously and efficiently remove pollutants such as ammonia nitrogen, total phosphorus, COD (Chemical Oxygen Demand) and suspended matters in water.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polyaluminium chloride water purifiers, in particular to a polyaluminium chloride-based water purifier and a preparation method thereof. Background Art

[0002] Polyaluminium chloride, referred to as PAC, is a water-soluble inorganic high molecular polymer between AlCl3 and Al(OH)3. It is usually a white, yellow, or brown resinous solid and can be used in drinking water, industrial water, and sewage treatment. Compared with traditional inorganic coagulants, the structure of polyaluminium chloride is composed of polycarboxyl complexes with various forms. It has the characteristics of fast flocculation and precipitation, wide applicable pH range, non-corrosive to pipeline equipment, and obvious water purification effect. However, with the development of science and technology, the types and contents of pollutants in industrial and urban sewage are gradually increasing. When ordinary polyaluminium oxide water purifiers are used for water purification, the presence of high concentrations of ammonia nitrogen, total phosphorus, and heavy metal ions in the sewage will lead to poor water purification effects. During flocculation and sedimentation, the decolorization rate of wastewater is low, and other disposal equipment is required, resulting in increased sewage treatment costs. Therefore, it is necessary to develop new and efficient water purifiers to solve this situation. Summary of the invention

[0003] The purpose of the present invention is to provide a water purifier based on polyaluminium chloride and a preparation method thereof. The water purifier is added with nano-iron oxide, magnesium salt, modified starch, modified chitosan and activated kaolin, which are high-efficiency water purification components, and can effectively remove high-concentration ammonia nitrogen, total phosphorus and heavy metal ions in sewage, decolorize the sewage, and the water purifier of the present invention has strong adsorption capacity and a wide range of application.

[0004] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0005] A method for preparing a water purifier based on polyaluminium chloride, the preparation method of the water purifier is specifically as follows:

[0006] The polyaluminium chloride-magnesium silicate composite solution, the modified starch-modified chitosan composite solution and the magnetically active kaolin are mixed, stirred evenly, ultrasonically dispersed, aged and dried to obtain a water purifier.

[0007] As a limitation of the present invention, the mass ratio of the polyaluminium chloride-magnesium silicate composite solution, the modified starch-modified chitosan composite solution and the magnetically activated kaolin is (24-26):(98-102):(6-8).

[0008] As a limitation of the present invention, during the ultrasonic dispersion treatment, the ultrasonic frequency is 34 to 60 kHz, the ultrasonic power is 600 to 1200 W, and the ultrasonic dispersion treatment time is 80 to 200 min.

[0009] As a limitation of the present invention, the preparation of the polyaluminium chloride-magnesium silicate composite solution is specifically as follows:

[0010] Aluminum chloride and deionized water are mixed and stirred in a mass ratio of 1:(20-24) to fully dissolve, and sodium hydroxide solution is slowly added at 30-40°C and 480-520rpm to react for 2-4h to obtain a polyaluminum chloride solution;

[0011] Mix magnesium chloride hexahydrate, trichloroethylsilane and deionized water in a mass ratio of 1:(1.5-2.5):(19-23), stir evenly, and irradiate with low-temperature plasma to obtain a magnesium chloride silicate solution;

[0012] The polyaluminium chloride solution and the magnesium aluminium silicate solution are mixed in a volume ratio of (4-6):1, reacted at 40-50°C and 50-60rpm for 20-40min, and allowed to stand for 2-6h to obtain a polyaluminium chloride-magnesium silicate composite solution.

[0013] As a limitation of the present invention, the preparation of the modified starch-modified chitosan composite solution is specifically:

[0014] Starch and deionized water are mixed at a mass ratio of 1:(42-48), stirred evenly, gelatinized at 80-90°C for 40-60min, cooled to room temperature to obtain a starch solution, dimethyldiallylammonium chloride, acrylamide, and starch solution are mixed at a mass ratio of 1:(0.6-1):(200-220), the pH is adjusted to 2 with dilute hydrochloric acid, reacted for 2-3h, and sodium hydroxide solution is added until the pH is neutral to obtain a modified starch solution;

[0015] Chitosan, acetic acid, glutaraldehyde, and deionized water are mixed in a mass ratio of (8-12):(5-6):(4-5):(490-510), and reacted at 30-50°C and 35-45rpm for 2-4h to obtain a cross-linked chitosan solution. Diethylenetriaminepentaacetic acid, N-(3-dimethylaminopropyl)-N'-ethylcarbodiimide hydrochloride, N-hydroxysuccinimide, a sodium hydroxide solution with a molar volume of 1 mol / L, and deionized water are mixed in a mass ratio of (9-11):(11-12). :(12~16):(12~16):(480~500) are mixed evenly, reacted at 30~50℃, 35~45rpm for 2~4h to obtain an activated group solution, the cross-linked chitosan solution and the activated group solution are mixed in a volume ratio of (1~3):1, reacted at 50~70℃ for 2~4h, added with tetrahydrofuran (1.2%~1.3% of the volume of the mixed solution) and a modified starch solution (the same volume as the mixed solution), and the reaction is continued for 1~3h to obtain a modified starch-modified chitosan composite solution.

