Quartz tube and preparation method thereof
By purifying quartz sand and adjusting process parameters in the melting and forming step, the bubble problems and high production costs in the preparation of quartz tubes are solved, and high-quality quartz tube preparation is achieved, with good mechanical properties and durability .
Patent Information
- Application Number
- CN202410980290.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-01
AI Technical Summary
The existing quartz tube preparation process has strict requirements on raw materials, and bubbles are easily generated during the melting process, which affects the quality and performance of the finished product, and has a high production cost.
By purifying the quartz sand and adjusting parameters such as melting temperature, air pressure and traction speed in the melting molding step, combined with slow temperature increase and cooling, and injecting nitrogen, reduce bubble formation and improve the quality of the finished product.
The prepared quartz tube has good compressive, tensile, deformation and high temperature resistance, and the preparation process is relatively simple, not easily affected by raw materials, and the quality of the finished product is significantly improved.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of quartz tube preparation, and in particular to a quartz tube and a preparation method thereof. Background Art
[0002] As a special industrial technical glass made of silicon dioxide, quartz tube is widely used in many fields due to its excellent physical and chemical properties. Due to its high temperature resistance, quartz tube is often used to manufacture heating equipment such as infrared heaters and ultraviolet heaters; quartz tube is also widely used in scientific research and laboratories, semiconductor industry, electronic communications and other fields. With the continuous development of science and technology, the application field of quartz tube is still developing further.
[0003] However, there are still some defects in the current process preparation. For example, the requirements for raw materials are strict, bubbles will be generated during the melting process, and it is difficult to remove the bubbles, thus affecting the quality and performance of the final product; precise control is required during the molding process to ensure that the quality of the final product is not affected; due to the high requirements for raw materials and conditions in the production process, the production cost will increase to a certain extent. Summary of the invention
[0004] In view of the above-mentioned existing technical problems, the present invention aims to provide a quartz tube and a preparation method thereof. The quartz tube prepared by this method is resistant to compression, tension, deformation and high temperature, and the preparation process is simple and uncomplicated, and the final product is not greatly affected by the raw materials.
[0005] The invention discloses a method for preparing a quartz tube, which comprises the following steps.
[0006] S1 Quartz sand preparation: Quartz ore is crushed, washed, sorted, acid washed, calcined, water quenched, screened, and acid-leached and dried in sequence to obtain quartz sand.
[0007] S2 melting and molding: the quartz sand obtained in step S1 is placed in a high-temperature furnace, heated and melted, and a flux is added during the melting process to melt the quartz sand into a molten state; the molten quartz is placed in a mold, and pressed and molded to pull out a rough quartz tube of a desired shape.
[0008] S3 dehydroxylation: placing the crude quartz tube obtained in step S2 in a dehydroxylation furnace, heating the crude quartz tube, and after the reaction is completed, cooling down and taking out the dehydroxylation quartz tube from the dehydroxylation furnace, and washing the dehydroxylation quartz tube in an acidic solution to obtain a quartz tube.
[0009] Preferably, in the S1 quartz sand preparation step, in the pickling and calcining stage, the acidic solution used for pickling is a mixed solution of hydrochloric acid and nitric acid.
[0010] Preferably, the concentration ratio of hydrochloric acid to nitric acid in the acidic solution is 1:(0.8-1.4).
[0011] Preferably, in the S1 quartz sand preparation step, during the acid leaching and drying process, the acid leaching pressure is 3~4kPa.
[0012] Preferably, in the S2 melt-molding step, the melting temperature is 2100-2200°C.
[0013] Preferably, in the S2 melting and molding step, nitrogen needs to be continuously introduced and the pressure in the furnace is 10-20 kPa.
[0014] Preferably, in the S2 melt forming step, the pulling speed is 350-470 mm / min.
[0015] Preferably, in the S3 dehydroxylation step, the temperature of the dehydroxylation furnace is 1300-1400°C.
