Novel ablation-resistant gradient composite coating of C / C composite material and preparation method

By designing the gradient composite coating structure of SiC transition inner coating, refractory metal carbide intermediate layer and lanthanum halate outer coating, the problem of mismatch between oxidation and thermal expansion of C/C composite materials at high temperatures is solved, and the super-improvement of super- Improvement of high-temperature ablation resistance and long-term protection of coatings.

CN118878352AActive Publication Date: 2024-11-01CENT SOUTH UNIV

Patent Information

Application Number
CN202410934685.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-01
Estimated Expiration
2044-07-12

AI Technical Summary

Technical Problem

C/C composites have oxidation problems in high temperature environments. The existing antioxidant coating fails at ultra-high temperatures. The lanthanum halate coating does not match the thermal expansion coefficient of the matrix and causes shedding, and is incompatible with carbon, which affects its ablation resistance. performance.

Method used

Design a gradient composite coating structure, consisting of SiC transition inner coating, refractory metal carbide intermediate layer and lanthanum harate outer coating, to alleviate the thermal expansion coefficient gap and chemical physical compatibility problems through the multi-layer structure, and adopt chemical The reaction process and plasma spraying process are prepared to ensure the bonding performance and structural stability of the coating.

Benefits of technology

It significantly improves the ultra-high temperature ablation resistance of C/C composite materials, extends the service life of the coating, ensures that the coating remains integrity and protective effect above 2400℃, and solves the heat of the lanthanum halate coating and the substrate. Matching and chemical compatibility issues.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118878352A_ABST
    Figure CN118878352A_ABST
Patent Text Reader

Abstract

The invention provides a novel ablation-resistant gradient composite coating of a C / C composite material and a preparation method, the gradient composite coating is mainly composed of a SiC transition inner coating, a refractory metal carbide middle layer and a La2Hf2O7 outer coating, and the preparation method comprises the following steps: (1) mixing hafnium oxide and lanthanum oxide powder and granulating; (2) carrying out high-temperature sintering reaction and synthesis on the lanthanum humate spraying powder; (3) high-temperature heat treatment before coating of the C / C composite material; (4) preparing a SiC transition inner coating through a high-temperature chemical reaction process; (5) preparing a refractory metal carbide intermediate layer by a plasma spraying process; and (6) preparing the lanthanum humate outer coating through a plasma spraying process. A new technical approach is provided for long-time ultrahigh-temperature ablation-resistant protection of the C / C composite material, the binding force and the high-temperature structural stability of the gradient coating are integrally enhanced, and the overall anti-scouring performance and the high-temperature protection performance of the gradient coating are further enhanced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of ultra-high temperature corrosion protection, and in particular to a novel ablation-resistant gradient composite coating of a C / C composite material and a preparation method thereof. Background Art

[0002] C / C composite materials have a series of excellent high-temperature properties, such as high high-temperature strength retention, thermal shock resistance, ablation resistance, good high-temperature stability (no melting point, sublimation temperature ≥ 3800℃), etc. In addition, the unique lightweight properties of carbon materials make them an ideal candidate for lightweight thermal structural materials in aerospace, so they are widely used in rocket throat linings, tail nozzles, brake discs, and new generation aircraft nose cones, leading edges and other parts and show great advantages. In addition, carbon materials also have excellent corrosion resistance, so they also have great application potential in high-temperature corrosion protection fields such as machinery, metallurgy, and new energy.

[0003] In a high-temperature oxygen atmosphere, C / C composites begin to oxidize at temperatures above 400°C. As the oxidation temperature increases, the oxidation rate increases, causing its mechanical and thermophysical properties to deteriorate rapidly. In order to improve the high-temperature oxidation resistance of C / C composites, domestic and foreign scholars have invented two methods: antioxidant coating and matrix modification. The matrix modification process improves the oxidation resistance of the carbon matrix to a certain extent, but does not solve the high-temperature oxidation resistance of carbon fibers. Therefore, it has obvious limitations. The antioxidant coating can effectively isolate the direct contact between oxygen and the carbon matrix, thereby fundamentally solving the problem of high-temperature oxidation protection of the carbon matrix and carbon fibers. It is considered to be the most mature and effective antioxidant protection method.

[0004] In recent years, around the high-temperature oxidation resistance and ablation protection of C / C composite materials, domestic and foreign scholars have developed a series of coating systems, including silicide, carbide, boride, precious metal, oxide and glass coating systems, relying on the good high-temperature self-healing properties of silicon oxide or borosilicate glass formed by oxidation, and basically achieved the long-term protection of C / C composite materials below 1600°C. However, with the increase of oxidation temperature, the silicon-based coating begins to change from inert oxidation to active oxidation, and its oxidation product changes from molten silicon oxide to gaseous SiO, resulting in the destruction of the oxide film structure and failure. In order to further improve the oxidation resistance and ablation resistance of C / C composite materials at temperatures above 1800℃, ultra-high temperature ceramic ablation-resistant coatings have been developed. During the ablation process of ultra-high temperature ceramic coatings, the self-healing oxide formed on its surface can adhere to the coating surface, thereby playing a good protective role. However, as the ablation time increases, the liquid phase in the molten oxide phase will be continuously consumed. When the molten liquid phase cannot effectively seal the cracks and holes caused by the phase transformation of high-melting-point zirconium oxide and hafnium oxide in the oxide film, the scouring and invasion of high-temperature gas at the defects will cause the oxide film to peel off and fail, thereby further affecting the improvement of its high-temperature ablation resistance. Therefore, in order to further improve the oxidation resistance and ablation resistance of C / C composite materials above 1800℃, a new type of ablation-resistant coating must be developed.

