Super-hydrophobic silicon dioxide aerogel slurry as well as preparation method and application thereof

The slurry prepared by composited superhydrophobic silica aerogel powder and solvents, using its high pore volume and lipophilic properties to absorb waste oil in the range hood, solving the problems of complex preparation of existing oil absorption boxes and environmental pollution, realizing the Environmentally friendly and efficient oil absorption effect.

CN118878255APending Publication Date: 2024-11-01THE HIGH SCHOOL AFFILIATED TO SHANGHAI JIAOTONG UNIV JIADING BRANCH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411127795.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The preparation method of existing oil-absorbing boxes is complicated, and it uses expensive raw materials or requires high temperature and high pressure conditions. It is not suitable for use in range hoods. In addition, a large amount of chemical dishwashing liquid is required to clean waste oil, resulting in environmental pollution.

Method used

Superhydrophobic silica aerogel powder is combined with solvents, binders, interface agents, etc. to prepare superhydrophobic silica aerogel slurry through hydration reaction, and utilize its high pore volume and lipophilic properties in the range hood. Adsorb waste oil to achieve environmentally friendly and efficient oil absorption effect.

Benefits of technology

Through the adsorption capacity of superhydrophobic silica aerogel, efficient adsorption and cleaning of waste oil is achieved, avoiding the pollution of the environment by chemical cleaning, and the process is simple and the cost is low.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118878255A_ABST
    Figure CN118878255A_ABST
Patent Text Reader

Abstract

The invention relates to super-hydrophobic silicon dioxide aerogel slurry as well as a preparation method and application thereof. The super-hydrophobic silicon dioxide aerogel slurry comprises super-hydrophobic silicon dioxide aerogel powder, a low-boiling-point organic solvent, an organic silicon binder, an interface agent, water, alcohol and a catalyst; the mass fraction of the super-hydrophobic silicon dioxide aerogel powder is 5-20% by taking the total mass of the super-hydrophobic silicon dioxide aerogel powder, the low-boiling-point organic solvent and the organic silicon binder as 100%; the mass fraction of the low-boiling-point organic solvent is 60-90%; the mass fraction of the organic silicon binder is 5-20%; the interfacial agent, the water, the alcohol and the catalyst respectively account for 1-5%, 0.2-2%, 3-5% and 0.1-0.5% of the total mass of the super-hydrophobic silicon dioxide aerogel powder, the low-boiling-point organic solvent and the organic silicon binder.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of oil absorbing materials, and particularly relates to a super-hydrophobic silica aerogel slurry and a preparation method and application thereof. Background Art

[0002] Range hoods are an indispensable kitchen appliance in today's families. While protecting human health, they also produce a lot of waste oil. Unlike ordinary cooking oil, this waste oil has a strong adhesive force. When pouring, a thick layer of oil will adhere to the bottom and sides of the oil collection box, which is difficult to remove. At the same time, the cleaning and discharge of waste oil will inevitably use a large amount of chemical detergents and cooking oil cleaners, which will cause great harm to the environment. Therefore, there is an urgent need for an efficient, environmentally friendly and convenient oil suction box.

[0003] Superhydrophobic silica aerogel powder is a porous nanomaterial with high oleophilic properties, featuring high porosity, large specific surface area, and large pore volume. The surface of its silica nanoparticles is loaded with a large number of methyl functional groups, so it has a strong affinity for oily materials. However, the density of superhydrophobic silica aerogel powder is very low, and the commercial powder density is only 0.03-0.05g / cm 3 , which is very easily affected by ambient air disturbance and dispersed. Therefore, it is very necessary to develop a preparation method for a new oil absorption box that integrates superhydrophobic silica aerogel powder with the oil absorption box shell.

[0004] There have been several studies on aerogel materials in the field of oil absorption. Chinese patent CN202311732779.1 discloses a method for preparing an elastic composite silicon aerogel oil-absorbing material, wherein nano carbon black is placed in a nitric acid solution of a certain concentration, stirred in a water bath at a certain temperature for a certain period of time, filtered and dried for use, an acid catalyst, a surfactant, urea, and a silicon precursor are mixed and dissolved in a certain amount of deionized water to be fully hydrolyzed, a certain amount of nano carbon black is added thereto, and impregnated with a sponge, placed in an oven for heating to complete gelation and aging, and dried to obtain an elastic composite silicon aerogel oil-absorbing material. Chinese patent CN202311520554.X discloses a method for preparing a waste straw-based cellulose aerogel oil absorbent, specifically: drying the waste straw, crushing it, alkali washing, cleaning it, then soaking it in hydrogen peroxide, washing, drying it, and dissolving it in alkali solution to obtain a cellulose solution; adding N,N'-methylenebisacrylamide to the cellulose solution for static crosslinking, freezing-thawing, soaking it in water and ethanol in turn, freeze-drying it to obtain a cellulose aerogel; immersing the cellulose aerogel in a mixed solution of glacial acetic acid and acetic anhydride, dripping H2SO4 for soaking esterification, freeze-drying it, and obtaining a waste straw-based cellulose aerogel oil absorbent. Chinese patent CN201811119941.1 discloses a peanut shell graphene composite aerogel oil-absorbing material and a preparation method thereof, using peanut shells and graphite oxide as raw materials, thiourea as a crosslinking agent, and separating graphene sheets through the gas generated by thiourea under high temperature and high pressure to form a three-dimensional porous structure with peanut shells, etc. However, the existing preparation methods of oil-absorbing aerogels are complex processes, or use expensive raw materials such as graphene, or use special preparation conditions such as high temperature and high pressure, which is not conducive to their application in the field of oil absorption boxes of range hoods. Summary of the invention

