Branched thioether dispersing agent as well as preparation and application thereof
Through the preparation method of branched sulfide ether dispersant, the lengthy and wastewater problems of the pigment dispersant preparation process in the prior art are solved, and the efficient preparation of nano-scale pigments and high-contrast color filters and photoresist are realized, satisfying the The performance requirements of the modern display industry.
Patent Information
- Application Number
- CN202410917771.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-01
AI Technical Summary
The preparation process of existing pigment dispersants is lengthy and complicated, with many side reactions, high energy consumption and large amounts of wastewater, which limits the contrast and application potential of color filters and photoresist.
Using the preparation method of branched sulfide ether dispersant, a monomer with branched or long-chain carbon-carbon unsaturated bond and a thiol compound are catalyzed under heating and alkaline conditions through click chemical reaction to obtain branched sulfide ether Dispersants and are added during pigment synthesis to control particle size and inhibit crystal growth.
The efficient preparation of nanoscale organic pigments is achieved, the dispersion and particle size uniformity of pigments are improved, the contrast, transmittance and color saturation of color filters and photoresist are improved, and the manufacturing cost and environmental pollution are reduced.
Smart Images

Figure BDA0004935657530000031 
Figure BDA0004935657530000032 
Figure BDA0004935657530000041
Abstract
Description
Technical Field
[0001] The invention relates to a branched sulfide dispersant and preparation and application thereof, belonging to the technical field of photoresists. Background Art
[0002] With the continuous advancement of technology and the continuous expansion of applications in the fields of aerospace, automobiles, electronics, chemicals, and medicine, the demand for high-tech new materials has become more and more extensive. Among them, dispersants, as additives in the new materials industry, play an important role in research and development and production.
[0003] At present, in the field of coloring materials, such as coatings, printing inks, fiber colorants, and inkjet toners, the required pigment particle size is mostly measured in microns; while for products such as color filters and photoresists, the required pigment particle size is measured in nanometers. However, the conventional pigment synthesis method is limited by its synthesis method and post-processing method, resulting in a relatively low contrast of the color filter, which limits its application.
[0004] The Chinese invention patent application with publication number CN1487852A provides a dendritic structure dispersant with Boltorn dendritic polyester as the core and a large number of pigment affinity groups such as amino, hydroxyl, carboxyl, phosphoric acid, sulfonic acid and nitrogen-containing heterocyclic groups as the exterior. The dendritic structure external groups form affinity with the pigment and are used to disperse the pigment. During the synthesis of the dispersant, a high temperature of 170°C is used for the esterification reaction, and the reaction temperature is high, so the reaction is prone to many side reactions and the energy consumption is high.
[0005] The Chinese invention patent with the announcement number CN101117450B provides a method of reacting a hydrophobic hyperbranched structure of polyester, polyurethane, polyamine, polyamide, polyurea, etc. with a diisocyanate binder and a hydrophilic chain to obtain a solid dispersant, and compounding it with other dispersants to modify the pigment to obtain a nano-scale organic pigment with high solid content, good fluidity, high stability and bright color. However, the synthesis process of the dispersant is lengthy and complicated, and a large amount of wastewater containing VOCs will be generated, which increases the manufacturing cost and the risk of environmental pollution. Summary of the invention
[0006] Aiming at the defects of the existing pigment dispersant preparation process being lengthy and complicated, with many side reactions and a large amount of wastewater, the present invention provides a branched sulfide dispersant and a preparation method and application thereof.
[0007] The technical solution of the present invention to solve the above technical problems is as follows:
[0008] One of the purposes of the present invention is to provide a method for preparing a branched sulfide dispersant, wherein a monomer having a branched or long-chain carbon-carbon unsaturated bond is added to a solvent, and a catalyst and a thiol compound are added under heating and alkaline conditions, and under the catalytic action of the catalyst, the monomer having a branched or long-chain carbon-carbon unsaturated bond and the thiol compound undergo a click chemical reaction to obtain the branched sulfide dispersant.