[0005] Lanthanum halogenate has the advantages of high melting point (≥2420℃) and low thermal conductivity (only 1.34W / mK at 1000℃). As an ablation-resistant coating, it can play an effective role in heat insulation and oxygen barrier. In addition, its excellent high-temperature structural stability is unmatched by other oxide ceramics. From room temperature to melting point, it does not undergo any phase change. Therefore, during the ultra-high temperature ablation process, it can effectively maintain the structural stability and integrity of the coating. Compared with the oxide film formed by ablation of ultra-high temperature ceramic coatings, it has significant structural stability and erosion resistance advantages. Therefore, its application in ablation-resistant coatings can further effectively improve the ultra-high temperature ablation-resistant protection performance of C / C composites (≥2000℃). However, there are few literature reports on the preparation of lanthanum halogenate ablation-resistant coatings.

[0006] Although the lanthanum halogenate coating has excellent oxygen barrier and heat insulation effects and good high-temperature structural stability, as an ablation-resistant coating for C / C composites, the thermal expansion coefficient of the lanthanum halogenate coating is too large (8.76×10 -6 K -1 ), and C / C composite materials (1~2×10 -6 K -1)The thermal expansion coefficients of C / C composites are very different. During the ablation process, the mismatch in thermal expansion coefficients of the two will directly lead to the failure of the coating to fall off. In addition, under high temperature conditions, lanthanum halogenate and carbon are incompatible. The two will react to form carbides, resulting in failure of the coating interface. Therefore, in order to achieve ultra-high temperature protection of C / C composites by lanthanum halogenate coating, it is necessary to solve the problems of thermal matching and chemical and physical compatibility between lanthanum halogenate coating and C / C composites. Summary of the invention

[0007] In order to solve the above problems, the present invention provides a new type of ablation-resistant gradient composite coating of C / C composite material. The gradient composite coating has a gradually increasing linear expansion coefficient from the inside to the outside, and is mainly composed of a SiC transition inner coating, a refractory metal carbide intermediate layer and a lanthanum halogenate (La2Hf2O7) outer coating. The present invention effectively alleviates the ablation of the lanthanum halogenate outer coating (8.76×10 -6 K -1 ) and C / C matrix (1~2×10 -6 K -1 ) The three-layer gradient structure also has the following significant advantages: the silicon carbide transition inner coating prepared by chemical reaction process makes the coating and the substrate have excellent bonding performance, and can effectively hinder the diffusion and penetration of carbon in the substrate to the outer layer; the refractory metal carbide intermediate layer can further alleviate the linear expansion coefficient mismatch problem between the SiC inner coating and the lanthanum halogenate outer coating, further inhibit the diffusion of C in the substrate and O in the outside, and can also play the role of secondary ablation protection barrier; the lanthanum halogenate coating has a high melting point (≥2420℃) and a low thermal conductivity (only 1.34W / mK at 1000℃), which can play the role of oxygen barrier and heat insulation and anti-gas erosion as an outer layer. In addition, the lanthanum halogenate coating also has excellent high-temperature stability. There is no phase change in the process of heating from room temperature to melting point. It has excellent high-temperature structural stability and can still maintain a complete and continuous coating structure during the ablation process. The gradient composite coating structure not only solves the failure problem caused by the mismatch of thermal expansion coefficients between the lanthanum halogenate outer coating and the C / C substrate, but also brings into play the excellent high temperature resistance, heat insulation, oxygen barrier and structural stability of the lanthanum halogenate coating. The construction of the double-layer ablation-resistant coating of the ablation-resistant refractory metal carbide intermediate layer and the lanthanum halogenate outer coating further enhances the long-term ablation-resistant protection life of the gradient coating, and significantly enhances the ablation-resistant performance of traditional ultra-high temperature ceramic coatings. The design and preparation of this new gradient composite coating provides a new technical approach for the long-term ablation-resistant protection of C / C composite materials.

[0008] A method for preparing a novel ablation-resistant gradient composite coating of a C / C composite material comprises the following steps:

[0009] (1) Mixing and granulation of hafnium oxide and lanthanum oxide powders: Before mixing, the hafnium oxide and lanthanum oxide fine powders were dried, and then mixed at a molar ratio of 2:1, and then anhydrous ethanol was added for thorough ball milling. After the ball milling was uniform, granulation and drying were performed. To prevent the granulated powder from absorbing water, the granulated powder was vacuum dried and set aside.

[0010] (2) High-temperature sintering reaction and synthesis of lanthanum halogenate spray powder: The granulated powder dried in (1) is subjected to a high-temperature sintering reaction to prepare lanthanum halogenate spray powder. The high-temperature sintering atmosphere is air or an inert atmosphere. The sintering reaction temperature is 1300-1500°C and the sintering reaction time is 4-10 hours.

[0011] (3) High-temperature heat treatment of C / C composite material before coating: The C / C composite material is placed in a high-temperature furnace for high-temperature hole opening treatment, and then the treated material is machined into a predetermined size and polished with sandpaper, ultrasonically cleaned, and dried for use.

