Modified lightweight aggregate reinforced green light acid-activated geopolymer mortar and preparation method thereof

Through the combination of phosphoric acid-excited modified ceramic sand and metakaolin and other materials, high-strength and low-density acid-excited polymer mortar is formed, which solves the problem of insufficient strength of traditional light mortars and realizes simple preparation and high-performance application of materials .

CN118878262APending Publication Date: 2024-11-01GUILIN UNIV OF ELECTRONIC TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410973719.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Traditional lightweight mortars have low strength, which limits their application. The existing improved methods have complex materials and high energy consumption in the preparation process, so simpler and more effective solutions are needed.

Method used

Using phosphoric acid-excited modified ceramic sand, metakaolin, polycarboxylic acid water reducer and other materials, through vacuum soaking and steam curing, a high-strength, low-density acid-excited polymer mortar is formed, and the microporous structure and phosphoric acid of ceramic sand are used. The sustained release mechanism improves the density and durability of the mortar.

Benefits of technology

It realizes light acid-activated polymer mortar with high strength and fluidity. It has simple material and low energy consumption. It is suitable for high-temperature fire-proof and corrosion-resistant applications, improving the performance and durability of building materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004953946570000081
    Figure BDA0004953946570000081
Patent Text Reader

Abstract

The invention provides modified lightweight aggregate reinforced green light acid-activated geopolymer mortar and a preparation method thereof, and the preparation method comprises the following steps: placing pottery sand in phosphoric acid for soaking, adsorption and modification, and then carrying out surface drying to obtain modified pottery sand; mixing the modified pottery sand, metakaolin, phosphoric acid, water and a polycarboxylate superplasticizer to obtain a mixture; injecting the mixture into a mold, and performing steam curing to obtain an early mortar test block; and curing the early mortar test block at room temperature. According to the invention, phosphoric acid is utilized to excite metakaolin to prepare a novel gel material, traditional cement is replaced, the pottery sand soaked and modified by phosphoric acid is further added into the mortar, the micropore structure of the pottery sand causes the effect of slow release of an internal pump in the mortar, high-concentration phosphoric acid in the pottery sand is slowly released along with the prolonging of the curing time, and the effect of slow release of the internal pump in the mortar is achieved. The interface reaction around the pottery sand is more sufficient, so that the compactness and the strength of the material are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building materials, and in particular to a modified lightweight aggregate reinforced green lightweight acid-activated geopolymer mortar and a preparation method thereof. Background Art

[0002] Lightweight mortar is a material made of lightweight aggregate (such as perlite, expanded perlite, expanded vermiculite, ceramic sand, etc.) as the main raw materials, mixed with cement, lime and other ingredients. Due to the low density of lightweight aggregate, lightweight mortar has a lower density and lighter weight. It is lighter than ordinary mortar and is suitable for use in lightweight walls such as interior walls, exterior walls, roofs, thermal insulation layers, sound insulation layers and other parts of buildings. It has the advantages of thermal insulation, heat insulation and sound insulation. However, traditional lightweight mortar generally has low strength, which limits its application.

[0003] At present, the commonly used solutions include: (1) using high-performance cementitious materials, that is, using composite cementitious materials to replace single cement, such as using cement and silica fume, slag or kaolin in combination to improve the strength of mortar; (2) adding fiber: adding fiber to lightweight mortar can improve its crack resistance and toughness; (3) adding fine high-strength aggregate: adding quartz sand, river sand, machine-made sand, etc. to lightweight mortar can improve the strength of mortar; (4) adding lightweight aggregate: adding glass beads, floating beads, polyurethane rigid foam particles, rubber particles, etc. to mortar can reduce the density of mortar, but the strength will be reduced; (5) application of admixtures: using admixtures such as water reducers, dispersants and defoamers, these admixtures can improve the workability and strength development of mortar. However, the above methods use complex materials and have high energy consumption in the preparation process, and other solutions need to be further developed. Summary of the invention

[0004] Based on this, the present invention provides a method for preparing a modified lightweight aggregate reinforced green lightweight acid-activated geopolymer mortar with high strength and fluidity and simple materials.