[0009] The beneficial effects of the present invention are:
[0010] The preparation method of the branched thioether dispersant provided by the present invention takes a monomer with an unsaturated bond having a double bond structure as the core, utilizes the characteristic that a thiol bond can undergo a click chemical reaction with a double bond, and synthesizes a series of dispersants capable of improving the particle size of organic pigment particles at the molecular level. Through further surface grafting reaction in the compounding process, the embedding effect of the dispersant on the pigment particles can be adjusted, and the dispersibility of the pigment particles in the system can be improved. The dispersed nano-organic pigment of the present invention can be applied to advanced display industries such as color filters and photoresists. The obtained product pigment is compounded with a (methyl) acrylate adhesive to obtain a color photoresist, and the hydrophilic and hydrophobic properties of the pigment can be adjusted to meet the performance requirements of the color filter formula such as high transmittance, high contrast ratio, easy processing, high color saturation, precise color point, thermal stability, etc.
[0011] The pigment dispersants in the prior art are mainly added in the post-treatment of the pigment synthesis product. The branched sulfide dispersant obtained by the preparation method of the branched sulfide dispersant provided by the present invention can be directly added in the synthesis reaction of the pigment without participating in the reaction, and can control the primary particle size of the product to be at the nanometer level, thereby inhibiting crystal growth. Therefore, it is also a crystal growth inhibitor.
[0012] On the basis of the above technical solution, the present invention can also make the following improvements:
[0013] Furthermore, the monomer having branched or long-chain carbon-carbon unsaturated bonds is selected from aliphatic compounds and their derivatives or (heterocyclic) aromatic compounds and their derivatives.
[0014] Furthermore, the aliphatic compound and its derivatives are selected from the following general formula I:
[0015]
[0016] Where n is an integer ≥ 1,
[0017] R1, R2, and R3 are independently selected from hydrogen atoms, methyl groups, C2-C20 alkyl groups and their derivatives, or aromatic rings and their derivatives, or propylene oxide groups, or heterocyclic structure derivatives containing O, N or S elements, or alicyclic groups and their derivatives,
[0018] R4 is methyl or hydrogen,
[0019] X is one of O, N or S elements.
[0020] Furthermore, the aliphatic compound and its derivatives are selected from any one or two or more of ethylene glycol di(meth)acrylate, trimethylolpropane trimethacrylate, pentaerythritol (meth)acrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol (meth)acrylate, dipentaerythritol di(meth)acrylate, dipentaerythritol tri(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, tri(acryloyloxyethyl) isocyanurate, diethanol diglycerol acrylate, 1,3-diglycerol alcohol diacrylate, and ethanolamine (meth)acrylate.
[0021] Furthermore, the (heterocyclic) aromatic compound and its derivatives are selected from the following general formula II:
[0022]
[0023] Wherein, m is an integer ≥ 1,
[0024] R4 is methyl or hydrogen,
[0025] R5, R6, R7, R8, and R9 are independently selected from hydrogen atoms, methyl groups, C2-C20 alkyl groups and their derivatives, or aromatic rings and their derivatives, or propylene oxide groups, or heterocyclic structure derivatives containing O, N or S elements, or alicyclic groups and their derivatives.
[0026] X is one of O, N or S elements,
[0027] Y is C, or one or two of O, N or S elements.
[0028] Furthermore, the (heterocyclic) aromatic compound and its derivatives are selected from one or two or more of 1,3,5-dihydroxyphenol (meth)acrylate, o-diphenol di(meth)acrylate, o-benzyl di(meth)acrylate, iso-benzyl tri(meth)acrylate, 1,3,5-trihydroxyphenol tri(meth)acrylate, 1,3,5-trihydroxyphenol di(meth)acrylate, iso-benzyl trimethylacrylate, o-benzyl di(meth)acrylate, iso-benzyl tri(meth)acrylate, 1,3,5-trihydroxyphenol di(meth)acrylate, iso-benzyl trimethylacrylate, o-benzylamide di(meth)acrylate, iso-benzylamide tri(meth)acrylate, 1,3,5-trihydroxy-s-triazine ring di(meth)acrylate, and 1,3,5-trihydroxy-s-triazine ring tri(meth)acrylate.