[0012] (4) Preparation of SiC transition inner coating by high temperature chemical reaction process: The heat treated and machined C / C composite material is placed in silicon powder and placed in a graphite crucible together. The graphite crucible containing the C / C sample and silicon powder is then placed in a high temperature furnace and heated to 1700-1900°C for high temperature reaction to prepare the SiC transition inner coating. By controlling the number of high temperature reactions, a SiC transition inner coating with a certain thickness can be obtained.

[0013] (5) Preparation of refractory metal carbide intermediate layer by plasma spraying process: The SiC coating C / C sample in (3) is ultrasonically cleaned and dried, and a refractory metal carbide intermediate layer is prepared by plasma spraying process. By controlling the spraying time and number of times, the thickness of the prepared intermediate layer is maintained in the range of 50 to 120 μm.

[0014] (6) Preparation of lanthanum halogenide outer coating by plasma spraying process: The lanthanum halogenide spray powder in (2) is used as raw material, and the lanthanum halogenide outer coating is prepared by plasma spraying process. By controlling the spraying time and number of times, the thickness of the prepared outer coating is maintained in the range of 120 to 230 μm.

[0015] Furthermore, the novel ablation-resistant gradient composite coating of the C / C composite material has a total coating thickness of 320 to 550 μm.

[0016] Furthermore, in step (5), the refractory metal carbide intermediate layer is two or more of HfC, ZrC, TaC, TiC, NbC, and SiC.

[0017] Furthermore, in step (1), the particle sizes of the hafnium oxide and lanthanum oxide fine powders are both ≤1 μm.

[0018] Furthermore, the particle size of the lanthanum halogenate powder obtained after the sintering reaction in step (2) is 20 to 70 μm.

[0019] Furthermore, the density of the C / C composite material in step (3) is 1.70-1.75 g / cm 3 .

[0020] Furthermore, the high temperature heat treatment temperature in step (3) is 2000-2200° C., and the heat treatment holding time is 0.5-2 h.

[0021] Furthermore, in step (4), when the thickness of the SiC transition inner coating after the first high-temperature reaction is ≤70 μm, a second high-temperature reaction is required to increase its thickness. Preferably, the thickness of the SiC transition inner coating is 70 to 200 μm.

[0022] Furthermore, the process parameters of the plasma spraying process in step (5) are as follows: spraying power is 38-46KW, argon flow rate is 35-55L / min, hydrogen flow rate is 5-12L / min, and spraying distance is 80-120mm.

[0023] Furthermore, the process parameters of the plasma spraying process in step (5) are as follows: spraying power is 35-40KW, argon flow rate is 35-55L / min, hydrogen flow rate is 4-8L / min, and spraying distance is 80-120mm.

[0024] The new gradient composite coating invented by this patent has the following advantages:

[0025] (1) In order to further solve the ablation protection problem of C / C composites above 2000℃, a three-layer coating with a linear expansion coefficient gradient distribution from the inside to the outside was invented. It mainly consists of a SiC transition inner coating, a refractory metal carbide middle layer and a lanthanum halogenate outer coating. The construction of the gradient structure effectively solves the failure problem caused by the mismatch of the linear expansion coefficient between the lanthanum halogenate coating and the C / C substrate, and gives full play to the excellent oxygen barrier and heat insulation and good high-temperature structural stability advantages of the lanthanum halogenate outer coating. After 2400℃ oxyacetylene ablation for 60s, the lanthanum halogenate outer coating is intact and the layers of the coating are well bonded, indicating that it has the potential for ultra-high temperature and long-term ablation resistance, providing a new technical approach for long-term ultra-high temperature ablation resistance of C / C composites.

[0026] (2) By designing different transition layers, intermediate layers and outer coatings, a thick (320-550 μm) ablation-resistant multilayer gradient composite coating was prepared. On the basis of constructing a double-layer carbide transition layer and intermediate layer, the high-temperature chemical and physical compatibility problem between the lanthanum carbide coating and the C / C matrix was effectively solved. In addition, the SiC thick coating prepared by chemical reaction process effectively solved the bonding problem of the gradient ultra-thick coating, and overall enhanced the bonding strength and high-temperature structural stability of the gradient coating.

[0027] (3) According to the spraying characteristics of refractory metal carbide coating and lanthanum halogenate coating, a differential spraying process is adopted to prepare a refractory metal carbide intermediate layer and a lanthanum halogenate outer coating. When spraying the intermediate layer, the protective gas hydrogen flow rate is appropriately increased to reduce the content of the oxidized phase in the refractory metal carbide coating, thereby improving the temperature resistance and structural stability of the overall coating. During the spraying process, there is no oxidation of lanthanum halogenate, so the structure of the lanthanum halogenate oxide outer layer obtained by spraying is denser, further enhancing the overall anti-erosion performance of the gradient coating. In addition, the prepared refractory metal carbide intermediate layer and lanthanum halogenate outer layer provide a double-layer protective barrier for the ultra-high temperature ablation resistance of the C / C composite material, further improving its high temperature protection performance and service life. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 The XRD pattern of the outermost lanthanum hafnate coating of the La2Hf2O7 / ZrC-SiC / SiC gradient coating prepared in Example 1;

[0029] Figure 2 This is a surface microscopic morphology of the La2Hf2O7 / ZrC-SiC / SiC gradient coating prepared in Example 1;