[0016] Preferably, in the S3 dehydroxylation step, the required dehydroxylation time is 1 to 2.25 h.
[0017] A quartz tube is prepared by any one of the above-mentioned methods for preparing a quartz tube.
[0018] Compared with the prior art, the present invention has the following beneficial effects: The present invention provides a method for preparing a quartz tube, wherein the raw material quartz sand is purified in the initial stage. The use of high-purity quartz sand as a raw material to prepare the quartz tube can effectively increase the service life of the quartz tube product. In the melting molding step, by adjusting various parameters in the preparation process, and keeping the temperature rising and falling slowly during the calcination and cooling process, and keeping nitrogen introduced all the time, this is not only to maintain the pressure in the furnace, but also to reduce bubbles in the finished quartz tube product, thereby improving the quality and durability of the finished quartz tube product.
[0019] The melting temperature is set at 2100~2200℃ to avoid crystallization. At this temperature, the viscosity of the quartz tube is also within an optimal range, which effectively reduces cracks and bubbles in the finished quartz tube. DETAILED DESCRIPTION
[0020] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.
[0021] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.
[0022] Embodiment 1: A method for preparing a quartz tube comprises the following steps.
[0023] S1 Preparation of quartz sand: crush the quartz ore into small pieces of 1~3cm, then wash it, and then continue to crush it for the second time after washing, sieve and collect, then crush the collected quartz ore powder for the third time, sieve and collect for the last time, put the finally collected quartz ore powder into a reactor, add an acidic solution prepared by hydrochloric acid and nitric acid at a concentration ratio of 1:0.8, and carry out acid leaching. The pressure in the reactor is 3kPa during acid leaching. After the acid leaching is completed, all the quartz powder in the acidic solution is fished out, washed and dried to obtain quartz sand.
[0024] S2 melting and molding: the quartz sand obtained in step S1 is placed in a high-temperature furnace, and the temperature is slowly heated to 2100°C to melt the quartz sand in the high-temperature furnace. During the melting process, nitrogen gas needs to be continuously introduced to maintain the gas pressure in the furnace at 10 kPa. During the melting process, the flux sodium carbonate is added to melt the quartz sand into a molten state. Subsequently, the molten quartz is placed in a mold, and a rough quartz tube of a desired shape is pulled out by pressure molding, wherein the pulling speed is 350-470 mm / min.
[0025] S3 dehydroxylation: the crude quartz tube obtained in step S2 is placed in a dehydroxylation furnace for heating. The temperature of the dehydroxylation furnace is increased in three stages. Each temperature is 100°C higher than the previous temperature. The heating time of each stage is 20 minutes. The temperature of the last stage is 1500°C. After the dehydroxylation reaction is completed, the dehydroxylated quartz tube is pulled out of the dehydroxylation furnace at a pulling speed of 350mm / min. Finally, the dehydroxylated quartz tube is placed in an acid solution for cleaning to obtain a quartz tube.
[0026] Embodiment 2: A method for preparing a quartz tube comprises the following steps.
[0027] S1 Preparation of quartz sand: crush the quartz ore into small pieces of 1~3cm, then wash it, and then continue to crush it for the second time after washing, sieve and collect, then crush the collected quartz ore powder for the third time, sieve and collect for the last time, put the finally collected quartz ore powder into a reactor, add an acid solution prepared by hydrochloric acid and nitric acid at a concentration ratio of 1:0.9, and carry out acid leaching. The pressure in the reactor is 3.2kPa during acid leaching. After the acid leaching is completed, all the quartz powder in the acid solution is fished out, washed and dried to obtain quartz sand.
[0028] S2 melting and molding: the quartz sand obtained in step S1 is placed in a high-temperature furnace, and the temperature is slowly heated to 2120°C to melt the quartz sand in the high-temperature furnace. During the melting process, nitrogen needs to be continuously introduced to maintain the gas pressure in the furnace at 12 kPa. During the melting process, a flux sodium carbonate is added to melt the quartz sand into a molten state. Subsequently, the molten quartz is placed in a mold, and a rough quartz tube of a desired shape is pulled out by pressure molding, wherein the pulling speed is 350-470 mm / min.