[0005] In view of the above problems, the present invention provides a super-hydrophobic silica aerogel slurry and a preparation method and application thereof. The method uses super-hydrophobic silica aerogel powder as a core raw material, and prepares super-hydrophobic silica aerogel slurry by compounding with a solvent, a binder, an auxiliary agent (an interface agent, water, an alcohol and a catalyst), etc. through a hydration reaction. The super-hydrophobic silica aerogel slurry is then used to prepare a super-hydrophobic silica aerogel, and applied to a high-efficiency and environmentally friendly oil absorption box for a range hood. The ultra-high pore volume and unique oleophilic properties of the silica aerogel are fully utilized to adsorb the condensed waste oil into its nanopores, thereby facilitating cleaning and avoiding waste oil and cleaning chemicals for cleaning the waste oil from polluting the environment.

[0006] In a first aspect, the present invention provides a super-hydrophobic silica aerogel slurry, comprising: super-hydrophobic silica aerogel powder, a low-boiling point organic solvent, an organic silicon binder, an interface agent, water, alcohol and a catalyst; Taking the total mass of the super-hydrophobic silica aerogel powder, the low-boiling point organic solvent and the organosilicon binder as 100%, the mass fraction of the super-hydrophobic silica aerogel powder is 5-20%; the mass fraction of the low-boiling point organic solvent is 60-90%; the mass fraction of the organosilicon binder is 5-20%; the interfacial agent accounts for 1-5% of the total mass of the super-hydrophobic silica aerogel powder, the low-boiling point organic solvent and the organosilicon binder; the water accounts for 0.2-2% of the total mass of the super-hydrophobic silica aerogel powder, the low-boiling point organic solvent and the organosilicon binder; the alcohol accounts for 3-5% of the total mass of the super-hydrophobic silica aerogel powder, the low-boiling point organic solvent and the organosilicon binder; the catalyst accounts for 0.1-0.5% of the total mass of the super-hydrophobic silica aerogel powder, the low-boiling point organic solvent and the organosilicon binder.

[0007] Preferably, the tap density of the super hydrophobic silica aerogel powder is 0.03-0.05 g / cm 3 ; The average pore diameter is less than 50nm; the pore volume is greater than 3ml / g; the water contact angle is greater than 150°.

[0008] Preferably, the low-boiling point organic solvent is an alkane organic solvent with a boiling point of 60 to 80°C, including at least one of n-hexane, cyclohexane, and carbon tetrachloride; the silicone binder is a room temperature vulcanized silicone rubber with a molecular weight of 100,000 to 300,000; the interface agent is methyl silicate, ethyl silicate or a combination thereof; the alcohol is ethanol, isopropanol or a combination thereof; the catalyst is an organic acid, including at least one of acetic acid, formic acid, citric acid, and oxalic acid.

[0009] Preferably, the viscosity of the super hydrophobic silica aerogel slurry is 30,000 to 60,000 cp.

[0010] In a second aspect, the present invention provides a method for preparing a super-hydrophobic silica aerogel slurry, comprising: mixing an organosilicon binder with a low-boiling point organic solvent, sequentially adding alcohol, water, an interfacial agent, a catalyst and half the mass of super-hydrophobic silica aerogel powder, reacting under a closed condition of 50 to 70° C. for 20 to 200 minutes, and then adding the remaining mass of the super-hydrophobic silica aerogel powder to obtain the super-hydrophobic silica aerogel slurry.

[0011] In a third aspect, the present invention provides a method for preparing a super-hydrophobic silica aerogel, comprising: pouring the super-hydrophobic silica aerogel slurry into an oil collecting box mold, placing the mold in a vacuum drying oven, and curing and drying the mold to obtain the super-hydrophobic silica aerogel.

[0012] Preferably, after pouring the super-hydrophobic silica aerogel slurry into the oil collecting box mold, the oil collecting box mold is vibrated on a rubber pad for several times to ensure that the slurry is evenly filled; the number of vibrations is 50 to 200 times.

[0013] Preferably, the curing and drying temperature is 80-100° C.; the curing and drying time is 1-48 hours; preferably 2-8 hours.

[0014] Preferably, after solidification and drying, the low boiling point organic solvent is condensed and recovered in a suitable manner; for example, the low boiling point organic solvent extracted under vacuum is recovered by a condenser.

[0015] In a fourth aspect, the present invention provides a super hydrophobic silica aerogel prepared according to the above preparation method.

[0016] Preferably, the compressive strength of the superhydrophobic silica aerogel is 0.1-0.2 MPa.