[0030] Figure 3 The cross-sectional microstructure and element surface scanning analysis results of the La2Hf2O7 / ZrC-SiC / SiC gradient coating prepared in Example 1;

[0031] Figure 4 This is a photo of the La2Hf2O7 / ZrC-SiC / SiC gradient coating prepared in Example 1 after ablation;

[0032] Figure 5 The surface temperature variation curve of the La2Hf2O7 / ZrC-SiC / SiC gradient coating prepared in Example 1 during oxyacetylene flame ablation for 60 seconds;

[0033] Figure 6 XRD patterns of the La2Hf2O7 / ZrC-SiC / SiC gradient coating prepared in Example 1 after ablation for different times;

[0034] Figure 7The surface microstructure of the central area of ​​the La2Hf2O7 / ZrC-SiC / SiC gradient coating prepared in Example 1 after ablation at different times;

[0035] Figure 8 The cross-sectional morphology and elemental surface scanning analysis results of the ablation center area, transition area and edge area of ​​the La2Hf2O7 / ZrC-SiC / SiC gradient coating prepared in Example 1;

[0036] Fig. 9 The cross-sectional microstructure and element surface scanning analysis results of the La2Hf2O7 / ZrC-TaC / SiC gradient coating prepared in Example 2;

[0037] Fig.10 This is a photo of the La2Hf2O7 / ZrC-TaC / SiC gradient coating prepared in Example 2 after ablation for 30 seconds; Fig.11 The surface microstructure of the La2Hf2O7 / ZrC-TaC / SiC gradient coating prepared in Example 2 after ablation for 30 seconds;

[0038] Fig.12 The cross-sectional microstructure and element surface scanning analysis results of the La2Hf2O7 / ZrC-HfC / SiC gradient coating prepared in Example 3;

[0039] Fig.13 This is a photo of the La2Hf2O7 / ZrC-HfC / SiC gradient coating prepared in Example 3 after ablation for 30 seconds; Fig.14 This is the surface micromorphology of the La2Hf2O7 / ZrC-HfC / SiC gradient coating prepared in Example 3 after ablation for 30 seconds. DETAILED DESCRIPTION

[0040] Example 1: Dry hafnium oxide and lanthanum oxide fine powders with a particle size of 1 μm, then mix the two at a molar ratio of 2:1, and then add anhydrous ethanol for thorough ball milling. After ball milling and mixing evenly, granulation and drying are performed. To prevent the granulated powder from absorbing water, the granulated powder is vacuum dried and set aside. The dried granulated powder is subjected to a high-temperature sintering reaction at 1350°C to prepare lanthanum hafnium oxide spray powder. The high-temperature sintering atmosphere is an inert atmosphere, and the sintering reaction time is 5 hours. After sintering, the particle size of the lanthanum hafnium oxide spray powder obtained is 20 to 61 μm. The density is selected to be 1.70 g / cm 3 The needle-punched C / C composite material was subjected to a high temperature heat treatment at 2000℃ for 2h, and then the treated material was machined into φ30×10mm 3The disc sample is polished with sandpaper, ultrasonically cleaned and dried for later use. The heat-treated and machined C / C composite material is placed in silicon powder and placed in a graphite crucible together. The graphite crucible containing the C / C sample and silicon powder is then placed in a high-temperature furnace and heated to 1900°C for high-temperature reaction to prepare a SiC transition inner coating. The high-temperature reaction time is 1 hour. The prepared SiC coating sample is subjected to a secondary high-temperature reaction, and the thickness of the prepared SiC transition inner coating is in the range of 70 to 150 μm.

[0041] The prepared SiC coating C / C sample was ultrasonically cleaned and dried, and the ZrC-SiC composite spray powder was used as the raw material (mass ratio was 5:1), and the ZrC-SiC intermediate layer was prepared by plasma spraying. The process parameters of ion spraying were as follows: spraying power was 38-46KW, argon flow rate was 35-55L / min, hydrogen flow rate was 5-12L / min, and spraying distance was 100mm. By controlling the spraying time and number of times, the thickness of the prepared ZrC-SiC intermediate layer was kept in the range of 50-100μm. The prepared lanthanum hafnium oxide spray powder was used as the raw material, and the lanthanum hafnium oxide outer coating was prepared on the surface of the ZrC-SiC intermediate layer by plasma spraying. The ion spraying process parameters were as follows: spraying power was 35-40KW, argon flow rate was 35-55L / min, hydrogen flow rate was 4-8L / min, and spraying distance was 100mm. By controlling the spraying time and number of times, the thickness of the prepared outer coating is maintained within the range of 150 to 200 μm.

[0042] Figure 1 This is the XRD spectrum of the outermost coating of the La2Hf2O7 / ZrC-SiC / SiC gradient coating prepared in Example 1. From the phase analysis results, it can be seen that only the diffraction peak of lanthanum hafnium oxide appears on the surface of the coating, indicating that the prepared coating is pure in phase and has no other impurities. At the same time, it shows that the prepared lanthanum hafnium oxide outer coating has a dense structure and a certain thickness, and X-rays cannot penetrate the outer coating.

[0043] Figure 2 This is the surface microscopic morphology of the La2Hf2O7 / ZrC-SiC / SiC gradient coating prepared in Example 1. It can be seen that the outermost lanthanum hafnium oxide coating presents a typical plasma sprayed coating morphology, which is mainly composed of a completely molten phase and particles that are not fully melted during the spraying process.