[0016] As a limitation of the present invention, the preparation of magnetically activated kaolin is specifically as follows:

[0017] The ferric chloride hexahydrate and ethylene glycol are mixed uniformly at a mass ratio of 1:(44-45), stirred until the solution is clear, and the ferric chloride hexahydrate solution is obtained; polyethylene glycol and sodium acetate are mixed at a mass ratio of 1:(3-4), added to the ferric chloride hexahydrate solution, reacted at 180-220° C. and 20-40 rpm for 16-24 hours, cooled after the reaction is completed, washed with ethanol, and vacuum dried to obtain magnetic iron oxide nanoparticles;

[0018] The magnetic iron oxide nanoparticles, deionized water and sodium silicate are uniformly mixed in a mass ratio of (7-9):(120-130):(18-22), and the pH value of the mixed system is adjusted to 1 with a sulfuric acid solution and a sodium hydroxide solution. The mixture is reacted at 35-45° C. and 20-40 rpm for 2-3 hours. After the reaction is completed, the mixture is aged at 45-55° C. for 5-7 hours to obtain a magnetic iron oxide silicate solution.

[0019] The kaolin is calcined at 500-700°C for 3-5h, cooled to room temperature, and then 0.25-0.28 times the mass of kaolin and 40wt% sulfuric acid solution is added, and the mixture is reacted at 85-95°C for 3-5h. After the reaction, the filtrate is washed with deionized water until the pH value of the filtrate is neutral, and then 4-6 times the weight of kaolin and magnetic silicate iron oxide solution are added, and the mixture is dried at 70-90°C for 20-28h, crushed, sieved, and the magnetized active kaolin is separated with a magnet.

[0020] As a limitation of the present invention, the low-temperature plasma irradiation time is 40 to 80 minutes, the low-temperature plasma irradiation voltage is 4 to 6 kV, and the low-temperature plasma atmosphere is oxygen.

[0021] The beneficial effects achieved by the present invention are as follows: compared with common polyaluminium chloride water purifiers, the water purifier of the present invention is added with magnesium salt, modified starch, modified chitosan and magnetized activated kaolin. Magnesium salt can quickly form large and dense flocs when treating sewage, increase the sedimentation rate of fine particles, and improve the sedimentation effect. The modified starch and chitosan structures contain abundant active adsorption sites such as amino and hydroxyl groups, have strong adsorption capacity for anions, and are environmentally friendly, non-toxic and have good degradability. Magnetized activated kaolin has a unique layered structure, abundant surface siloxane groups and strong ion exchange capacity. The flocs formed when treating sewage have good dispersibility and chemical stability, and are easily separated from the solution by an external magnetic field. DETAILED DESCRIPTION

[0022] The following is a preferred implementation of the embodiment of the present invention. Obviously, the described embodiment is only a part of the embodiment of the present invention, not all of the embodiments. For ordinary technicians in this technical field, all other embodiments obtained by ordinary technicians in this field without creative work without departing from the principle of the embodiment of the present invention are within the scope of protection of the present invention.

[0023] Diethylenetriaminepentaacetic acid (D807203), 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride (N808856), N-hydroxysuccinimide (H6231), kaolin (K812211), sodium silicate (S871946), magnesium chloride hexahydrate (M813913) were provided by Shanghai MacLean; aluminum chloride (A433483), trichloroethylsilane (E156100), starch (S16 4486), dimethyldiallylammonium chloride (D110133), acrylamide (A108465), chitosan (C434551), acetic acid (A11616), glutaraldehyde (G359127), tetrahydrofuran (T103259), ferric chloride hexahydrate (F102742), ethylene glycol (E103318), polyethylene glycol (P432430), and sodium acetate (S299552) were provided by Shanghai Aladdin.

[0024] Example 1: A water purifier based on polyaluminium chloride, the preparation method is:

[0025] Step 1: Prepare polyaluminium chloride solution

[0026] Aluminum chloride and deionized water were mixed and stirred at a mass ratio of 1:22 to fully dissolve, and a 0.18 mol / L sodium hydroxide solution (3 times the weight of aluminum chloride) was slowly added at 35° C. and 500 rpm to react for 3 hours to obtain a polyaluminum chloride solution.

[0027] Step 2: Preparation of polyaluminium chloride-magnesium silicate composite solution

[0028] Mix magnesium chloride hexahydrate, trichloroethylsilane and deionized water in a mass ratio of 1:2:21, stir evenly, and irradiate with low-temperature plasma for 60 minutes to obtain a magnesium chloride silicate solution;

[0029] The polyaluminium chloride solution and the magnesium chloride silicate solution were mixed at a volume ratio of 5:1, reacted at 45°C and 55 rpm for 30 minutes, and allowed to stand and mature for 4 hours to obtain a polyaluminium chloride-magnesium silicate composite solution.

[0030] Step 3: Prepare modified starch solution

[0031] Starch and deionized water were mixed in a mass ratio of 1:45, stirred evenly, gelatinized at 85°C for 50 minutes, cooled to room temperature to obtain a starch solution, dimethyldiallylammonium chloride, acrylamide, and starch solution were mixed in a mass ratio of 1:0.8:210, the pH was adjusted to 2 with 0.1 mol / L dilute hydrochloric acid, reacted for 2.5 hours, and then 30 wt% sodium hydroxide solution was added until the pH was neutral to obtain a modified starch solution.