[0029] Furthermore, the thiol compound is a long-chain or multi-branched monomer containing one or more thiol structures, as shown in the following structure:
[0030]
[0031] Among them, R 10 , R 11 , R 12 The structures can be the same or different. Specifically, R 10 , R 11 , R 12 They can be independently selected from one or two or more of a hydrogen atom, or a long chain or multi-branched structure containing a thiol structure, or a (heterocyclic) aromatic or aliphatic derivative containing an active reaction functional group such as a hydroxyl group, a carboxyl group, an amino group, a sulfonic acid group, a mercapto group, or an aromatic or aliphatic derivative without a reactive group, or hydrogen, etc.
[0032] Further, the thiol compound is selected from one or two or more of dodecanethiol, mercapto-hexaethylene glycol-tert-butyl propionate, 1,6-hexanedithiol, 2,3-pentanedithiol, n-octyl mercaptan, 4-fluorobenzyl mercaptan, 3,4-hexanedithiol, 1.2-octanedithiol, 1,9-nonanedithiol, octadecanethiol, 1-hexadecanethiol, n-tetradecanethiol, phenylethanethiol, 3-(pyridin-2-yl)propane-1-thiol, 2-(pyrrolidin-1-yl)ethanethiol, 1,10-decanethiol, 2,4,6-trimercapto-s-triazine, and 2,2-bis(mercaptomethyl)-1,3-propanethiol.
[0033] Furthermore, the molar ratio of the monomer having a branched or long-chain carbon-carbon unsaturated bond to the thiol compound is 1:1-10, preferably 1:1-8, and more preferably 1:1-6.
[0034] Furthermore, the catalyst is an inorganic base or an organic base.
[0035] Furthermore, the inorganic base is selected from one or two or more of sodium carbonate, ammonium carbonate, sodium bicarbonate, sodium hydroxide, potassium carbonate, potassium bicarbonate, and potassium hydroxide.
[0036] Further, the organic base is selected from one or two or more of sodium methoxide, sodium ethoxide, sodium propoxide, sodium butoxide, sodium pentanol, 4-dimethylaminopyridine (DMAP), 1,8-diazabicyclo-bicyclo (5,4,0)-7-undecene (DBU), 1,5-diazabicyclo (4.3.0) non-5-ene (DBN), ethylenediamine, ethanolamine, n-propylamine, and 3-dimethylaminopropylamine.
[0037] Furthermore, the solvent is selected from one or two or more of methanol, ethanol, propanol, isopropanol, butanol, isobutanol, pentanol, isopentanol, ethylene glycol, polyethylene glycol, N,N-dimethylformamide (DMF), N,N-dimethylacetamide, N-methylpyrrolidone (NMP), N-ethylpyrrolidone, acetylacetone, acetone, dimethyl sulfoxide (DMSO), chloroform, dichloromethane, pyridine, benzene, toluene, dichloromethane, and chloroform.
[0038] Furthermore, the reaction temperature is 10°C to 140°C, preferably 40°C to 100°C, more preferably 50°C to 80°C, the reaction time is 1h to 48h, preferably 1.5h to 12h, more preferably 5h to 10h.
[0039] Furthermore, the preparation method of the branched sulfide dispersant specifically comprises the following steps:
[0040] (1) Adding a monomer having a branched or long-chain carbon-carbon unsaturated bond and a solvent into a container, placing the container on a heating device, and starting stirring;
[0041] (2) adding a catalyst to provide an alkaline environment to the system, then adding a thiol compound, and stirring for 20 to 40 minutes;
[0042] (3) heating, starting the timing after the system reaches the reaction temperature, and reacting for 1 h to 48 h under constant temperature conditions;
[0043] (4) The clear liquid obtained after the reaction is subjected to rotary evaporation, and the target product is taken out and rinsed with ethanol for 3 to 5 times to obtain a light yellow solid product, that is, the branched sulfide dispersant.
[0044] The second object of the present invention is to provide a branched sulfide dispersant prepared by the preparation method of the branched sulfide dispersant.