[0044] Figure 3The cross-sectional microstructure and element surface scanning analysis results of the La2Hf2O7 / ZrC-SiC / SiC gradient coating prepared in Example 1. It can be seen from the element surface scanning analysis results that the coating forms a SiC transition layer, a ZrC-SiC intermediate layer and a La2Hf2O7 outer coating from the inside to the outside, and their thicknesses are 100-150μm, 50-100μm, and 150-210μm, respectively. It can be seen that the interface characteristics between the three layers of coating, the SiC layer, the ZrC-SiC layer and the La2Hf2O7 outer layer, are relatively obvious. Since the surface of the SiC layer formed by high-temperature chemical reaction is relatively rough, the ZrC-SiC coating after spraying can form a jagged structure with the SiC layer, ensuring good bonding between the coatings; in addition, the La2Hf2O7 outer layer and the ZrC-SiC intermediate layer are also tightly bonded, and no obvious cracks, pores and other defects are formed at the interface between the two. Since the linear expansion coefficients of SiC, ZrC, and La2Hf2O7 are 4.5, 6.7, and 8.76×10 -6 K -1 Therefore, from the inside to the outside, the linear expansion coefficient of the multilayer coating presents a gradient distribution characteristic.

[0045] After 30s of oxyacetylene flame ablation, the mass ablation rate and line ablation rate of the La2Hf2O7 / ZrC-SiC / SiC gradient coating prepared in Example 1 were -0.53mg / s and -11.30μm / s, respectively. When the ablation time was further extended to 60s, the mass ablation rate and line ablation rate were 1.12mg / s and 6.79μm / s, respectively, indicating that it has excellent high-temperature ablation resistance.

[0046] Figure 4 The following are photos of the La2Hf2O7 / ZrC-SiC / SiC gradient coating prepared in Example 1 after oxyacetylene ablation for different times. Figure 4 From the actual photo after ablation for 30 seconds, it can be seen that after ablation, the color in the center of the coating is the darkest, and the color becomes lighter and lighter towards the edge, close to the bright white color when sprayed. Obviously different from the ultra-high temperature coating, the surface of the coating after ablation is dense, smooth and flat, with no obvious bulges and peeling marks, and the integrity of the coating structure is maintained macroscopically. Figure 4 b is a photo of the object after 60s of ablation. The surface of the coating in the ablation center area is transparent and molten glass, indicating that the surface phase is close to melting. After ablation, the coating as a whole does not show obvious peeling, convexity and concave state, and the surface still maintains a complete structural morphology, further indicating that the coating has good high-temperature structural stability and long-term ablation resistance potential.

[0047] Figure 5The surface temperature variation curve of the La2Hf2O7 / ZrC-SiC / SiC gradient coating prepared in Example 1 during oxyacetylene flame ablation for 60 seconds. It can be observed that the surface temperature rises sharply from about 1300°C to 2200°C, and then rises slowly, with the highest temperature reaching 2414°C. During the ablation process, the outer layer of lanthanum hafnium oxide still maintains a good structural morphology, indicating that it still has good structural stability under ultra-high temperature conditions of 2400°C.

[0048] Figure 6 XRD patterns of the La2Hf2O7 / ZrC-SiC / SiC gradient coating prepared in Example 1 after ablation for different times. The phase analysis results show that after ablation for different times, the phase of the outer coating remains consistent with that during spraying, which is the La2Hf2O7 phase. Under an oxyacetylene flame at a temperature exceeding 2400°C, the phase of the La2Hf2O7 coating still does not undergo significant changes, further demonstrating its excellent high-temperature structural stability.

[0049] Figure 7 The surface microstructure of the central area of ​​the La2Hf2O7 / ZrC-SiC / SiC gradient coating prepared in Example 1 after ablation at different times. Figure 7 It can be seen from Figure 1 that after 30s of ablation, the surface of the La2Hf2O7 coating is still smooth and dense, and the overall morphology before spraying is basically maintained. Figure 7 b is the surface morphology after 60s of ablation. As the ablation time increases, more molten phases appear on the surface of the La2Hf2O7 coating. Under the long-term scouring of the oxyacetylene flame, the molten phase flows on the surface to fill the defects and form a denser coating morphology.