[0005] A method for preparing modified lightweight aggregate reinforced green lightweight acid-activated geopolymer mortar comprises the following steps:

[0006] The ceramic sand is placed in phosphoric acid for immersion adsorption modification, and then surface drying is performed to obtain modified ceramic sand;

[0007] Mix 5 to 10 parts of the modified pottery sand, 98 to 102 parts of metakaolin, 72 to 74 parts of phosphoric acid, 65 to 67 parts of water and 1 to 1.4 parts of a polycarboxylic acid water reducer by weight to obtain a mixture;

[0008] The mixture is injected into a mold and steam cured to obtain an early mortar test block;

[0009] The early mortar test block is placed at room temperature for curing to obtain the modified lightweight aggregate reinforced green lightweight acid-activated geopolymer mortar.

[0010] In one embodiment, the soaking adsorption modification is carried out under vacuum negative pressure conditions, the negative pressure is controlled at 0.084-0.087 MPa, and the soaking time is 23-25 ​​hours. Under vacuum, the ceramic sand can absorb more phosphoric acid, which plays the role of internal pump release. In the later stage of curing, the ceramic sand continuously provides reaction products to the surrounding area, thereby increasing the degree of reaction around the interface and thus improving the overall strength.

[0011] In one embodiment, the ceramic sand is composed of ceramic sand with a particle size of 0.08-0.15 mm, ceramic sand with a particle size of 0.15-0.315 mm, and ceramic sand with a particle size of 0.315-0.625 mm. The fluidity and density can be improved by setting the mixed gradation, and the modified ceramic sand can be more densely distributed in the mortar under limited dosage, thereby improving the strength.

[0012] In one of the embodiments, the mass ratio of the 0.08-0.15 mm particle size pottery sand, the 0.15-0.315 mm particle size pottery sand and the 0.315-0.625 mm particle size pottery sand is 1.5-3:2.5-3.5:4-5.

[0013] In one embodiment, the steam curing comprises the following steps: injecting the mixture into the mold and then placing it in a 38-42°C steam curing box for curing for 23-25 ​​hours, then demolding and continuing to heat up to 58-62°C for curing for 23-25 ​​hours. Curing at about 40°C for 1 day is to fully harden it and avoid surface cracking and internal damage caused by too high an early curing temperature, and subsequent curing at about 60°C is to improve its early strength.

[0014] In one embodiment, the early mortar test block is placed at room temperature for curing under the conditions of 92% to 98% humidity and 0.38 to 0.42 MPa vacuum. Vacuum negative pressure curing can exert a driving force on the phosphoric acid in the ceramic sand, making the internal phosphoric acid easier to diffuse outward and diffuse more widely, thereby further improving the strength at the interface.

[0015] In one embodiment, the following steps are further included before the soaking adsorption modification: the ceramic sand is ultrasonically cleaned and then dried at 55-65° C. for 22-26 hours. The cleaning of the ceramic sand can remove some dust and other impurities that block the pores of the ceramic sand, and the high-temperature drying of the fine wet ceramic sand will cause fine cracks in the ceramic sand, so that the ceramic sand soaking modification can adsorb more phosphoric acid.

[0016] In one embodiment, the loose bulk density of the ceramic sand is 700-800 kg / m 3 , the saturated water absorption rate is 4.5%.

[0017] In one embodiment, the particle size of the metakaolin is 4000-6000 mesh, wherein the weight percentage of silicon dioxide is 54% and the weight percentage of aluminum oxide is 43%.

[0018] The present invention also provides a modified lightweight aggregate reinforced green lightweight acid-activated geopolymer mortar, which is prepared according to the above preparation method.

[0019] The above solution of the present invention has the following beneficial effects:

[0020] The present invention utilizes phosphoric acid to activate metakaolin to prepare a new gel material, which replaces traditional cement. The gel material has the advantages of light weight, environmental protection, low cost, corrosion resistance, low carbon emission, etc. Moreover, phosphoric acid-soaked modified pottery sand is further added to the mortar, and the microporous structure of the pottery sand causes it to play an "internal pump release" effect inside the mortar. As the curing time increases, the high concentration of phosphoric acid in the pottery sand is slowly released, so that the interface reaction around the pottery sand is more sufficient, thereby improving the density and strength of the material. In addition, the use of phosphoric acid-based materials and pottery sand can effectively avoid the alkali aggregate reaction problem similar to that of cement materials, and improve the durability of the mortar. The added pottery sand has a reasonable grading, and the pottery sand is more densely distributed in the mortar, and the "internal pump release" effect is more obvious; the reasonable grading also improves the fluidity, and the fine pottery sand has good filling of the capillary pores, and the aggregates are densely filled, which also improves the performance of the mortar. Because the acid-activated geopolymer material has excellent mechanical properties, high temperature stability and corrosion resistance. It can be used to make heat-insulating and high-temperature resistant fireproof panels, such as in subways, tunnels, high-rise buildings and other areas with fire hazards; and can be used in construction projects in areas prone to alkali-aggregate reaction, areas corroded by chemical media, and the reinforcement, repair and new construction of certain buildings damaged by corrosion. DETAILED DESCRIPTION

[0021] In order to make the technical problems, technical solutions and advantages to be solved by the present invention clearer, the following will be described in detail in conjunction with specific embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0022] In addition, the technical features involved in the different embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other. The reagents and instruments used in the examples are conventionally selected in the art unless otherwise specified. The experimental methods without specific conditions in the examples are implemented according to conventional conditions, such as the conditions described in the literature, books or methods recommended by the manufacturer.

[0023] The following are specific examples. The metakaolin involved in the following examples comes from Shanghai Haofu Chemical Co., Ltd., and the phosphoric acid comes from Guilin Hongshengda Chemical Reagent Co., Ltd. The H3PO4 content of the phosphoric acid is 84-85%, and the water content is about 14%-15%. The chemical composition of the metakaolin is shown in Table 1.

[0024] Table 1 Chemical composition of raw materials (wt%)

[0025] Element <![CDATA[SiO2]]> <![CDATA[Al2O3]]> <![CDATA[Fe2O3]]> <![CDATA[TiO2]]> other Metakaolin 54.0 43.0 1.0 1.2 1.3

[0026] Example 1

[0027] A modified lightweight aggregate reinforced green lightweight acid-activated geopolymer mortar. The raw materials include the following components in parts by weight: 1.5 kg of 0.08-0.15 mm-diameter pottery sand, 1.5 kg of 0.15-0.315 mm-diameter pottery sand, 3.0 kg of 0.315-0.625 mm-diameter pottery sand, 100.0 kg of metakaolin, 73.3 kg of phosphoric acid, 66.8 kg of water, and 1.2 kg of polycarboxylic acid water reducer.

[0028] The preparation method comprises the following steps:

[0029] Step S1, weighing basic ceramic sand of different particle sizes according to the particle size ratio of the modified lightweight aggregate, washing the ceramic sand in an ultrasonic cleaning machine, replacing clean water every 5 minutes, and washing 5 times in total. Spreading the washed ceramic sand thinly on a sieve, putting it in an electric heating blower and drying it at 60°C for 24 hours until the moisture in the ceramic sand is dried.

[0030] Step S2, soaking the cleaned and dried pottery sand in phosphoric acid for vacuum soaking adsorption modification, the vacuum negative pressure is controlled at 0.087MPa, and the vacuum soaking time is 24h. After soaking, the modified pottery sand is placed in a permeable bag to squeeze and filter out excess phosphoric acid on the surface to obtain modified pottery sand with a relatively dry surface.

[0031] Step S3, weighing various raw materials according to the composition and proportion of the modified lightweight aggregate reinforced green lightweight acid-activated geopolymer mortar, mixing the gel raw materials for 5 minutes, and then adding modified pottery sand and stirring for 5 minutes to obtain a mixture.

[0032] Step S4, injecting the mixture into a mold, covering the top surface with a film, and then putting it into a 40°C steam curing box for high-temperature curing for 24 hours, demolding, and continuing to heat up to 60°C for high-temperature curing for 24 hours to obtain an early mortar test block.

[0033] Step S5, placing the early mortar test block in a vacuum box at room temperature, 95% humidity and 0.04 MPa vacuum degree, and performing negative pressure wet curing.

[0034] Example 2

[0035] A modified lightweight aggregate reinforced green lightweight acid-activated geopolymer mortar, the raw materials of which include the following components in parts by weight: 6.0 kg of 0.315-0.625 mm particle size pottery sand, 100.0 kg of metakaolin, 73.3 kg of phosphoric acid, 66.8 kg of water, and 1.2 kg of polycarboxylic acid water reducer.