[0032] Step 4: Preparation of modified starch-modified chitosan composite solution

[0033] Chitosan, acetic acid, glutaraldehyde and deionized water were mixed in a mass ratio of 10:5.5:4.5:500, reacted at 40°C and 40rpm for 3h to obtain a cross-linked chitosan solution, diethylenetriaminepentaacetic acid, N-(3-dimethylaminopropyl)-N'-ethylcarbodiimide hydrochloride, N-hydroxysuccinimide, a sodium hydroxide solution with a molar volume of 1 mol / L and deionized water were mixed in a mass ratio of 10:11.5:14:14:490, reacted at 40°C and 40rpm for 3h to obtain an activated group solution, the cross-linked chitosan solution and the activated group solution were mixed in a volume ratio of 2:1, reacted at 60°C for 3h, tetrahydrofuran (1.25% of the volume of the mixed solution) and a modified starch solution (equal to the volume of the mixed solution) were added, and the reaction was continued for 2h to obtain a modified starch-modified chitosan composite solution.

[0034] Step 5: Preparation of magnetic iron oxide nanoparticles

[0035] Ferric chloride hexahydrate and ethylene glycol were mixed uniformly at a mass ratio of 1:44.5, and stirred until the solution was clear to obtain a ferric chloride hexahydrate solution. Polyethylene glycol and sodium acetate were mixed at a mass ratio of 1:3.5, added to the ferric chloride hexahydrate solution, and reacted at 200°C and 30rpm for 20h. After the reaction was completed, the mixture was cooled, washed with ethanol, and vacuum dried to obtain magnetic iron oxide nanoparticles.

[0036] Step 6: Preparation of Magnetized Activated Kaolin

[0037] The magnetic iron oxide nanoparticles, deionized water and sodium silicate were uniformly mixed in a mass ratio of 8:125:20, and the pH of the mixed system was adjusted to 1 with 30wt% sulfuric acid and 0.1mol / L sodium hydroxide solution, and the mixture was reacted at 40°C and 30rpm for 2.5h. After the reaction was completed, the mixture was aged at 50°C for 6h to obtain a magnetic silicate iron oxide solution;

[0038] The kaolin was calcined at 600°C for 4 hours, cooled to room temperature, and then a 40wt% sulfuric acid solution (0.26 times the weight of the kaolin) was added, and the mixture was reacted at 90°C for 4 hours. After the reaction, the filtrate was washed with deionized water until the pH value of the filtrate was neutral. A magnetic silicate iron oxide solution (5 times the weight of the kaolin) was added, and the mixture was dried at 80°C for 24 hours. The mixture was crushed, sieved, and the magnetized active kaolin was separated with a magnet.

[0039] Step 7: Prepare water purifier

[0040] The polyaluminium chloride-magnesium silicate composite solution, the modified starch-modified chitosan composite solution and the magnetized active kaolin were mixed in a mass ratio of 25:100:7, and magnetically stirred at 27°C and 300rpm for 25min. After the stirring, ultrasonic dispersion and mixing treatment was performed. After the ultrasonic dispersion treatment was completed, the mixture was aged at 75°C for 24h and freeze-dried to obtain a water purifier.

[0041] Example 2: A water purifier based on polyaluminium chloride, the preparation method is:

[0042] Step 1: Prepare polyaluminium chloride solution

[0043] Aluminum chloride and deionized water were mixed and stirred at a mass ratio of 1:24 to fully dissolve, and a 0.18 mol / L sodium hydroxide solution (3 times the weight of aluminum chloride) was slowly added at 35° C. and 500 rpm to react for 3 hours to obtain a polyaluminum chloride solution.

[0044] Step 2: Preparation of polyaluminium chloride-magnesium silicate composite solution

[0045] Mix magnesium chloride hexahydrate, trichloroethylsilane and deionized water in a mass ratio of 1:2.5:23, stir evenly, and irradiate with low-temperature plasma for 60 minutes to obtain a magnesium chloride silicate solution;

[0046] The polyaluminium chloride solution and the magnesium aluminium silicate solution were mixed in a volume ratio of 6:1, reacted at 45°C and 55 rpm for 30 minutes, and allowed to stand and mature for 4 hours to obtain a polyaluminium chloride-magnesium silicate composite solution.

[0047] Step 3: Prepare modified starch solution

[0048] Starch and deionized water were mixed in a mass ratio of 1:48, stirred evenly, gelatinized at 85°C for 50 minutes, cooled to room temperature to obtain a starch solution, dimethyldiallylammonium chloride, acrylamide, and starch solution were mixed in a mass ratio of 1:1:220, the pH was adjusted to 2 with 0.1 mol / L dilute hydrochloric acid, reacted for 2.5 hours, and then 30 wt% sodium hydroxide solution was added until the pH was neutral to obtain a modified starch solution.