[0017] In a fifth aspect, the present invention provides an oil absorption box comprising the above-mentioned superhydrophobic silica aerogel.

[0018] In a sixth aspect, the present invention provides an application of the above-mentioned oil suction box in a range hood.

[0019] In the present invention, super-hydrophobic silica aerogel powder is used as the core raw material, and is compounded with a solvent, a binder, an auxiliary agent (interfacial agent, water, alcohol and catalyst), etc., and aerogel slurry is prepared through a hydration reaction, and then the slurry is poured into the oil collecting box shell, and the super-hydrophobic silica aerogel is obtained through high-temperature curing and solvent drying. Among them, the interfacial agent (such as silicate) is hydrolyzed under the action of water and catalyst, and a bridge is established between the silica aerogel nanoparticles and the organosilicon binder molecules, so that the silica aerogel powder and the organosilicon adhesive are firmly connected together to enhance the structural stability.

[0020] The super-hydrophobic silica aerogel oil absorption box prepared by the above process has aerogel powder in the box firmly bonded together by an adhesive to form a block with a certain strength and a fixed shape, and the super-hydrophobic silica aerogel fits well with the inner wall of the oil absorption box without any gaps. The compressive strength of the super-hydrophobic silica aerogel surface is about 0.1-0.2MPa.

[0021] After the aerogel oil absorption box prepared by the present invention is used, the internal pores of the superhydrophobic silica aerogel will be saturated with oil smoke, and the appearance will change from white to the brown color of waste oil. The silica aerogel that absorbs oil can be pried out of the box with a hard tool and cleaned, thereby realizing the reuse of the oil absorption box.

[0022] Beneficial effects: (1) The present invention compounds super-hydrophobic silica aerogel powder with an organosilicon binder to prepare a super-hydrophobic silica aerogel solid adsorption block with a certain strength and directly formed and cured in an oil collecting box, thereby avoiding the disadvantages of the silica powder having too low density and being easily blown away by the ambient airflow and the working airflow of the range hood, and being more convenient to use; (2) The present invention uses a low-boiling-point alkane organic solvent as the solvent of the organic silicone adhesive in the preparation of the super-hydrophobic silica aerogel slurry. On the one hand, it can fully dissolve and disperse the organic silicone binder, thereby promoting the close connection between the organic silicone long-chain molecules and the aerogel micron particles on a microscopic scale; on the other hand, due to its low boiling point and much smaller surface tension than water and ordinary solvents, it can be discharged by thermal evaporation after penetrating into the nanopores of the silica aerogel, and will not affect the pore structure of the silica aerogel, nor the oil absorption performance of the aerogel adsorption block; (3) The present invention introduces an interfacial agent (such as silicate) into the aerogel slurry, and pre-hydrolyzes it under the action of alcohol, water and a catalyst to form an organic silicon segment that is compatible with both the organic silicon adhesive and the silica aerogel particles, thereby enhancing the uniformity, integrity and mechanical properties of the composite system; (4) The strength of the superhydrophobic silica aerogel prepared by the present invention after molding is maintained at a relatively low level (0.1-0.2 MPa). After the aerogel is saturated with oil in the oil absorption box, the aerogel solid can be pried out by a hard tool and the box body can be cleaned, thereby realizing the reuse of the box body. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 The present invention is a flow chart of the preparation of a super-hydrophobic silica aerogel oil absorption box; Figure 2 Schematic diagram of the structure of the super-hydrophobic silica aerogel oil absorption box prepared by the present invention; wherein, 1-the outer wall of the oil collecting box; 2-the porous structure formed by the curing of the aerogel and the silicone adhesive; 3-the central column of the oil collecting box. DETAILED DESCRIPTION

[0024] To further explain the content, characteristics and practical effects of the present invention, the present invention is described in detail below in conjunction with the embodiments. It should be pointed out that the modification method of the design of the present invention is not limited to these specific embodiments. Without departing from the spirit and connotation of the design of the present invention, the equivalent replacement and modification made by those skilled in the art on the basis of reading the content of the present invention are also within the scope of the present invention. In the absence of special instructions, each percentage refers to the percentage by mass.

[0025] First, the present invention provides a super-hydrophobic silica aerogel slurry, including: super-hydrophobic silica aerogel powder, low-boiling point organic solvent, organosilicon binder, interface agent, water, alcohol and catalyst. In order to achieve the close fit of organosilicon binder and super-hydrophobic aerogel particles at a microscopic scale, the present invention adopts a variety of additives. Among them, the role of the interface agent (such as silicate) is to establish a bridge between aerogel nanoparticles and organosilicon binder molecules through hydrolysis, so that the aerogel powder and the organosilicon binder are firmly connected together to enhance structural stability. The interface agent must be hydrolyzed to play its interfacial bridging role. The role of water is a reactant for the hydrolysis of ethyl silicate; the role of alcohol is a solvent for water, which can promote the uniform dispersion of water in a low-boiling point organic solvent; the role of the catalyst is to catalyze the hydrolysis rate of silicate.