[0045] The third object of the present invention is to provide the use of the branched sulfide dispersant in the preparation of nano pigments.
[0046] The beneficial effect of the above technical solution of the present invention is that the branched sulfide dispersant of the present invention is added during the preparation process of nano-pigment, which can effectively improve the particle size of organic pigments such as CI254, CI291, CI255 and their dispersion performance in color paste and color photoresist.
[0047] Furthermore, the addition amount of the branched sulfide dispersant is 0.5% to 10% of the mass of the nano-pigment, preferably 1% to 8%, and more preferably 2% to 5%.
[0048] The nanopigment of the present invention is used to prepare a pigment composition.
[0049] The binder material in the pigment composition can be a polymer obtained by polymerizing (meth)acrylate monomers, specifically, polyethylene glycol (meth)acrylate, trimethyl propane di(meth)acrylate, polypropylene glycol (meth)acrylate, trimethyl propane tri(meth)acrylate, trimethylol propane tri(meth)acrylate, phenoxyethyl (meth)acrylate, pentadiene glycol ester, polyethylene glycol di(meth)acrylate, poly(ethylene glycol) diglycerol diacrylate, poly(propylene glycol) diglycerol diacrylate, any one or two or more thereof. The polymer formed by such unsaturated monomers can be used alone or mixed according to the formula.
[0050] The solvent in the pigment composition is firstly removed by rotary evaporation after the reaction is completed, and then a washing solvent can be selected to remove the raw materials that have not reacted completely. The principle is that the washing solvent is not the same as the reaction solvent and cannot dissolve the reaction product. The washing solvent can be selected from diethylene glycol dimethyl ether, methyl methoxypropyl ester, ethylene glycol dimethyl ether, propylene glycol dimethyl ether, propyl acrylate, methyl cellulose, ethyl cellulose, diethylene glycol methyl acetate, diethylene glycol ethyl acetate, methyl isobutyl ketone, cyclohexanone, N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), N-methyl-2-pyrrolidone (NMP), γ-butadiene, diphosphine (D igl The solvents include methyl cellulose, ethylene glycol monomethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, dipropylene glycol monomethyl ether, ethylene glycol monomethyl ether acetate, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, diethylene glycol dimethyl ether, cyclohexanone, 2-heptanone, 3-heptanone, ethyl 2-hydroxypropionate, 3-methyl-3-methoxybutyl propionate, ethyl 3-methoxypropionate, methyl 3-ethoxypropionate, ethyl 3-ethoxypropionate, n-butyl acetate, isobutyl acetate, n-amyl acetate, isoamyl acetate, n-butyl propionate, ethyl butyrate, isopropyl butyrate, n-butyl butyrate, ethyl pyruvic acid, γ-butyrolactone and other medium and high boiling point solvents. Such solvents can be used alone or in combination of two or more in different proportions.
[0051] The photoinitiator in the pigment composition can be selected from ketone series, triazine series, oxadiazole series, acylphosphine oxide series, organic peroxide, thio compound, aromatic onium salt, ketoxime ether photoreactant, specifically benzophenone, 1-hydroxy-1-phenylcyclohexane, benzyl acetone, 1-benzyl-1-dimethylamino-1-(4-pentadiene-phenyl ketone) propane, 2-pentadiene-2-(4-methyl methacrylate) phenyl propane, thioxanthone (thioxanthone) oxanthone), 1-chloro-4-propoxypropiophenone, isopropoxypropiophenone, diethoxypropiophenone, ethoxypropiophenone, 4-phenyl-4-methyldiphenylsulfonamide, phenyl butyl ether, 2-hydroxy-2-phenylpropane, 2-hydroxy-2-(4-isopropyl) ethyl benzoate, 4-butylbenzenetrichloromethane, 4-phenoxybenzenedichloromethane, ethyl benzoate, diphenyl (2,4,6-trimethylbenzoyl)-phosphonate, 4,4'-bis (diethylamino)- Benzophenone, 2-[2-(4-methoxy-phenyl)-ethylene]-4,6-bis-trichloromethyl-[1,3,5]triazine, 2-benzo[1,3]dioxol-5-yl-4,6-trichloromethyl[1,3,5]trichloromethane, 2-methyl-4,6-bis(trichloromethyl)-s-triazine, 2-benzene-4,6-bis(trichloromethyl)-s-triazine, 2-naphthalene-4,6-bis(trichloromethyl)-s-triazine, etc., are used alone or in combination of two or more.