[0049] Step 4: Preparation of modified starch-chitosan composite solution

[0050] Chitosan, acetic acid, glutaraldehyde and deionized water were mixed in a mass ratio of 12:6:5:510, and reacted at 40°C and 40 rpm for 3 h to obtain a cross-linked chitosan solution. N-(3-dimethylaminopropyl)-N'-ethylcarbodiimide hydrochloride, N-hydroxysuccinimide and deionized water were mixed in a mass ratio of (11-12):(12-16):(480-500), and diethylenetriamine (1-1.5 times the mass of N-hydroxysuccinimide) was added. Amine pentaacetic acid, at 30-50°C, 35-45rpm, slowly add sodium hydroxide solution of equal mass to N-hydroxysuccinimide, react for 2-4h to obtain an activated group solution, mix the cross-linked chitosan solution and the activated group solution in a volume ratio of 2:1, react at 60°C for 3h, add tetrahydrofuran (1.25% times the volume of the mixed solution) and a modified starch solution of equal volume to the mixed solution, continue to react for 2h to obtain a modified starch-modified chitosan composite solution.

[0051] Step 5: Preparation of magnetic iron oxide nanoparticles

[0052] Ferric chloride hexahydrate and ethylene glycol were mixed uniformly at a mass ratio of 1:45, and stirred until the solution was clear to obtain a ferric chloride hexahydrate solution. Polyethylene glycol and sodium acetate were mixed at a mass ratio of 1:4, and added to the ferric chloride hexahydrate solution. The mixture was reacted at 200°C and 30 rpm for 20 hours. After the reaction was completed, the mixture was cooled, washed with ethanol, and vacuum dried to obtain magnetic iron oxide nanoparticles.

[0053] Step 6: Preparation of Magnetized Activated Kaolin

[0054] The magnetic iron oxide nanoparticles, deionized water and sodium silicate were uniformly mixed in a mass ratio of 9:130:22, and the pH of the mixed system was adjusted to 1 with 30wt% sulfuric acid and 0.1mol / L sodium hydroxide solution, and the mixture was reacted at 40°C and 30rpm for 2.5h. After the reaction was completed, the mixture was aged at 50°C for 6h to obtain a magnetic silicate iron oxide solution;

[0055] The kaolin was calcined at 600°C for 4 hours, cooled to room temperature, and then a 40wt% sulfuric acid solution (0.28 times the weight of the kaolin) was added, and the mixture was reacted at 90°C for 4 hours. After the reaction, the filtrate was washed with deionized water until the pH value of the filtrate was neutral. A magnetic silicate iron oxide solution (6 times the weight of the kaolin) was added, and the mixture was dried at 80°C for 24 hours. The mixture was crushed, sieved, and the magnetized active kaolin was separated with a magnet.

[0056] Step 7: Prepare water purifier

[0057] The polyaluminium chloride-magnesium silicate composite solution, the modified starch-modified chitosan composite solution and the magnetized active kaolin were mixed in a mass ratio of 26:102:8, and magnetically stirred at 27°C and 300rpm for 25min. After the stirring, ultrasonic dispersion and mixing treatment was performed. After the ultrasonic dispersion treatment was completed, the mixture was aged at 75°C for 24h and freeze-dried to obtain a water purifier.

[0058] Embodiment 3: A water purifier based on polyaluminium chloride, the preparation method is as follows:

[0059] Step 1: Prepare polyaluminium chloride solution

[0060] Aluminum chloride and deionized water were mixed and stirred at a mass ratio of 1:20 to fully dissolve, and a 0.18 mol / L sodium hydroxide solution (3 times the weight of aluminum chloride) was slowly added at 35° C. and 500 rpm to react for 3 hours to obtain a polyaluminum chloride solution.

[0061] Step 2: Preparation of polyaluminium chloride-magnesium silicate composite solution

[0062] Mix magnesium chloride hexahydrate, trichloroethylsilane and deionized water in a mass ratio of 1:1.5:19, stir evenly, and irradiate with low-temperature plasma for 60 minutes to obtain a magnesium chloride silicate solution;

[0063] The polyaluminium chloride solution and the magnesium aluminium silicate solution were mixed in a volume ratio of 4:1, reacted at 45°C and 55 rpm for 30 minutes, and allowed to stand and mature for 4 hours to obtain a polyaluminium chloride-magnesium silicate composite solution.

[0064] Step 3: Prepare modified starch solution

[0065] Starch and deionized water were mixed in a mass ratio of 1:42, stirred evenly, gelatinized at 85°C for 50 minutes, cooled to room temperature to obtain a starch solution, dimethyldiallylammonium chloride, acrylamide, and starch solution were mixed in a mass ratio of 1:0.6:200, the pH was adjusted to 2 with 0.1 mol / L dilute hydrochloric acid, reacted for 2.5 hours, and then 30 wt% sodium hydroxide solution was added until the pH was neutral to obtain a modified starch solution.