[0026] In an optional embodiment, the tap density of the super hydrophobic silica aerogel powder is 0.03 to 0.05 g / cm 3 ; Average pore size less than 50nm; Pore volume greater than 3ml / g; Water contact angle greater than 150°. The material, type and characteristics of aerogel powders vary, which will significantly affect the oil absorption performance of the final molded product. For example, hydrophilic silica aerogel powders have poor oil absorption performance; aerogel powders with low pore volume have low total oil absorption capacity; products with too low water contact angles have hydrophilic groups that are not conducive to oil adsorption.

[0027] In an optional embodiment, the low-boiling organic solvent is an alkane organic solvent with a boiling point of 60 to 80°C, including at least one of n-hexane, cyclohexane, and carbon tetrachloride. The purpose of using a low-boiling organic solvent in the present invention is: on the one hand, by utilizing its compatibility with the organosilicon binder, the organosilicon molecules with higher viscosity can be fully dispersed in the solvent, so that the long-chain organosilicon molecules and the aerogel micron particles are more firmly combined at the microscopic scale; on the other hand, its surface tension is much smaller than that of water and ordinary solvents. After penetrating into the nanopores of the silica aerogel, it can be discharged by thermal evaporation, and will not affect the pore structure and oil absorption performance of the silica aerogel. Solvents with a boiling point below 60°C evaporate very quickly and are more flammable, with greater safety risks; solvents with a boiling point above 80°C generally have a larger surface tension, and their evaporation process may cause the aerogel pores to collapse, affecting the oil absorption performance.

[0028] In an optional embodiment, the organosilicon binder is a room temperature vulcanized silicone rubber with a molecular weight of 100,000 to 300,000. The organosilicon binder (room temperature vulcanized silicone rubber) with a specific molecular weight (100,000 to 300,000) has a long chain structure, which can fully connect or wrap adjacent aerogel micron particles, and can achieve rapid curing at room temperature or under heating conditions. If the molecular weight of the organosilicon binder is too low, it will be difficult to effectively wrap a large number of aerogel particles; if the molecular weight is too high, the viscosity is too high, and it is difficult to form a uniform dispersion in the solvent, which is also not conducive to the formation of organosilicon-aerogel inclusions.

[0029] In an optional embodiment, the interface agent is methyl silicate, ethyl silicate or a combination thereof.

[0030] In an optional embodiment, the alcohol is ethanol, isopropanol or a combination thereof. The catalyst is an organic acid, including at least one of acetic acid, formic acid, citric acid and oxalic acid.

[0031] In an optional embodiment, taking the total mass of the super-hydrophobic silica aerogel powder, the low-boiling point organic solvent and the organosilicon binder as 100%, the mass fraction of the super-hydrophobic silica aerogel powder is 5-20%; the mass fraction of the low-boiling point organic solvent is 60-90%; the mass fraction of the organosilicon binder is 5-20%; the interfacial agent accounts for 1-5% of the total mass of the super-hydrophobic silica aerogel powder, the low-boiling point organic solvent and the organosilicon binder; the water accounts for 0.2-2% of the total mass of the super-hydrophobic silica aerogel powder, the low-boiling point organic solvent and the organosilicon binder; the alcohol accounts for 3-5% of the total mass of the super-hydrophobic silica aerogel powder, the low-boiling point organic solvent and the organosilicon binder; the catalyst accounts for 0.1-0.5% of the total mass of the super-hydrophobic silica aerogel powder, the low-boiling point organic solvent and the organosilicon binder.

[0032] In an optional embodiment, the viscosity of the super hydrophobic silica aerogel slurry is 30,000 to 60,000 cp.

[0033] The following is an exemplary description of the method for preparing the super-hydrophobic silica aerogel slurry provided by the present invention.

[0034] The preparation method of the super-hydrophobic silica aerogel slurry comprises: firstly mixing an organosilicon binder with a low-boiling point organic solvent, stirring evenly, then sequentially adding alcohol, water, an interfacial agent, a catalyst and half the mass of super-hydrophobic silica aerogel powder, reacting for 20 to 200 minutes under a closed condition of 50 to 70° C. to form an initial aerogel slurry, and then adding the remaining mass of the super-hydrophobic silica aerogel powder to obtain the super-hydrophobic silica aerogel slurry.

[0035] Since the organosilicon binder used in the present invention has a high viscosity, it can be appropriately heated, the stirring rate can be increased, and the equipment can be rinsed multiple times during the mixing process with the low-boiling point organic solvent. The reaction temperature of the system after adding alcohol, water, and interface agent is preferably 55-65°C, which should be lower than the boiling point of the solvent, and the reaction time is preferably 30-90 minutes. During the heating reaction, the interface agent (such as silicate) is hydrolyzed and undergoes cross-linking reaction with the silanol groups on the surface of the aerogel particles and the silanol groups on the surface of the organosilicon binder molecules to form a "bridge". The purpose of adding the aerogel powder in two batches is to avoid adding too much aerogel in the early stage, which affects the fluidity of the system and the degree of "bridging" reaction.

[0036] The preparation method of the super-hydrophobic silica aerogel (or super-hydrophobic silica aerogel oil absorption box) provided by the present invention specifically comprises the steps of: mold preparation, aerogel slurry casting, aerogel slurry curing and drying. The following is an exemplary description of the preparation method of super-hydrophobic silica aerogel (such as Figure 1 shown).