[0029] S3 dehydroxylation: the crude quartz tube obtained in step S2 is placed in a dehydroxylation furnace for heating. The temperature of the dehydroxylation furnace is increased in three stages. Each temperature is 100°C higher than the previous temperature. The heating time of each stage is 25 minutes. The temperature of the last stage is 1500°C. After the dehydroxylation reaction is completed, the dehydroxylated quartz tube is pulled out of the dehydroxylation furnace at a pulling speed of 370 mm / min. Finally, the dehydroxylated quartz tube is placed in an acid solution for cleaning to obtain a quartz tube.
[0030] Example 3: A method for preparing a quartz tube comprises the following steps.
[0031] S1 Preparation of quartz sand: crush the quartz ore into small pieces of 1~3cm, then wash it, and then continue to crush it for the second time after washing, sieve and collect, then crush the collected quartz ore powder for the third time, sieve and collect for the last time, put the finally collected quartz ore powder into a reactor, add an acid solution prepared by hydrochloric acid and nitric acid at a concentration ratio of 1:1.0, and carry out acid leaching. The pressure in the reactor is 3.4kPa during acid leaching. After the acid leaching is completed, all the quartz powder in the acid solution is fished out, washed and dried to obtain quartz sand.
[0032] S2 melting and molding: the quartz sand obtained in step S1 is placed in a high-temperature furnace, and the temperature is slowly heated to 2140°C to melt the quartz sand in the high-temperature furnace. During the melting process, nitrogen needs to be continuously introduced to maintain the gas pressure in the furnace at 14 kPa. During the melting process, a flux sodium carbonate is added to melt the quartz sand into a molten state. Subsequently, the molten quartz is placed in a mold, and a rough quartz tube of a desired shape is pulled out by pressure molding, wherein the pulling speed is 350-470 mm / min.
[0033] S3 dehydroxylation: the crude quartz tube obtained in step S2 is placed in a dehydroxylation furnace for heating. The temperature of the dehydroxylation furnace is increased in three stages. Each temperature is 100°C higher than the previous temperature. The heating time of each stage is 30 minutes. The temperature of the last stage is 1500°C. After the dehydroxylation reaction is completed, the dehydroxylated quartz tube is pulled out of the dehydroxylation furnace at a pulling speed of 390 mm / min. Finally, the dehydroxylated quartz tube is placed in an acid solution for cleaning to obtain a quartz tube.
[0034] Example 4: A method for preparing a quartz tube comprises the following steps.
[0035] S1 Preparation of quartz sand: crush the quartz ore into small pieces of 1~3cm, then wash it, and then continue to crush it for the second time after washing, sieve and collect, then crush the collected quartz ore powder for the third time, sieve and collect for the last time, put the finally collected quartz ore powder into a reactor, add an acid solution prepared by hydrochloric acid and nitric acid at a concentration ratio of 1:1.1, and carry out acid leaching. The pressure in the reactor is 3.6kPa during acid leaching. After the acid leaching is completed, all the quartz powder in the acid solution is fished out, washed and dried to obtain quartz sand.
[0036] S2 melting and molding: the quartz sand obtained in step S1 is placed in a high-temperature furnace, and the temperature is slowly heated to 2160°C to melt the quartz sand in the high-temperature furnace. During the melting process, nitrogen needs to be continuously introduced to maintain the gas pressure in the furnace at 16 kPa. During the melting process, a flux sodium carbonate is added to melt the quartz sand into a molten state. Subsequently, the molten quartz is placed in a mold, and a rough quartz tube of a desired shape is pulled out by pressure molding, wherein the pulling speed is 350-470 mm / min.