[0050] Figure 8 The cross-sectional micromorphology and elemental surface scanning analysis results of the ablation center area, transition area and edge area of ​​the La2Hf2O7 / ZrC-SiC / SiC gradient coating prepared in Example 1. Figure 8 a is the cross-sectional morphology of the ablation center area. It can be seen that the overall structure of the La2Hf2O7 outer coating is intact, and the structure of the intermediate layer and the transition inner coating has hardly changed. In addition, the interface between the coating layers is still tightly bonded, indicating that it has good bonding performance. Although obvious extended cracks appeared in the La2Hf2O7 outer coating, in the transition ( Figure 8 b) and marginal areas ( Figure 8c), the La2Hf2O7 outer coating and the ZrC-SiC intermediate layer interface are still tightly bonded, indicating that it has good structural integrity. Since the La2Hf2O7 outer coating is relatively brittle, during the sample mounting and repeated grinding process, external forces will have a certain degree of destructive effect on the coating structure, resulting in a certain number of cracks. In addition, in view of the fact that part of the lanthanum hafnium oxide molten phase formed during the ablation process has a self-healing effect and can effectively flow and seal cracks and other defects, the appearance of cracks in the La2Hf2O7 outer coating is mainly related to the external force damage to the coating caused by the sample mounting and grinding process, rather than being formed during the ablation process. At the same time, the element surface scanning analysis results also confirmed that ( Figure 8 d), after 60s of ablation, almost no oxygen element appears in the ZrC-SiC intermediate layer and the SiC transition inner coating, which further shows that the La2Hf2O7 outer coating has a good oxygen barrier and heat insulation effect, and can effectively protect the intermediate and inner coatings. Since the ZrC-SiC intermediate layer and the SiC transition inner coating also have good ablation resistance and protection capabilities, in the later stage of ablation, assuming that the La2Hf2O7 outer coating fails due to ablation, it can also serve as a second layer of ablation protection barrier. Therefore, the new ablation-resistant coating designed and prepared by the present invention has good long-term ablation resistance potential, and provides a new technical approach for ultra-high temperature and long-term ablation resistance protection of C / C composite materials.

[0051] Example 2: Dry hafnium oxide and lanthanum oxide fine powders with a particle size of 1 μm, then mix the two at a molar ratio of 2:1, and then add anhydrous ethanol for thorough ball milling. After ball milling and mixing evenly, granulation and drying are performed. To prevent the granulated powder from absorbing water, the granulated powder is vacuum dried and set aside. The dried granulated powder is subjected to a high-temperature sintering reaction at 1350°C to prepare lanthanum hafnium oxide spray powder. The high-temperature sintering atmosphere is an inert atmosphere, and the sintering reaction time is 5 hours. After sintering, the particle size of the lanthanum hafnium oxide spray powder obtained is 20 to 61 μm. The density is selected to be 1.70 g / cm 3 The needle-punched C / C composite material was subjected to a high temperature heat treatment at 2000℃ for 2h, and then the treated material was machined into φ30×10mm 3 The disc sample is polished with sandpaper, ultrasonically cleaned and dried for later use. The heat-treated and machined C / C composite material is placed in silicon powder and placed in a graphite crucible together. The graphite crucible containing the C / C sample and silicon powder is then placed in a high-temperature furnace and heated to 1800-1850°C for high-temperature reaction to prepare a SiC transition inner coating. The high-temperature reaction time is 1 hour. The prepared SiC coating sample is subjected to a secondary high-temperature reaction, and the thickness of the prepared SiC transition inner coating is in the range of 70-100 μm.

[0052] The prepared SiC coating C / C sample was ultrasonically cleaned and dried, and the ZrC-TaC intermediate layer was prepared by plasma spraying process using ZrC-TaC spray powder as raw material (mass ratio of 2:1). The process parameters of ion spraying were as follows: spraying power of 38-46KW, argon flow rate of 35-55L / min, hydrogen flow rate of 5-12L / min, and spraying distance of 100mm. By controlling the spraying time and number of times, the thickness of the prepared ZrC-TaC intermediate layer was kept in the range of 80-120μm. Using the prepared lanthanum hafnium oxide spray powder as raw material, the lanthanum hafnium oxide outer coating was prepared on the surface of the ZrC-TaC intermediate layer by plasma spraying process. The ion spraying process parameters were as follows: spraying power of 35-40KW, argon flow rate of 35-55L / min, hydrogen flow rate of 4-8L / min, and spraying distance of 100mm. By controlling the spraying time and number of times, the thickness of the prepared outer coating is maintained within the range of 150 to 200 μm.

[0053] Fig. 9 The cross-sectional microstructure and elemental surface scanning analysis results of the La2Hf2O7 / ZrC-TaC / SiC gradient coating prepared in Example 2. As can be seen from the figure, the thicknesses of the prepared SiC transition layer, ZrC-TaC intermediate layer and La2Hf2O7 outer coating are 70-100μm, 80-120μm and 150-200μm respectively. It can be seen that the interface between the three coatings is obvious and tightly bonded. Since the linear expansion coefficients of SiC, ZrC, TaC and La2Hf2O7 are 4.5, 6.7, 7.08 and 8.76×10 -6 K -1 Therefore, from the inside to the outside, the linear expansion coefficient of the multilayer coating presents a gradient distribution characteristic.

[0054] The La2Hf2O7 / ZrC-TaC / SiC gradient coating prepared in Example 2 was tested for oxyacetylene ablation resistance. After 30 seconds of ablation, the linear ablation rate and mass ablation rate of the coating were -0.41 mg / s and 10.30 μm / s, respectively. The negative mass ablation rate indicated that it had good high-temperature ablation resistance.

[0055] Fig.10 This is a photo of the La2Hf2O7 / ZrC-TaC / SiC gradient coating prepared in Example 2 after oxyacetylene ablation for 30 seconds. As can be seen from the figure, the coating surface is relatively smooth and dense after ablation, without obvious protrusions and peeling marks, and the macroscopic structure is still intact, indicating that it has good ablation resistance and anti-gas erosion performance.