[0037] Pour the superhydrophobic silica aerogel slurry into the cleaned oil collecting box mold, and vibrate it several times (such as 100 times) on the rubber pad to make the slurry fill evenly. Since the internal structure of most oil collecting boxes is relatively complex, there are cylinders and hooks in the middle for fixing, and the aerogel slurry is thicker, with a viscosity ranging from 30,000 to 60,000 cp, it is necessary to apply vibration to make the aerogel slurry evenly dispersed and densely filled in the narrow oil absorption box. The viscosity of the aerogel slurry should not be too low or too high. If the viscosity is low, the amount of solvent used is large, and the volume shrinks greatly after curing, resulting in a small volume of the aerogel oil absorption block; if the viscosity is high, it is more difficult to pour in the oil collecting box and it is more difficult to disperse evenly.

[0038] In an optional embodiment, the oil collecting box may be made of plastic or metal. The oil collecting box needs to be cleaned before use, and may be surface treated if necessary to enhance its affinity with the organic silicone adhesive.

[0039] The oil collecting box filled with the super-hydrophobic silica aerogel slurry is placed in a vacuum oven for curing and drying to recover the solvent, thereby obtaining the super-hydrophobic silica aerogel.

[0040] In an optional embodiment, the curing and drying temperature is 80 to 100° C.; the curing and drying time is 1 to 48 hours; preferably 2 to 8 hours.

[0041] In an optional embodiment, the compressive strength of the super hydrophobic silica aerogel is controlled at 0.1-0.2 MPa. If the compressive strength is too low, it is easy to be damaged, and if it is too high, it is difficult to remove after use.

[0042] The oil absorption box including super-hydrophobic silica aerogel prepared by the present invention can absorb waste oil obtained by condensing oil smoke into the nanopores of the aerogel, thereby facilitating the cleaning of the oil box and also preventing waste oil and cleaning chemicals used in conventional cleaning processes from polluting the environment.

[0043] The following further examples are given to illustrate the present invention in detail. It should also be understood that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention belong to the scope of protection of the present invention. The specific process parameters and the like in the following examples are also only examples within a suitable range, that is, those skilled in the art can make a selection within a suitable range through the description herein, and are not limited to the specific values ​​​​exemplified below.

[0044] Example 1 (1) Material selection: Laboratory-made super-hydrophobic silica aerogel powder (tap density 0.035 g / cm 3 , average pore size less than 17nm, pore volume 5.5ml / g, water contact angle greater than 158°); low boiling point organic solvent is cyclohexane; commercial room temperature curing silicone rubber adhesive (viscosity 40000cp); interfacial agent is ethyl silicate; water is deionized water; alcohol is ethanol; catalyst is hydrochloric acid. The raw material ratio is: hydrophobic silica aerogel powder: cyclohexane: silicone rubber adhesive: ethyl silicate: water: ethanol: hydrochloric acid = 16.3: 74.5: 9.2: 3: 0.5: 4.2: 0.1. A commercially available plastic oil collecting box is selected as the shell and molding mold; (2) Preparation of aerogel slurry: Under stirring, the silicone rubber binder and cyclohexane were mixed evenly, and ethanol, water, ethyl silicate, and hydrochloric acid were added in sequence, and half of the mass of aerogel powder was slowly added. The mixture was reacted at 60° C. in a closed condition for 60 minutes, and finally the remaining mass of superhydrophobic silica aerogel powder was added. The mixture was stirred evenly and cooled for later use. (3) Aerogel slurry casting: Pour the aerogel slurry into the oil collecting box mold and vibrate it on a rubber pad for 100 times to ensure that the slurry is evenly filled; (4) Solidification and drying of aerogel slurry: The oil collecting box filled with aerogel slurry is placed in a vacuum oven at 95°C and heated for 3 hours for solidification. After the oil collecting box is taken out, the aerogel oil absorbing box is obtained. The cyclohexane extracted by vacuum is recovered by a condenser.

[0045] The super hydrophobic silica aerogel oil absorption box prepared in Example 1 is as follows Figure 2The surface strength of the obtained super-hydrophobic silica aerogel is relatively hard. The compressive strength of the obtained super-hydrophobic silica aerogel is 0.15MPa when the sample made with the same raw materials, proportion and process is tested according to the method specified in GB / T5486-2008. The obtained aerogel oil absorption box is installed on the range hood for two months. Its oil absorption performance is good, and there is no trace of oil on the surface of the oil absorption box. The aerogel in the box is earthy brown. The aerogel core that absorbs oil can be pried out of the box with a hard tool. After a simple scrubbing, the oil collection box can be reused.