[0066] Step 4: Preparation of modified starch-modified chitosan composite solution

[0067] Chitosan, acetic acid, glutaraldehyde and deionized water were mixed in a mass ratio of 8:5:4:490, reacted at 40°C and 40rpm for 3h to obtain a cross-linked chitosan solution, diethylenetriaminepentaacetic acid, N-(3-dimethylaminopropyl)-N'-ethylcarbodiimide hydrochloride, N-hydroxysuccinimide, a sodium hydroxide solution with a molar volume of 1 mol / L and deionized water were mixed in a mass ratio of 9:11:12:12:480, reacted at 40°C and 40rpm for 3h to obtain an activated group solution, the cross-linked chitosan solution and the activated group solution were mixed in a volume ratio of 3:1, reacted at 60°C for 3h, tetrahydrofuran 1.25% times the volume of the mixed solution and a modified starch solution of the same volume as the mixed solution were added, and the reaction was continued for 2h to obtain a modified starch-modified chitosan composite solution.

[0068] Step 5: Preparation of magnetic iron oxide nanoparticles

[0069] Ferric chloride hexahydrate and ethylene glycol were mixed uniformly at a mass ratio of 1:44, and stirred until the solution was clear to obtain a ferric chloride hexahydrate solution. Polyethylene glycol and sodium acetate were mixed at a mass ratio of 1:3, added to the ferric chloride hexahydrate solution, and reacted at 200°C and 30rpm for 20h. After the reaction was completed, the mixture was cooled, washed with ethanol, and vacuum dried to obtain magnetic iron oxide nanoparticles.

[0070] Step 6: Preparation of Magnetized Activated Kaolin

[0071] The magnetic iron oxide nanoparticles, deionized water and sodium silicate were uniformly mixed in a mass ratio of 7:120:18, and the pH of the mixed system was adjusted to 1 with 30wt% sulfuric acid and 0.1mol / L sodium hydroxide solution, and the mixture was reacted at 40°C and 30rpm for 2.5h. After the reaction was completed, the mixture was aged at 50°C for 6h to obtain a magnetic silicate iron oxide solution;

[0072] The kaolin was calcined at 600°C for 4 hours, cooled to room temperature, and then a 40wt% sulfuric acid solution (0.25 times the weight of the kaolin) was added, and the mixture was reacted at 90°C for 4 hours. After the reaction, the filtrate was washed with deionized water until the pH value of the filtrate was neutral. A magnetic silicate iron oxide solution (4 times the weight of the kaolin) was added, and the mixture was dried at 80°C for 24 hours. The mixture was crushed, sieved, and the magnetized active kaolin was separated with a magnet.

[0073] Step 7: Prepare water purifier

[0074] The polyaluminium chloride-magnesium silicate composite solution, the modified starch-modified chitosan composite solution and the magnetized active kaolin were mixed in a mass ratio of 24:98:6, and magnetically stirred at 27°C and 300rpm for 25min. After the stirring, ultrasonic dispersion and mixing treatment was performed. After the ultrasonic dispersion treatment was completed, the mixture was aged at 75°C for 24h and freeze-dried to obtain a water purifier.

[0075] Based on Example 1, a control experiment was carried out, specifically Comparative Example 1 and Comparative Example 2, as described below:

[0076] Comparative Example 1: The amount of the polyaluminium chloride-magnesium silicate composite solution was reduced, and the other conditions were the same as those in Example 1.

[0077] A water purifier based on polyaluminium chloride, the preparation method is:

[0078] Step 1: Prepare polyaluminium chloride solution

[0079] Aluminum chloride and deionized water were mixed and stirred at a mass ratio of 1:22 to fully dissolve, and a 0.18 mol / L sodium hydroxide solution (3 times the weight of aluminum chloride) was slowly added at 35° C. and 500 rpm to react for 3 hours to obtain a polyaluminum chloride solution.

[0080] Step 2: Preparation of polyaluminium chloride-magnesium silicate composite solution

[0081] Mix magnesium chloride hexahydrate, trichloroethylsilane and deionized water in a mass ratio of 1:2:21, stir evenly, and irradiate with low-temperature plasma for 60 minutes to obtain a magnesium chloride silicate solution;

[0082] The polyaluminium chloride solution and the magnesium aluminium silicate solution were mixed at a volume ratio of 5:1, reacted at 45°C and 55 rpm for 30 minutes, and allowed to stand and mature for 4 hours to obtain a polyaluminium chloride-magnesium silicate composite solution.

[0083] Step 3: Prepare modified starch solution

[0084] Starch and deionized water were mixed in a mass ratio of 1:45, stirred evenly, gelatinized at 85°C for 50 minutes, cooled to room temperature to obtain a starch solution, dimethyldiallylammonium chloride, acrylamide, and starch solution were mixed in a mass ratio of 1:0.8:210, the pH was adjusted to 2 with 0.1 mol / L dilute hydrochloric acid, reacted for 2.5 hours, and then 30 wt% sodium hydroxide solution was added until the pH was neutral to obtain a modified starch solution.

[0085] Step 4: Preparation of modified starch-modified chitosan composite solution

[0086] Chitosan, acetic acid, glutaraldehyde and deionized water were mixed in a mass ratio of 10:5.5:4.5:500, reacted at 40°C and 40rpm for 3h to obtain a cross-linked chitosan solution, diethylenetriaminepentaacetic acid, N-(3-dimethylaminopropyl)-N'-ethylcarbodiimide hydrochloride, N-hydroxysuccinimide, a sodium hydroxide solution with a molar volume of 1 mol / L and deionized water were mixed in a mass ratio of 10:11.5:14:14:490, reacted at 40°C and 40rpm for 3h to obtain an activated group solution, the cross-linked chitosan solution and the activated group solution were mixed in a volume ratio of 2:1, reacted at 60°C for 3h, tetrahydrofuran 1.25% times the volume of the mixed solution and a modified starch solution of the same volume as the mixed solution were added, and the reaction was continued for 2h to obtain a modified starch-modified chitosan composite solution.