[0056] Fig.11The surface microstructure of the La2Hf2O7 / ZrC-TaC / SiC gradient coating prepared in Example 2 after oxyacetylene ablation for 30 seconds. Fig.11 a), transition zone ( Fig.11 b) and marginal areas ( Fig.11 c), the surface of the La2Hf2O7 coating maintains a similar morphology to that before spraying, the overall structure is relatively continuous and dense, and the grain sizes in different areas have certain differences. Since the temperature in the ablation center is the highest and the temperature in the edge is the lowest, the grain sizes in the ablation center and edge are the largest and smallest, respectively. Under the continuous scouring of the oxyacetylene flame, the La2Hf2O7 grain structure on the surface is undulating, and there are no obvious ablation pits and pore structures, indicating that the coating has excellent high-temperature structural stability.

[0057] Example 3: Dry hafnium oxide and lanthanum oxide fine powders with a particle size of 1 μm, then mix the two at a molar ratio of 2:1, and then add anhydrous ethanol for thorough ball milling. After ball milling and mixing evenly, granulation and drying are performed. To prevent the granulated powder from absorbing water, the granulated powder is vacuum dried and set aside. The dried granulated powder is subjected to a high-temperature sintering reaction at 1350°C to prepare lanthanum hafnium oxide spray powder. The high-temperature sintering atmosphere is an inert atmosphere, and the sintering reaction time is 5 hours. After sintering, the particle size of the lanthanum hafnium oxide spray powder obtained is 20 to 61 μm. The density is selected to be 1.70 g / cm 3 The needle-punched C / C composite material was subjected to a high temperature heat treatment at 2000℃ for 2h, and then the treated material was machined into φ30×10mm 3 The disc sample is polished with sandpaper, ultrasonically cleaned and dried for later use. The heat-treated and machined C / C composite material is placed in silicon powder and placed in a graphite crucible together. The graphite crucible containing the C / C sample and silicon powder is then placed in a high-temperature furnace and heated to 1900°C for high-temperature reaction to prepare a SiC transition inner coating. The high-temperature reaction time is 1 hour. The prepared SiC coating sample is subjected to a secondary high-temperature reaction, and the thickness of the prepared SiC transition inner coating is in the range of 80 to 120 μm.

[0058] The prepared SiC coating C / C sample was ultrasonically cleaned and dried, and the ZrC-HfC spray powder was used as the raw material (mass ratio was 1:1), and the ZrC-HfC intermediate layer was prepared by plasma spraying. The process parameters of ion spraying were as follows: spraying power was 38-46KW, argon flow rate was 35-55L / min, hydrogen flow rate was 5-12L / min, and spraying distance was 100mm. By controlling the spraying time and number of times, the thickness of the prepared ZrC-HfC intermediate layer was kept in the range of 70-100μm. The prepared lanthanum hafnium oxide spray powder was used as the raw material, and the lanthanum hafnium oxide outer coating was prepared on the surface of the ZrC-HfC intermediate layer by plasma spraying. The ion spraying process parameters were as follows: spraying power was 35-40KW, argon flow rate was 35-55L / min, hydrogen flow rate was 4-8L / min, and spraying distance was 100mm. By controlling the spraying time and number of times, the thickness of the prepared outer coating is maintained in the range of 120 to 150 μm.

[0059] Fig.12 The cross-sectional microstructure and elemental surface scanning analysis results of the La2Hf2O7 / ZrC-HfC / SiC gradient coating prepared in Example 3. As can be seen from the figure, the thicknesses of the prepared SiC transition layer, ZrC-HfC intermediate layer and La2Hf2O7 outer coating are 80-120μm, 70-100μm and 120-150μm respectively. It can be seen that the interface between the three coating layers is obvious and tightly bonded. Since the linear expansion coefficients of SiC, ZrC, TaC and La2Hf2O7 are 4.5, 6.7, 7.66 and 8.76×10 -6 K -1 Therefore, from the inside to the outside, the linear expansion coefficient of the multilayer coating presents a gradient distribution characteristic.

[0060] The La2Hf2O7 / ZrC-HfC / SiC gradient coating prepared in Example 3 was tested for its oxyacetylene ablation resistance. After 30 seconds of ablation, the linear ablation rate and mass ablation rate of the coating were 8.21 mg / s and 10.70 μm / s, respectively, indicating that the coating has a relatively low ablation rate.

[0061] Fig.13 This is a photo of the La2Hf2O7 / ZrC-HfC / SiC gradient coating prepared in Example 3 after 30s of oxyacetylene ablation. It can be seen that after 30s of ablation, the coating is smooth and dense as a whole, and has no obvious protrusions or peeling marks, indicating that its structure is intact.

[0062] Fig.14 This is the surface microscopic morphology of the La2Hf2O7 / ZrC-HfC / SiC gradient coating prepared in Example 3 after ablation for 30 seconds. Fig.14 a) Transition zone ( Fig.14 b) and marginal areas ( Fig.14 The La2Hf2O7 coating of c) still maintains the structural morphology at the time of spraying. Although the local grains have grown to a certain extent, the coating is continuous and dense as a whole, and there are no defects such as cracks and holes on the surface, indicating that it has high high-temperature stability and can provide good protection against ablation and gas erosion.

[0063] This specific embodiment is merely an explanation of the present invention and is not a limitation of the present invention. After reading this specification, those skilled in the art may make non-creative modifications to the present embodiment as needed. However, as long as they are within the scope of the claims of the present invention, they are protected by the patent law.

Claims

1. A new type of ablation-resistant gradient composite coating of C / C composite material, characterized in that: The gradient composite coating is composed of a SiC transition inner coating, a refractory metal carbide intermediate layer and a lanthanum halogenate (La2Hf2O7) outer coating, and its linear expansion coefficient increases gradually from the inside to the outside.