[0046] Example 2 (1) Material selection: Laboratory-made super-hydrophobic silica aerogel powder (tap density 0.043 g / cm 3 , average pore size less than 15nm, pore volume 4.5ml / g, water contact angle greater than 152°); low boiling point organic solvent is cyclohexane; commercial room temperature curing silicone rubber adhesive (viscosity 45000cp); interfacial agent is ethyl silicate; water is deionized water; alcohol is ethanol; catalyst is sulfuric acid. The raw material ratio is: hydrophobic silica aerogel powder: cyclohexane: silicone rubber adhesive: ethyl silicate: water: ethanol: hydrochloric acid = 13.6: 70.9: 15.5: 3: 0.5: 4: 0.1. A commercially available plastic oil collecting box is selected as the shell and molding mold; (2) Preparation of aerogel slurry: Under stirring, the silicone rubber binder and cyclohexane were mixed evenly, ethanol, water, and ethyl silicate were added in sequence, and half of the mass of aerogel powder was slowly added. The mixture was reacted at 65° C. in a closed condition for 60 minutes, and finally the remaining mass of superhydrophobic silica aerogel powder was added. The mixture was stirred evenly and cooled for later use. (3) Aerogel slurry casting: Pour the aerogel slurry into the oil collecting box mold and vibrate it on a rubber pad for 100 times to ensure that the slurry is evenly filled; (4) Curing and drying of aerogel slurry: The oil collecting box filled with aerogel slurry is placed in a vacuum oven at 90°C and heated for 8 hours for curing. After the oil collecting box is taken out, the finished aerogel oil absorbing box is obtained. The cyclohexane extracted by vacuum is recovered by a condenser.

[0047] The surface strength of the aerogel oil absorption box obtained in Example 2 is relatively hard. A small sample made with the same raw materials, ratio and process was tested according to the method specified in GB / T5486-2008, and the compressive strength of the obtained superhydrophobic silica aerogel was 0.18 MPa; the obtained aerogel oil absorption box was installed on a range hood for 2 months, and the oil absorption and cleaning effects were good.

[0048] Example 3 (1) Material selection: Laboratory-made super-hydrophobic silica aerogel powder (tap density 0.035 g / cm 3, average pore size less than 35nm, pore volume 4ml / g, water contact angle greater than 155°); low boiling point organic solvent is n-hexane; commercial room temperature curing silicone rubber adhesive (viscosity 43000cp); interfacial agent is methyl silicate; water is deionized water; alcohol is isopropanol; catalyst is acetic acid. The raw material ratio is: hydrophobic silica aerogel powder: cyclohexane: silicone rubber adhesive: ethyl silicate: water: ethanol: hydrochloric acid = 11.8:70:18.2:2.2:0.3:3.5:0.1. A commercially available plastic oil collecting box is selected as the shell and molding mold; (2) Preparation of aerogel slurry: Under stirring, the silicone rubber binder and n-hexane were mixed evenly, isopropanol, water, and methyl silicate were added in sequence, and half of the mass of aerogel powder was slowly added. The mixture was reacted at 55° C. in a closed condition for 50 minutes, and finally the remaining mass of superhydrophobic silica aerogel powder was added. The mixture was stirred evenly and cooled for later use. (3) Aerogel slurry casting: Pour the aerogel slurry into the oil collecting box mold and vibrate it on a rubber pad for 100 times to ensure that the slurry is evenly filled; (4) Solidification and drying of aerogel slurry: The oil collecting box filled with aerogel slurry is placed in a vacuum oven at 85°C and heated for 8 hours for solidification. After the oil collecting box is taken out, the aerogel oil absorbing box is obtained. The n-hexane extracted by vacuum is recovered by a condenser.

[0049] The surface strength of the aerogel obtained in Example 3 is relatively hard. A small sample made with the same raw materials, ratio and process was tested according to the method specified in GB / T5486-2008, and the compressive strength of the obtained superhydrophobic silica aerogel was 0.12 MPa; the obtained aerogel oil absorption box was installed on a range hood for 2 months, and the oil absorption and cleaning effects were good.

[0050] Comparative Example 1

[0051] In this comparative example 1, the aerogel selected was commercially available hydrophilic silica aerogel powder to prepare the aerogel oil absorption box, and other raw materials and preparation process were the same as those in Example 1.

[0052] After heating and drying, the volume of the aerogel in the oil absorption box obtained in Comparative Example 1 shrinks to only half of the initial casting volume, and the surface hydrophilic silica aerogel is not suitable for the application of the aerogel oil absorption box of the present invention.

[0053] Comparative Example 2

[0054] The materials and preparation process of the aerogel oil absorption box in Comparative Example 2 are the same as those in Example 1, except that the ratio of the raw materials is: hydrophobic silica aerogel powder: cyclohexane: silicone rubber binder: ethyl silicate: water: ethanol: hydrochloric acid = 30:60:10:3:0.5:4.2:0.1.

[0055] The aerogel slurry obtained in this comparative example 2 has too high a consistency, and part of the powder is not completely wetted by the solvent; after curing and drying, the aerogel in the oil absorption box is in the form of discrete particles with no strength. This shows that the ratio of aerogel powder to silicone rubber binder should be within a reasonable range, and too much aerogel will lead to failure in molding.

[0056] Comparative Example 3

[0057] The materials and preparation process of the aerogel oil absorption box in Comparative Example 3 are the same as those in Example 1, except that the interface agent ethyl silicate is not used.