[0087] Step 5: Preparation of magnetic iron oxide nanoparticles

[0088] Ferric chloride hexahydrate and ethylene glycol were mixed uniformly at a mass ratio of 1:44.5, and stirred until the solution was clear to obtain a ferric chloride hexahydrate solution. Polyethylene glycol and sodium acetate were mixed at a mass ratio of 1:3.5, added to the ferric chloride hexahydrate solution, and reacted at 200°C and 30rpm for 20h. After the reaction was completed, the mixture was cooled, washed with ethanol, and vacuum dried to obtain magnetic iron oxide nanoparticles.

[0089] Step 6: Preparation of Magnetized Activated Kaolin

[0090] The magnetic iron oxide nanoparticles, deionized water and sodium silicate were uniformly mixed in a mass ratio of 8:125:20, and the pH of the mixed system was adjusted to 1 with 30wt% sulfuric acid and 0.1mol / L sodium hydroxide solution, and the mixture was reacted at 40°C and 30rpm for 2.5h. After the reaction was completed, the mixture was aged at 50°C for 6h to obtain a magnetic silicate iron oxide solution;

[0091] The kaolin was calcined at 600°C for 4 hours, cooled to room temperature, and then a 40wt% sulfuric acid solution (0.26 times the weight of the kaolin) was added, and the mixture was reacted at 90°C for 4 hours. After the reaction, the filtrate was washed with deionized water until the pH value of the filtrate was neutral. A magnetic silicate iron oxide solution (5 times the weight of the kaolin) was added, and the mixture was dried at 80°C for 24 hours. The mixture was crushed, sieved, and the magnetized active kaolin was separated with a magnet.

[0092] Step 7: Prepare water purifier

[0093] The polyaluminium chloride-magnesium silicate composite solution, deionized water, modified starch-modified chitosan composite solution and magnetized active kaolin were mixed in a mass ratio of 5:20:100:7, and magnetically stirred at 27°C and 300rpm for 25min. After the stirring, ultrasonic dispersion and mixing treatment was performed. After the ultrasonic dispersion treatment was completed, the mixture was aged at 75°C for 24h and freeze-dried to obtain a water purifier.

[0094] Comparative Example 2: The amount of the modified starch-modified chitosan composite solution was reduced, and the other conditions were the same as those in Example 1.

[0095] A water purifier based on polyaluminium chloride, the preparation method is:

[0096] Step 1: Prepare polyaluminium chloride solution

[0097] Aluminum chloride and deionized water were mixed and stirred at a mass ratio of 1:22 to fully dissolve, and a 0.18 mol / L sodium hydroxide solution (3 times the weight of aluminum chloride) was slowly added at 35° C. and 500 rpm to react for 3 hours to obtain a polyaluminum chloride solution.

[0098] Step 2: Preparation of polyaluminium chloride-magnesium silicate composite solution

[0099] Mix magnesium chloride hexahydrate, trichloroethylsilane and deionized water in a mass ratio of 1:2:21, stir evenly, and irradiate with low-temperature plasma for 60 minutes to obtain a magnesium chloride silicate solution;

[0100] The polyaluminium chloride solution and the magnesium aluminium silicate solution were mixed at a volume ratio of 5:1, reacted at 45°C and 55 rpm for 30 minutes, and allowed to stand and mature for 4 hours to obtain a polyaluminium chloride-magnesium silicate composite solution.

[0101] Step 3: Prepare modified starch solution

[0102] Starch and deionized water were mixed in a mass ratio of 1:45, stirred evenly, gelatinized at 85°C for 50 minutes, cooled to room temperature to obtain a starch solution, dimethyldiallylammonium chloride, acrylamide, and starch solution were mixed in a mass ratio of 1:0.8:210, the pH was adjusted to 2 with 0.1 mol / L dilute hydrochloric acid, reacted for 2.5 hours, and then 30 wt% sodium hydroxide solution was added until the pH was neutral to obtain a modified starch solution.

[0103] Step 4: Preparation of modified starch-modified chitosan composite solution

[0104] Chitosan, acetic acid, glutaraldehyde and deionized water were mixed in a mass ratio of 10:5.5:4.5:500, reacted at 40°C and 40rpm for 3h to obtain a cross-linked chitosan solution, diethylenetriaminepentaacetic acid, N-(3-dimethylaminopropyl)-N'-ethylcarbodiimide hydrochloride, N-hydroxysuccinimide, a sodium hydroxide solution with a molar volume of 1 mol / L and deionized water were mixed in a mass ratio of 10:11.5:14:14:490, reacted at 40°C and 40rpm for 3h to obtain an activated group solution, the cross-linked chitosan solution and the activated group solution were mixed in a volume ratio of 2:1, reacted at 60°C for 3h, tetrahydrofuran 1.25% times the volume of the mixed solution and a modified starch solution of the same volume as the mixed solution were added, and the reaction was continued for 2h to obtain a modified starch-modified chitosan composite solution.