[0037] S3 dehydroxylation: the crude quartz tube obtained in step S2 is placed in a dehydroxylation furnace for heating. The temperature of the dehydroxylation furnace is increased in three stages. Each temperature is 100°C higher than the previous temperature. The heating time of each stage is 35 minutes. The temperature of the last stage is 1500°C. After the dehydroxylation reaction is completed, the dehydroxylated quartz tube is pulled out of the dehydroxylation furnace at a pulling speed of 410 mm / min. Finally, the dehydroxylated quartz tube is placed in an acid solution for cleaning to obtain a quartz tube.
[0038] Example 5: A method for preparing a quartz tube comprises the following steps.
[0039] S1 Preparation of quartz sand: crush the quartz ore into small pieces of 1~3cm, then wash it, and then continue to crush it for the second time after washing, sieve and collect, then crush the collected quartz ore powder for the third time, sieve and collect for the last time, put the finally collected quartz ore powder into a reactor, add an acid solution prepared by hydrochloric acid and nitric acid at a concentration ratio of 1:1.2, and carry out acid leaching. The pressure in the reactor is 3.8kPa during acid leaching. After the acid leaching is completed, all the quartz powder in the acid solution is fished out, washed and dried to obtain quartz sand.
[0040] S2 melting and molding: the quartz sand obtained in step S1 is placed in a high-temperature furnace, and the temperature is slowly heated to 2180°C to melt the quartz sand in the high-temperature furnace. During the melting process, nitrogen needs to be continuously introduced to maintain the gas pressure in the furnace at 18 kPa. During the melting process, a flux sodium carbonate is added to melt the quartz sand into a molten state. Subsequently, the molten quartz is placed in a mold, and a rough quartz tube of a desired shape is pulled out by pressure molding, wherein the pulling speed is 350-470 mm / min.
[0041] S3 dehydroxylation: the crude quartz tube obtained in step S2 is placed in a dehydroxylation furnace for heating. The temperature of the dehydroxylation furnace is increased in three stages. Each temperature is 100°C higher than the previous temperature. The heating time of each stage is 40 minutes. The temperature of the last stage is 1500°C. After the dehydroxylation reaction is completed, the dehydroxylated quartz tube is pulled out of the dehydroxylation furnace at a pulling speed of 430 mm / min. Finally, the dehydroxylated quartz tube is placed in an acid solution for cleaning to obtain a quartz tube.
[0042] Example 6: A method for preparing a quartz tube comprises the following steps.
[0043] S1 Preparation of quartz sand: crush the quartz ore into small pieces of 1~3cm, then wash it, and then continue to crush it for the second time after washing, sieve and collect, then crush the collected quartz ore powder for the third time, sieve and collect for the last time, put the finally collected quartz ore powder into a reactor, add an acid solution prepared by hydrochloric acid and nitric acid at a concentration ratio of 1:1.4, and carry out acid leaching. The pressure in the reactor is 4.0kPa during acid leaching. After the acid leaching is completed, all the quartz powder in the acid solution is fished out, washed and dried to obtain quartz sand.
[0044] S2 melting and molding: the quartz sand obtained in step S1 is placed in a high-temperature furnace, and the temperature is slowly heated to 2200°C to melt the quartz sand in the high-temperature furnace. During the melting process, nitrogen needs to be continuously introduced to maintain the gas pressure in the furnace at 20 kPa. During the melting process, the flux sodium carbonate is added to melt the quartz sand into a molten state. Subsequently, the molten quartz is placed in a mold, and a rough quartz tube of a desired shape is pulled out by pressure molding, wherein the pulling speed is 350-470 mm / min.