[0058] The aerogel in the oil absorption box obtained in this comparative example 3 has low strength, slightly powdered and granular on the surface, too thick slurry, and part of the powder is not completely wetted by the solvent; after curing and drying, the aerogel in the oil absorption box is in the form of discrete particles, and the compressive strength of the obtained aerogel is 0.08MPa when the sample made with the same raw materials, proportion and process is tested according to the method specified in GB / T5486-2008. This shows that the interface agent has a good effect in enhancing the curing strength of the aerogel slurry.

[0059] Comparative Example 4

[0060] The materials and preparation process of the aerogel oil absorption box in Comparative Example 4 are the same as those in Example 1, except that, during the preparation of the aerogel slurry, all the aerogel powders are added at once and then subjected to a hydrolysis reaction.

[0061] In this comparative example 4, after all the aerogel powders were added at once, the slurry obtained had a very high consistency, and some aerogel particles could not be wetted by the solvent. After the oil absorption box was made, the aerogel in the box was severely powdered and had no strength. This shows that the way of adding aerogel powders into the slurry can significantly affect the dispersibility of the adhesive, the powders, and the solvent, and affect the curing effect and strength of the final aerogel slurry.

[0062] Comparative Example 5

[0063] The materials and preparation process of the aerogel oil absorption box in this comparative example 5 are the same as those in Example 1, except that the organic solvent in the raw material is xylene, that is, the raw material ratio is: hydrophobic silica aerogel powder: xylene: silicone rubber binder: ethyl silicate: water: ethanol: hydrochloric acid = 16.3: 74.5: 9.2: 3: 0.5: 4.2: 0.1.

[0064] In this comparative example 5, since the solvent is the common solvent xylene instead of the low-boiling point organic solvent of the present invention, although the aerogel slurry can be prepared and the slurry can be smoothly cast and molded in the oil collecting box, the xylene solvent cannot be completely removed during the curing and drying stage after vacuum drying at 95°C for 3 hours, resulting in the solvent remaining in the cured aerogel oil-absorbing block, making subsequent cooking oil adsorption impossible.

[0065] Comparative Example 6

[0066] The materials and preparation process of the aerogel oil absorption box in this comparative example 6 are the same as those in Example 1, except that the organic solvent in the raw material is the common solvent ethanol, that is, the raw material ratio is: hydrophobic silica aerogel powder: ethanol: silicone rubber binder: ethyl silicate: water: ethanol: hydrochloric acid = 16.3: 74.5: 9.2: 3: 0.5: 4.2: 0.1.

[0067] In this comparative example 6, since the solvent is the common solvent ethanol instead of the low-boiling point organic solvent of the present invention, although the aerogel slurry can be prepared and the slurry can be smoothly cast and molded in the oil collecting box, the surface strength of the obtained aerogel oil absorption block is low, and the compressive strength of the corresponding sample is 0.08MPa; the obtained aerogel oil absorption box is installed on the range hood for actual measurement, and the oil absorption performance reaches saturation in only 13 days. This is because the silica nanoparticles produced after the hydrolysis of ethyl silicate diffuse into the aerogel nanopores with the ethanol solvent, resulting in weak interface strength of the aerogel particles, and the silica nanoparticles entering the aerogel pores block the aerogel nanopores, reducing the overall oil absorption effect.

[0068] Comparative Example 7

[0069] The materials and preparation process of the aerogel oil absorption box in Comparative Example 7 are the same as those in Example 1, except that the low-boiling point organic solvent is petroleum ether with a lower boiling point (boiling point is 30-60° C.).

[0070] In this comparative example 7, since petroleum ether with a lower boiling point is used as a solvent, although aerogel slurry can be prepared, the petroleum ether evaporates more during the stirring and feeding processes, resulting in the slurry being significantly thicker than that in Example 1. Therefore, it is impossible to achieve complete and dense filling of the slurry in the oil collecting box during the casting and molding stage; at the same time, the large amount of volatilization of petroleum ether in the operating environment also poses a great safety hazard.

[0071] Comparative Example 8

[0072] The materials and preparation process of the aerogel oil absorption box in Comparative Example 8 are the same as those in Example 1, except that the low boiling point organic solvent is replaced with dimethylacetamide with a higher boiling point of 164-166°C.

[0073] In this comparative example 8, since dimethylacetamide with a higher boiling point is used as the solvent, although the aerogel slurry can be prepared and the slurry can be smoothly cast and molded in the oil collecting box, during the curing and drying stage, the dimethylacetamide solvent cannot be completely removed by vacuum drying at 95°C for 3 hours, resulting in the solvent remaining in the cured aerogel oil-absorbing block, making subsequent cooking oil adsorption impossible.

[0074] Comparative Example 9

[0075] The materials and preparation process of the aerogel oil absorption box in this comparative example 9 are the same as those in Example 1, except that the binder is a phenolic resin binder, that is, the raw material ratio is: hydrophobic silica aerogel powder: cyclohexane: phenolic resin: ethyl silicate: water: ethanol: hydrochloric acid = 16.3: 74.5: 9.2: 3: 0.5: 4.2: 0.1.