[0036] The preparation method comprises the following steps:

[0037] Step S1, weigh the basic ceramic sand, put the ceramic sand into an ultrasonic cleaning machine for cleaning, replace the clean water every 5 minutes, and clean it 5 times in total. Spread the cleaned ceramic sand thinly on the sieve, put it into an electric blower and dry it at 60°C for 24 hours until the moisture in the ceramic sand is dried.

[0038] Step S2, soaking the cleaned and dried pottery sand in phosphoric acid for vacuum soaking adsorption modification, the vacuum negative pressure is controlled at 0.087MPa, and the vacuum soaking time is 24h. After soaking, the modified pottery sand is placed in a permeable bag to squeeze and filter out excess phosphoric acid on the surface to obtain modified pottery sand with a relatively dry surface.

[0039] Step S3, weighing various raw materials according to the composition and proportion of the modified lightweight aggregate reinforced green lightweight acid-activated geopolymer mortar, mixing the gel raw materials for 5 minutes, and then adding modified pottery sand and stirring for 5 minutes to obtain a mixture.

[0040] Step S4, injecting the mixture into a mold, covering the top surface with a film, and then putting it into a 40°C steam curing box for high-temperature curing for 24 hours, demolding, and continuing to heat up to 60°C for high-temperature curing for 24 hours to obtain an early mortar test block.

[0041] Step S5, placing the early mortar test block in a vacuum box at room temperature, 95% humidity and 0.04 MPa vacuum degree, and performing negative pressure wet curing.

[0042] Example 3

[0043] A modified lightweight aggregate reinforced green lightweight acid-activated geopolymer mortar. The raw materials include the following components in parts by weight: 1.2 kg of 0.08-0.15 mm-diameter ceramic sand, 2.8 kg of 0.15-0.315 mm-diameter ceramic sand, 4.0 kg of 0.315-0.625 mm-diameter ceramic sand, 100.0 kg of metakaolin, 73.3 kg of phosphoric acid, 66.8 kg of water, and 1.2 kg of polycarboxylic acid water reducer.

[0044] The preparation method comprises the following steps:

[0045] Step S1, weighing basic ceramic sand of different particle sizes according to the particle size ratio of the modified lightweight aggregate, washing the ceramic sand in an ultrasonic cleaning machine, replacing clean water every 5 minutes, and washing 5 times in total. Spreading the washed ceramic sand thinly on a sieve, putting it in an electric heating blower and drying it at 60°C for 24 hours until the moisture in the ceramic sand is dried.

[0046] Step S2, soaking the cleaned and dried pottery sand in phosphoric acid for vacuum soaking adsorption modification, the vacuum negative pressure is controlled at 0.087MPa, and the vacuum soaking time is 24h. After soaking, the modified pottery sand is placed in a permeable bag to squeeze and filter out excess phosphoric acid on the surface to obtain modified pottery sand with a relatively dry surface.

[0047] Step S3, weighing various raw materials according to the composition and proportion of the modified lightweight aggregate reinforced green lightweight acid-activated geopolymer mortar, mixing the gel raw materials for 5 minutes, and then adding modified pottery sand and stirring for 5 minutes to obtain a mixture.

[0048] Step S4, injecting the mixture into a mold, covering the top surface with a film, and then putting it into a 40°C steam curing box for high-temperature curing for 24 hours, demolding, and continuing to heat up to 60°C for high-temperature curing for 24 hours to obtain an early mortar test block.

[0049] Step S5, placing the early mortar test block in a vacuum box at room temperature, 95% humidity and 0.04 MPa vacuum degree, and performing negative pressure wet curing.

[0050] Example 4

[0051] A modified lightweight aggregate reinforced green lightweight acid-activated geopolymer mortar. The raw materials include the following components in parts by weight: 1.8 kg of 0.08-0.15 mm-diameter ceramic sand, 1.8 kg of 0.15-0.315 mm-diameter ceramic sand, 2.4 kg of 0.315-0.625 mm-diameter ceramic sand, 100.0 kg of metakaolin, 73.3 kg of phosphoric acid, 66.8 kg of water, and 1.2 kg of polycarboxylic acid water reducer.