[0105] Step 5: Preparation of magnetic iron oxide nanoparticles

[0106] Ferric chloride hexahydrate and ethylene glycol were mixed uniformly at a mass ratio of 1:44.5, and stirred until the solution was clear to obtain a ferric chloride hexahydrate solution. Polyethylene glycol and sodium acetate were mixed at a mass ratio of 1:3.5, added to the ferric chloride hexahydrate solution, and reacted at 200°C and 30rpm for 20h. After the reaction was completed, the mixture was cooled, washed with ethanol, and vacuum dried to obtain magnetic iron oxide nanoparticles.

[0107] Step 6: Preparation of Magnetized Activated Kaolin

[0108] The magnetic iron oxide nanoparticles, deionized water and sodium silicate were uniformly mixed in a mass ratio of 8:125:20, and the pH of the mixed system was adjusted to 1 with 30wt% sulfuric acid and 0.1mol / L sodium hydroxide solution, and the mixture was reacted at 40°C and 30rpm for 2.5h. After the reaction was completed, the mixture was aged at 50°C for 6h to obtain a magnetic silicate iron oxide solution;

[0109] The kaolin was calcined at 600°C for 4 hours, cooled to room temperature, and then a 40wt% sulfuric acid solution (0.26 times the weight of the kaolin) was added, and the mixture was reacted at 90°C for 4 hours. After the reaction, the filtrate was washed with deionized water until the pH value of the filtrate was neutral. A magnetic silicate iron oxide solution (5 times the weight of the kaolin) was added, and the mixture was dried at 80°C for 24 hours. The mixture was crushed, sieved, and the magnetized active kaolin was separated with a magnet.

[0110] Step 7: Prepare water purifier

[0111] The polyaluminium chloride-magnesium silicate composite solution, modified starch-modified chitosan composite solution, deionized water and magnetized activated kaolin were mixed in a mass ratio of 25:25:75:7, and magnetically stirred at 27°C and 300rpm for 25min. After the stirring, ultrasonic dispersion and mixing treatment was performed. After the ultrasonic dispersion treatment, the mixture was aged at 75°C for 24h and freeze-dried to obtain a water purifier. Detection experiment:

[0112] 25L of untreated sewage from a power plant in Jiangsu was taken and divided into 5 equal volumes. 10g of the water purifier prepared in Example 1, Example 2, Example 3, Comparative Example 1 and Comparative Example 2 were added respectively, stirred thoroughly, left to stand for 2h, and the performance was tested.

[0113] Determination of COD concentration: The COD concentration of the solution is determined in accordance with the national standard "Determination of Chemical Oxygen Demand of Water Quality-Dichromate Method" (GB 11914-1989).

[0114] Determination of suspended matter: The suspended matter in liquid shall be determined according to the Gravimetric Method for Determination of Suspended Matter in Water Quality (GB / T11901-1989).

[0115] Determination of ammonia nitrogen concentration: The concentration of ammonia nitrogen in the liquid is determined according to the “Determination of ammonia nitrogen in water quality-Salicylic acid spectrophotometry” (HJ 536-2009).

[0116] Determination of total phosphorus concentration: The concentration of total phosphorus in the liquid is determined in accordance with the "Determination of Total Phosphorus in Water Quality - Flow Injection-Ammonium Molybdate Spectrophotometry" (HJ 671-2013).

[0117] The results are as follows:

[0118] Water purifier performance Experimental Example 1 Experimental Example 2 Experimental Example 3 Comparative Example 1 Comparative Example 2 COD removal rate (%) 88.2% 88.0% 88.1% 82.4% 88.1% Suspended matter removal rate (%) 94.2% 93.9% 94.0% 85.2% 94.1% Ammonia nitrogen removal rate (%) 89.9% 90.1% 89.7% 89.7% 84.7% Total phosphorus removal rate (%) 91.6% 91.5% 91.8% 91.4% 83.2%

[0119] Conclusion: From the experiment, it can be seen that the performance of Example 1 is better than that of Comparative Example 1 and Comparative Example 2. Compared with Example 1, the water purifier of Comparative Example 2 reduces the proportion of modified starch-modified chitosan composite solution in the water purifier, which is manifested in the experiment as a decrease in the removal capacity of ammonia nitrogen and total phosphorus; Comparative Example 1 reduces the proportion of polyaluminum chloride-magnesium silicate composite solution in the water purifier, which is manifested in the experiment as a decrease in the removal capacity of COD and suspended solids. It shows that the water purifier of the present invention is indeed better than the ordinary polyaluminum chloride water purifier in terms of water purification effect. The water purifier of the present invention adds modified starch and modified chitosan, which not only saves costs, but is also more environmentally friendly; the added magnetic nanoparticles have relatively stable chemical properties and are easy to separate, and the magnetic nanoparticles have high reusability and regeneration capacity. On the whole, the water purifier of the present invention is better than the ordinary polyaluminum chloride water purifier.