[0076] In this comparative example 9, since the binder is a common binder phenolic resin instead of the silicone rubber binder of the present invention, although the aerogel slurry can be prepared and the slurry can be smoothly cast and molded in the oil collecting box, the surface strength of the obtained aerogel oil absorption block is also relatively high, and the corresponding compressive strength of the small sample is 0.28MPa; however, during the actual measurement on the range hood, the oil absorption performance reached saturation in only 8 days. This may be because the phenolic resin molecules are small, diffuse into the aerogel nanopores with the solvent, and undergo polymerization reaction in the pores, blocking the aerogel nanopores, thereby reducing the overall oil absorption effect.

[0077] Comparative Example 10

[0078] The materials and preparation process of the aerogel oil absorption box in Comparative Example 10 are the same as those in Example 1, except that the molecular weight of the silicone rubber binder used is 35,000.

[0079] The surface strength of the aerogel oil-absorbing box prepared in Comparative Example 10 is relatively low. The sample made with the same raw materials, proportions and process is tested according to the method specified in GB / T5486-2008. The compressive strength of the obtained superhydrophobic silica aerogel is 0.035MPa, which is easy to cause the aerogel oil-absorbing body to crack or powder under the action of external force or slight deformation of the box body. This shows that the molecular weight of the silicone rubber adhesive needs to be controlled within an appropriate range to ensure that the aerogel oil-absorbing box has certain strength and mechanical properties.

Claims

1. A super hydrophobic silica aerogel slurry, characterized in that: include: Super hydrophobic silica aerogel powder, low boiling point organic solvent, organosilicon binder, interface agent, water, alcohol and catalyst; Taking the total mass of the super-hydrophobic silica aerogel powder, the low-boiling point organic solvent and the organosilicon binder as 100%, the mass fraction of the super-hydrophobic silica aerogel powder is 5-20%; the mass fraction of the low-boiling point organic solvent is 60-90%; the mass fraction of the organosilicon binder is 5-20%; the interfacial agent accounts for 1-5% of the total mass of the super-hydrophobic silica aerogel powder, the low-boiling point organic solvent and the organosilicon binder; the water accounts for 0.2-2% of the total mass of the super-hydrophobic silica aerogel powder, the low-boiling point organic solvent and the organosilicon binder; the alcohol accounts for 3-5% of the total mass of the super-hydrophobic silica aerogel powder, the low-boiling point organic solvent and the organosilicon binder; the catalyst accounts for 0.1-0.5% of the total mass of the super-hydrophobic silica aerogel powder, the low-boiling point organic solvent and the organosilicon binder.

2. The super hydrophobic silica aerogel slurry according to claim 1, characterized in that The tap density of the super hydrophobic silica aerogel powder is 0.03-0.05 g / cm 3 ; The average pore diameter is less than 50nm; the pore volume is greater than 3ml / g; the water contact angle is greater than 150°.

3. The super hydrophobic silica aerogel slurry according to claim 1 or 2, characterized in that The low-boiling point organic solvent is an alkane organic solvent with a boiling point of 60 to 80°C, including at least one of n-hexane, cyclohexane, and carbon tetrachloride; the silicone binder is a room temperature vulcanized silicone rubber with a molecular weight of 100,000 to 300,000; the interface agent is methyl silicate, ethyl silicate or a combination thereof; the alcohol is ethanol, isopropanol or a combination thereof; the catalyst is an organic acid, including at least one of acetic acid, formic acid, citric acid, and oxalic acid.

4. The super hydrophobic silica aerogel slurry according to any one of claims 1 to 3, characterized in that The viscosity of the super hydrophobic silica aerogel slurry is 30000-60000 cp.

5. A method for preparing a super hydrophobic silica aerogel slurry according to any one of claims 1 to 4, characterized in that: include: The organosilicon binder is mixed with a low-boiling point organic solvent, and alcohol, water, an interfacial agent, a catalyst and half the mass of super-hydrophobic silica aerogel powder are added in sequence, reacting for 20 to 200 minutes under a closed condition of 50 to 70° C., and then the remaining mass of the super-hydrophobic silica aerogel powder is added to obtain the super-hydrophobic silica aerogel slurry.

6. A method for preparing a super-hydrophobic silica aerogel, characterized in that: include: The super-hydrophobic silica aerogel slurry according to any one of claims 1 to 4 is poured into an oil collecting box mold, and the super-hydrophobic silica aerogel is obtained by curing and drying.

7. The preparation method according to claim 6, characterized in that: The curing and drying temperature is 80-100° C.; the curing and drying time is 1-48 hours, preferably 2-8 hours.

8. A super hydrophobic silica aerogel prepared according to the preparation method according to claim 6 or 7, characterized in that: The compressive strength of the super hydrophobic silica aerogel is 0.1-0.2 MPa.

9. An oil absorption box comprising the super-hydrophobic silica aerogel according to claim 8.

10. Use of the oil suction box according to claim 9 in a range hood.

Citation Information

Patent Citations

  • Peanut hull graphene compound aerogel oil absorption material and preparation method thereof

    CN109513425A

  • Preparation method of waste straw-based cellulose aerogel oil absorbent

    CN117504827A

  • Preparation method, material and application of elastic composite silica aerogel oil absorption material

    CN117696025A