[0052] The preparation method comprises the following steps:

[0053] Step S1, weighing basic ceramic sand of different particle sizes according to the particle size ratio of the modified lightweight aggregate, washing the ceramic sand in an ultrasonic cleaning machine, replacing clean water every 5 minutes, and washing 5 times in total. Spreading the washed ceramic sand thinly on a sieve, putting it in an electric heating blower and drying it at 60°C for 24 hours until the moisture in the ceramic sand is dried.

[0054] Step S2, soaking the cleaned and dried pottery sand in phosphoric acid for vacuum soaking adsorption modification, the vacuum negative pressure is controlled at 0.087MPa, and the vacuum soaking time is 24h. After soaking, the modified pottery sand is placed in a permeable bag to squeeze and filter out excess phosphoric acid on the surface to obtain modified pottery sand with a relatively dry surface.

[0055] Step S3, weighing various raw materials according to the composition and proportion of the modified lightweight aggregate reinforced green lightweight acid-activated geopolymer mortar, mixing the gel raw materials for 5 minutes, and then adding modified pottery sand and stirring for 5 minutes to obtain a mixture.

[0056] Step S4, injecting the mixture into a mold, covering the top surface with a film, and then putting it into a 40°C steam curing box for high-temperature curing for 24 hours, demolding, and continuing to heat up to 60°C for high-temperature curing for 24 hours to obtain an early mortar test block.

[0057] Step S5, putting the early mortar test block into a fresh-keeping bag, sealing it, and placing it at room temperature for natural curing.

[0058] Example 5

[0059] A modified lightweight aggregate reinforced green lightweight acid-activated geopolymer mortar. The raw materials include the following components in parts by weight: 1.5 kg of 0.08-0.15 mm-diameter pottery sand, 1.5 kg of 0.15-0.315 mm-diameter pottery sand, 3.0 kg of 0.315-0.625 mm-diameter pottery sand, 100.0 kg of metakaolin, 73.3 kg of phosphoric acid, 66.8 kg of water, and 1.2 kg of polycarboxylic acid water reducer.

[0060] The preparation method comprises the following steps:

[0061] Step S1, weighing basic ceramic sand of different particle sizes according to the particle size ratio of the modified lightweight aggregate, washing the ceramic sand in an ultrasonic cleaning machine, replacing clean water every 5 minutes, and washing 5 times in total. Spreading the washed ceramic sand thinly on a sieve, putting it in an electric heating blower and drying it at 60°C for 24 hours until the moisture in the ceramic sand is dried.

[0062] Step S2, soaking the washed and dried pottery sand in phosphoric acid for normal pressure soaking adsorption modification, the normal pressure soaking time is 24 hours. After the soaking, the modified pottery sand is placed in a permeable bag to squeeze and filter out excess phosphoric acid on the surface to obtain modified pottery sand with a relatively dry surface.

[0063] Step S3, weighing various raw materials according to the composition and proportion of the modified lightweight aggregate reinforced green lightweight acid-activated geopolymer mortar, mixing the gel raw materials for 5 minutes, and then adding modified pottery sand and stirring for 5 minutes to obtain a mixture.

[0064] Step S4, injecting the mixture into a mold, covering the top surface with a film, and then putting it into a 40°C steam curing box for high-temperature curing for 24 hours, demolding, and continuing to heat up to 60°C for high-temperature curing for 24 hours to obtain an early mortar test block.

[0065] Step S5, placing the early mortar test block in a vacuum box at room temperature, 95% humidity and 0.04 MPa vacuum degree, and performing negative pressure wet curing.

[0066] Comparative Example 1

[0067] A geopolymer mortar, wherein raw materials include the following components in parts by weight: 1.5 kg of 0.08-0.15 mm-diameter ceramic sand, 1.5 kg of 0.15-0.315 mm-diameter ceramic sand, 3.0 kg of 0.315-0.625 mm-diameter ceramic sand, 100.0 kg of metakaolin, 73.3 kg of phosphoric acid, 66.8 kg of water, and 1.2 kg of polycarboxylic acid water reducer.