[0045] S3 dehydroxylation: the crude quartz tube obtained in step S2 is placed in a dehydroxylation furnace for heating. The temperature of the dehydroxylation furnace is increased in three stages. Each temperature is 100°C higher than the previous temperature. The heating time of each stage is 45 minutes. The temperature of the last stage is 1500°C. After the dehydroxylation reaction is completed, the dehydroxylated quartz tube is pulled out of the dehydroxylation furnace at a pulling speed of 470 mm / min. Finally, the dehydroxylated quartz tube is placed in an acid solution for cleaning to obtain a quartz tube.
[0046] The wall thickness, compressive strength, tensile strength, temperature tolerance, hydroxyl content, deformation resistance and presence of bubbles of the quartz tube products obtained in Examples 1 to 6 were tested, and the experimental data are shown in the following table:
[0047] It can be seen from the above table that for the quartz tube product obtained by the preparation method of a quartz tube provided by the present invention, in each embodiment, in the test items of tube wall thickness, compressive strength, tensile strength, temperature resistance, hydroxyl content, deformation resistance and the presence or absence of bubbles, the tube wall thickness will increase with the increase of melting temperature and pulling speed, but the difference in the range of thickening is not large; the compression resistance, tensile resistance and deformation resistance are all well reflected, and there are basically no bubbles in the finished product. Therefore, the quartz tube obtained by the preparation method of a quartz tube provided by the present invention is compression-resistant, tensile-resistant, deformation-resistant and high-temperature-resistant, and the preparation process is simple and uncomplicated, and the final product is not greatly affected by the raw materials.
[0048] In summary, the experimental conditions of Example 3 and Example 4 are better, and the quality of the quartz tube finally obtained is higher. Among them, the experimental conditions of Example 4 are relatively optimal.
[0049] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the scope of protection of the invention.
Claims
1. A method for preparing a quartz tube, It is characterized in that The following steps are involved: S1 Quartz sand preparation: Quartz ore is crushed, washed, sorted, acid-washed, calcined, water-quenched, screened, and acid-leached and dried to obtain quartz sand; S2 melting and molding: putting the quartz sand obtained in step S1 into a high-temperature furnace, heating and melting it, adding a flux during the melting process to melt the quartz sand into a molten state; putting the molten quartz into a mold, pressurizing and molding it to pull out a rough quartz tube of a desired shape; S3 dehydroxylation: placing the crude quartz tube obtained in step S2 in a dehydroxylation furnace, heating the crude quartz tube, and after the reaction is completed, cooling down and taking out the dehydroxylation quartz tube from the dehydroxylation furnace, and washing the dehydroxylation quartz tube in an acidic solution to obtain a quartz tube.
2. A method for preparing a quartz tube according to claim 1, It is characterized in that In the S1 quartz sand preparation step, in the pickling and calcining stage, the acidic solution used for pickling is a mixed solution of hydrochloric acid and nitric acid.
3. A method for preparing a quartz tube according to claim 2, It is characterized in that The concentration ratio of hydrochloric acid to nitric acid in the acidic solution is 1:(0.8-1.4).
4. The method for preparing a quartz tube according to claim 1, It is characterized in that In the S1 quartz sand preparation step, during the acid leaching and drying process, the acid leaching pressure is 3~4kPa.
5. The method for preparing a quartz tube according to claim 1, It is characterized in that In the S2 melt forming step, the melting temperature is 2100~2200℃.
6. The method for preparing a quartz tube according to claim 1, It is characterized in that In the S2 melting and molding step, nitrogen needs to be continuously introduced and the pressure in the furnace is 10~20kPa.
7. The method for preparing a quartz tube according to claim 1, It is characterized in that In the S2 melt forming step, the pulling speed is 350~470mm / min.
8. The method for preparing a quartz tube according to claim 1, It is characterized in that In the S3 dehydroxylation step, the temperature of the dehydroxylation furnace is 1300-1400°C.
9. The method for preparing a quartz tube according to claim 1, It is characterized in that In the S3 dehydroxylation step, the required dehydroxylation time is 1 to 2.25 h.
10. A quartz tube prepared by the method for preparing a quartz tube according to any one of claims 1 to 9.