[0120] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a water purifier based on polyaluminium chloride, characterized in that: The preparation method of the water purifier is specifically as follows: The polyaluminium chloride-magnesium silicate composite solution, the modified starch-modified chitosan composite solution and the magnetically active kaolin are mixed, stirred evenly, ultrasonically dispersed, aged and dried to obtain a water purifier.

2. The method for preparing a water purifier based on polyaluminium chloride according to claim 1, characterized in that: The mass ratio of the polyaluminium chloride-magnesium silicate composite solution, the modified starch-modified chitosan composite solution and the magnetically active kaolin is (24-26):(98-102):(6-8).

3. The method for preparing a water purifier based on polyaluminium chloride according to claim 1, characterized in that: During the ultrasonic dispersion treatment, the ultrasonic frequency is 34-60kHz, the ultrasonic power is 600-1200W, and the ultrasonic dispersion treatment time is 80-200min.

4. The method for preparing a water purifier based on polyaluminium chloride according to claim 1, characterized in that: The method for preparing polyaluminium chloride-magnesium silicate composite solution is: Fully dissolving aluminum chloride in deionized water, adding sodium hydroxide solution, and obtaining polyaluminum chloride solution after reaction; Mix magnesium chloride hexahydrate, trichloroethylsilane and deionized water, stir evenly, and irradiate with low-temperature plasma to obtain a magnesium chloride silicate solution; The polyaluminium chloride solution and the magnesium chloride silicate solution are mixed, stirred evenly, and allowed to stand for aging to obtain a polyaluminium chloride-magnesium silicate composite solution.

5. The method for preparing a water purifier based on polyaluminium chloride according to claim 1, characterized in that: The method for preparing the modified starch-modified chitosan composite solution is: The starch and deionized water are mixed and stirred for gelatinization to obtain a starch solution, and the dimethyldiallylammonium chloride, acrylamide and the starch solution are mixed and the pH is adjusted. After the reaction is completed, a modified starch solution is obtained; Chitosan, acetic acid, glutaraldehyde and deionized water are uniformly mixed to obtain a cross-linked chitosan solution after reaction, N-(3-dimethylaminopropyl)-N'-ethylcarbodiimide hydrochloride and N-hydroxysuccinimide are mixed and dissolved in deionized water, and diethylenetriamine pentaacetic acid and sodium hydroxide solution are added to react to obtain an activated group solution; The cross-linked chitosan solution and the activated group solution are mixed, and after the reaction is complete, tetrahydrofuran and the modified starch solution are added to continue the reaction to obtain a modified starch-modified chitosan composite solution.

6. The method for preparing a water purifier based on polyaluminium chloride according to claim 1, characterized in that: The method for preparing magnetized activated kaolin is: The ferric chloride hexahydrate and ethylene glycol are mixed, polyethylene glycol and sodium acetate are added to react, the product is washed with ethanol, and vacuum dried to obtain magnetic iron oxide nanoparticles; The magnetic iron oxide nanoparticles, deionized water and sodium silicate are uniformly mixed, the pH of the mixed system is adjusted with a sulfuric acid solution and a sodium hydroxide solution, and the mixture is aged after the reaction is completed to obtain a magnetic silicate iron oxide solution; The kaolin is calcined and then acidified, washed with deionized water, and then a magnetic silicate iron oxide solution is added, followed by drying, crushing, grinding, sieving, and separating the magnetically active kaolin with a magnet.

7. The method for preparing a water purifier based on polyaluminium chloride according to claim 4, characterized in that: The low-temperature plasma irradiation time is 40 to 80 minutes, the low-temperature plasma irradiation voltage is 4 to 6 kV, and the low-temperature plasma atmosphere is oxygen.

8. The method for preparing a water purifier based on polyaluminium chloride according to claim 5, characterized in that: The mass ratio of diethylenetriaminepentaacetic acid, N-(3-dimethylaminopropyl)-N'-ethylcarbodiimide hydrochloride and N-hydroxysuccinimide is (9-11):(11-12):(12-16); the volume ratio of cross-linked chitosan solution and activated group solution is (1-3):

1.

9. The method for preparing a water purifier based on polyaluminium chloride according to claim 6, characterized in that: The kaolin is calcined and then acidified. The calcination temperature is 500-700° C., the calcination time is 3-5 hours, and the acid used for the acidification is 40wt% sulfuric acid solution.

Citation Information

Patent Citations

  • Preparation method of magnetic kaolin

    CN104826600A

  • Preparation method and application of MCS / SA-PEI composite hydrogel beads

    CN111330553A

  • Composite fluorine removal agent for industrial wastewater and preparation method thereof and method for removing fluorine from industrial wastewater

    CN111547804A

  • Natural composite polyaluminium chloride water treatment agent and preparation method thereof

    CN111573798A

  • Methods For Flocculating Suspensions Using Biobased Renewable Flocculants

    US20110042321A1

Cited By

  • Modified polyaluminum chloride flocculant and preparation method thereof

    CN119873995A

  • Recyclable water treatment agent based on polyaluminum chloride and preparation method thereof

    CN119930004A

  • Process for producing coagulant through resource comprehensive utilization of polyaluminum chloride waste residues

    CN120325647A

  • Process for producing coagulant by comprehensive utilization of polyaluminum waste residue resources