[0068] The preparation method comprises the following steps:

[0069] Step S1, weigh basic ceramic sand of different particle sizes according to the particle size ratio, put the ceramic sand into an ultrasonic cleaning machine for cleaning, replace with clean water every 5 minutes, and clean for 5 times in total. Spread the cleaned ceramic sand thinly on a sieve, put it into an electric blower and dry it at 60°C for 24 hours until the moisture of the ceramic sand is dried.

[0070] Step S2, soaking the cleaned and dried pottery sand in water for vacuum soaking adsorption modification, the vacuum negative pressure is controlled at 0.087MPa, and the vacuum soaking time is 24h. After soaking, the modified pottery sand is placed in a water-permeable bag to squeeze and filter out excess water on the surface to obtain modified pottery sand with a relatively dry surface.

[0071] Step S3, weighing various raw materials according to the composition and proportion of the geopolymer mortar, mixing the gel raw material for 5 minutes, and then adding modified pottery sand and stirring for 5 minutes to obtain a mixture.

[0072] Step S4, injecting the mixture into a mold, covering the top surface with a film, and then putting it into a 40°C steam curing box for high-temperature curing for 24 hours, demolding, and continuing to heat up to 60°C for high-temperature curing for 24 hours to obtain an early mortar test block.

[0073] Step S5, placing the early mortar test block in a vacuum box at room temperature, 95% humidity and 0.04 MPa vacuum degree, and performing negative pressure wet curing.

[0074] Comparative Example 2

[0075] A geopolymer mortar is composed of the following raw materials in parts by weight: 100.0 kg of metakaolin, 73.3 kg of phosphoric acid, 66.8 kg of water, and 1.2 kg of a polycarboxylate water reducer.

[0076] The preparation method comprises the following steps:

[0077] Step S1, weighing various raw materials according to the composition and proportion of the geopolymer mortar, mixing and stirring the gel raw materials for 5 minutes to obtain a mixture.

[0078] Step S2, injecting the mixture into a mold, covering the top surface with a film, and then putting it into a 40°C steam curing box for high-temperature curing for 24 hours, demolding, and continuing to heat up to 60°C for high-temperature curing for 24 hours to obtain an early mortar test block.

[0079] Step S3, placing the early mortar test block in a vacuum box at room temperature, 95% humidity and 0.04 MPa vacuum degree, and performing negative pressure wet curing.

[0080] The materials prepared in the above Examples 1 to 5 and Comparative Examples 1 to 2 were subjected to performance tests, and the results are shown in Table 2 below.

[0081] Table 2 Compressive strength and fluidity

[0082]

[0083] From the results in Table 2, it can be seen that the gel used in the present invention belongs to the type of high-strength and lightweight gel, which is 30% to 40% lighter than the mortar in the traditional technology, and the strength can reach the strength grade of ordinary mortar M20 to M35. It can be seen from Examples 1 to 3 that setting a mixed gradation can enhance the strength and fluidity of the material more than a single particle size gradation. It can be seen from Examples 1 and 4 that vacuum curing can make the phosphoric acid inside the pottery sand easier to diffuse outward and diffuse more widely, enhance the "internal pump release" effect of the modified ceramsite, and improve the strength around the interface. The 28d strength increase of Example 1 is about 1.4 times higher than that of Example 4. It can be seen from Examples 1 to 5 that due to the small particle size of pottery sand and more closed pores, vacuum immersion adsorption can increase the acid adsorption amount of pottery sand. The microporous structure of pottery sand causes it to play an "internal pump release" effect inside the mortar, which can continuously provide more phosphoric acid for the reaction, thereby improving the strength. It can be seen from Examples 1 to 5 and Comparative Example 1 that the effect of acid-modified ceramic sand on improving the strength of mortar is better than that of the traditional pre-wetting treatment of ceramic sand. The commonly used pre-wetting method is not applicable to acid-activated polymers because the moisture in the ceramic sand will reduce the acid concentration at the interface, thereby reducing the interface strength. It can be seen from Examples 1 to 5 and Comparative Example 2 that the addition of phosphoric acid-modified ceramic sand can effectively enhance the strength and fluidity of the mortar, among which the effect of vacuum immersion adsorption and setting mixed grading is the best. It can be seen from Comparative Examples 1 to 2 that after high-temperature curing, the material reacts fully, and the unreacted phosphoric acid remains less, so the strength increment in 28 days is small. Similarly, when the modified ceramic sand is added, it plays an "internal pump release" effect, which can provide high-concentration acid in the later stage of the reaction, so that the hydration reaction continues. The strength increment after adding the modified ceramic sand is 2.7 to 9.7 times higher than that without adding.