2. A method for preparing a new type of gradient composite coating resistant to ablation of C / C composite materials, characterized in that: The following steps are involved: (1) Mixing and granulating hafnium oxide and lanthanum oxide powders: Before mixing, the hafnium oxide and lanthanum oxide fine powders are first dried, and then mixed at a molar ratio of 2:1, and then anhydrous ethanol is added to perform sufficient ball milling. After the ball milling is uniformly mixed, granulation and drying are performed. In order to prevent the granulated powder from absorbing water, the granulated powder is vacuum dried and set aside; (2) High-temperature sintering reaction and synthesis of lanthanum halogenate spray powder: The granulated powder dried in (1) is subjected to a high-temperature sintering reaction to prepare lanthanum halogenate spray powder. The high-temperature sintering atmosphere is air or an inert atmosphere. The sintering reaction temperature is 1300 to 1500° C. and the sintering reaction time is 4 to 10 hours. (3) High temperature heat treatment of C / C composite material before coating: the C / C composite material is placed in a high temperature furnace for high temperature hole opening treatment, and then the treated material is machined into a predetermined size, polished with sandpaper, ultrasonically cleaned and dried for use; (4) Preparation of SiC transition inner coating by high temperature chemical reaction process: The heat treated and machined C / C composite material is placed in silicon powder and placed in a graphite crucible together. The graphite crucible containing the C / C sample and silicon powder is then placed in a high temperature furnace and heated to 1700-1900°C for high temperature reaction to prepare the SiC transition inner coating. By controlling the number of high temperature reactions, a SiC transition inner coating with a certain thickness is obtained. (5) Preparation of refractory metal carbide intermediate layer by plasma spraying process: The SiC coating C / C sample in (3) is ultrasonically cleaned and dried, and a refractory metal carbide intermediate layer is prepared by plasma spraying process. By controlling the spraying time and number of times, the thickness of the prepared intermediate layer is kept in the range of 50 to 120 μm; (6) Preparation of lanthanum halogenide outer coating by plasma spraying process: The lanthanum halogenide spray powder in (2) is used as raw material, and the lanthanum halogenide outer coating is prepared by plasma spraying process. By controlling the spraying time and number of times, the thickness of the prepared outer coating is maintained in the range of 120 to 230 μm.

3. The method for preparing a novel ablation-resistant gradient composite coating of a C / C composite material according to claim 2, characterized in that: The novel ablation-resistant gradient composite coating of C / C composite material has a total coating thickness of 320 to 550 μm.

4. The method for preparing a novel ablation-resistant gradient composite coating of a C / C composite material according to claim 2, characterized in that: The refractory metal carbide intermediate layer is two or more of HfC, ZrC, TaC, TiC, NbC and SiC.

5. The method for preparing a novel ablation-resistant gradient composite coating of a C / C composite material according to claim 2, characterized in that: The hafnium oxide and lanthanum oxide fine powders described in (1) have a particle size of ≤1 μm.

6. The method for preparing a novel ablation-resistant gradient composite coating of a C / C composite material according to claim 2, characterized in that: (2) The particle size of the lanthanum halogenate powder obtained after the sintering reaction is 20 to 70 μm.

7. The method for preparing a novel ablation-resistant gradient composite coating of a C / C composite material according to claim 2, characterized in that: The density of the C / C composite material described in (3) is 1.70-1.75 g / cm 3 ; The high temperature heat treatment temperature described in (3) is 2000~2200℃, and the heat treatment holding time is 0.5~2h.

8. The method for preparing a novel ablation-resistant gradient composite coating of a C / C composite material according to claim 2, characterized in that: The SiC transition inner coating described in (4) needs to undergo a secondary high temperature reaction to increase its thickness when the thickness of the coating after the primary high temperature reaction is ≤70 μm. The preferred thickness of the SiC transition inner coating is 70 to 200 μm.

9. The method for preparing a novel ablation-resistant gradient composite coating of a C / C composite material according to claim 2, characterized in that: The plasma spraying process described in (5) has the following process parameters: spraying power is 38-46KW, argon flow rate is 35-55L / min, hydrogen flow rate is 5-12L / min, and spraying distance is 80-120mm.

10. The method for preparing a novel ablation-resistant gradient composite coating of a C / C composite material according to claim 2, characterized in that: The plasma spraying process described in (6) has the following process parameters: spraying power is 35-40KW, argon flow rate is 35-55L / min, hydrogen flow rate is 4-8L / min, and spraying distance is 80-120mm.

Citation Information

Patent Citations

  • C / C composite material superhigh temperature ceramic coating, and preparation method thereof

    CN108530110A

  • Thermal shock and thermal shock resistant thermal / environmental barrier coating and preparation method thereof

    CN116716570A

  • Rare earth hafnate coating structure and preparation method thereof

    CN117107187A

  • Carbon fiber-reinforced composite material

    EP0435039A1

  • CMAS mitigation compositions, environmental barrier coatings comprising the same, and ceramic components comprising the same

    US20100158680A1

Cited By

  • Method for rapidly preparing SiO2 coating on surface of C / C composite material

    CN120818785A

  • A method for rapidly preparing a SiO2 coating on a C / C composite material surface

    CN120818785B