[0084] When the acid concentration of the acid-excited geopolymer reaction system is high, the material reaction can be more sufficient, but at high acid concentrations, its poor fluidity will affect its working performance and reduce its strength. Therefore, when using a suitable acid concentration (about 6M according to the ratio of the embodiment) and a liquid-solid ratio (about 1.4 according to the ratio of the embodiment), adding acid-soaked modified pottery sand can play the role of "internal pump release", and continuously provide phosphoric acid in the later stage of maintenance, thereby improving the strength. Because the acid-excited geopolymer material has excellent mechanical properties, high temperature stability and corrosion resistance. It can be used to make heat insulation and high temperature resistant fireproof panels, such as subways, tunnels, high-rise buildings and other areas with fire hazards; and can be used in construction projects in areas prone to alkali aggregate reaction, areas eroded by chemical media, and reinforcement, repair and new construction projects of certain buildings damaged by corrosion.

[0085] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing modified lightweight aggregate reinforced green lightweight acid-activated geopolymer mortar, It is characterized in that The following steps are involved: The ceramic sand is placed in phosphoric acid for immersion adsorption modification, and then surface drying is performed to obtain modified ceramic sand; Mix 5 to 10 parts of the modified pottery sand, 98 to 102 parts of metakaolin, 72 to 74 parts of phosphoric acid, 65 to 67 parts of water and 1 to 1.4 parts of a polycarboxylate water reducer by weight to obtain a mixture; The mixture is injected into a mold and steam cured to obtain an early mortar test block; The early mortar test block is placed at room temperature for curing to obtain the modified lightweight aggregate reinforced green lightweight acid-activated geopolymer mortar.

2. The preparation method according to claim 1, It is characterized in that The soaking adsorption modification is carried out under vacuum negative pressure conditions, the negative pressure is controlled at 0.084-0.087 MPa, and the soaking time is 23-25 ​​hours.

3. The preparation method according to claim 1, It is characterized in that The pottery sand is composed of pottery sand with a particle size of 0.08-0.15 mm, pottery sand with a particle size of 0.15-0.315 mm and pottery sand with a particle size of 0.315-0.625 mm.

4. The preparation method according to claim 3, It is characterized in that The mass ratio of the 0.08-0.15 mm-diameter pottery sand, the 0.15-0.315 mm-diameter pottery sand and the 0.315-0.625 mm-diameter pottery sand is 1.5-3:2.5-3.5:4-5.

5. The preparation method according to claim 1, It is characterized in that The steam curing comprises the following steps: injecting the mixed material into the mold and then placing it in a 38-42° C. steam curing box for curing for 23-25 ​​hours, then demolding and continuing to heat up to 58-62° C. for curing for 23-25 ​​hours.

6. The preparation method according to claim 1, It is characterized in that The conditions for curing the early mortar test blocks at room temperature are humidity 92% to 98% and vacuum degree 0.38 to 0.42 MPa.

7. The preparation method according to any one of claims 1 to 6, It is characterized in that Before the soaking adsorption modification, the method further comprises the following steps: ultrasonic cleaning the ceramic sand, and then drying it at 55-65° C. for 22-26 hours.

8. The preparation method according to any one of claims 1 to 6, It is characterized in that The loose bulk density of the ceramic sand is 700-800 kg / m 3 , the saturated water absorption rate is 4.5%.

9. The preparation method according to any one of claims 1 to 6, It is characterized in that The particle size of the metakaolin is 4000-6000 meshes, wherein the weight percentage of silicon dioxide is 54% and the weight percentage of aluminum oxide is 43%.

10. A modified lightweight aggregate reinforced green lightweight acid-activated geopolymer mortar, It is characterized in that Prepared according to the preparation method according to any one of claims 1 to 9.

Citation Information

Cited By

  • Fly ash-based composite sound absorption material and preparation method thereof

    CN122608335A