[0052] In the pigment composition of the present invention, the (meth) acrylic resin binder is a multifunctional polymer that undergoes a bridging reaction in the presence of a photoinitiator, and the photoinitiator generally undergoes a free radical polymerization reaction under a wavelength of 310 to 420 nm ultraviolet light, and the amount of the acrylic resin binder is a multifunctional polymer that accounts for 60% to 60% of the total content of the photoresist composition, more preferably 80% to 50%, and more preferably 150% to 30%. The molecular weight of the acrylic resin binder is a multifunctional polymer that is generally selected from 3000 to 90000 g / mol, preferably in the range of 5000 to 60000, and more preferably in the range of 7000 to 40000, and the molecular weight is the weight average molecular weight measured by gel permeation chromatography (GPC, with tetrahydrofuran as solvent and polystyrene of different molecular weights as standard substances), and the ratio of the weight average molecular weight to the number average molecular weight is preferably 1 to 3, more preferably 1 to 2.5, and more preferably 1 to 2.
[0053] In addition, the pigment dispersant, crosslinking agent, adhesion improver, polymerization accelerator, photosensitizer, organic carboxylic acid or anhydride, thermal polymerization inhibitor, sensitizing dye, plasticizer, surfactant, storage stabilizer and texture improver used in the pigment composition are various suitable additives known in the art.
[0054] Preferably, the crosslinking agent is a (meth)acrylate with a functionality of three or more, and any one of trimethylolpropane tri(meth)acrylate, phenoxyethyl (meth)acrylate, pentadienol ester, polyethylene glycol di(meth)acrylate, ethylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, tri(acryloxyethyl)isocyanurate, glycerol 1,3-diglycerol diacrylate, diethanol diglycerol acrylate, poly(ethylene glycol) diglycerol diacrylate, 1,3-propylene glycol diglycerol diacrylate, and poly(propylene glycol) diglycerol diacrylate can be selected. The polymer formed by such unsaturated monomers can be used alone or mixed according to the formula.
[0055] The manufacturing processes for making color filters are well known and can be based on techniques such as photolithography, inkjet printing, lithography, gravure printing, relief printing, screen printing, stamping, continuous reverse printing and electrodeposition. The substrate can be transparent or reflective.
[0056] The present invention adopts a spin coating method to coat the plate and then perform photolithography, that is, the photoresist formulation (resist) is spin coated on the glass base at a rotation speed of 300 to 1000 rpm, dried on a hot plate at 100° C. to 120° C. for 1 min to 5 min, and then illuminated with LED or UV (365 nm, ±10 mJ / cm 2 , 10s~20s) exposure, and baked on a hot plate at 230℃ for 0.5h~2h, and the contrast of the obtained red filter segment was measured.
[0057] In order to determine the thermal stability, the samples were heat treated at 270 °C for 1 h and the contrast ratio was measured again. BRIEF DESCRIPTION OF THE DRAWINGS
[0058] Figure 1 is the infrared spectrum of the branched sulfide dispersant of Example 1;
[0059] Figure 2 is the infrared spectrum of dodecanethiol;
[0060] Figure 3 This is the pigment particle size diagram obtained in Example 1;
[0061] Figure 4 This is the pigment particle size diagram obtained in Comparative Example 1. DETAILED DESCRIPTION
[0062] The principles and features of the present invention are described below in conjunction with the accompanying drawings. The examples given are only used to explain the present invention and are not used to limit the scope of the present invention.
[0063] Example 1
[0064] Synthesis of Dipentaerythritol Hexaacrylate-Hexa-Dodecanedrine Sulfide
[0065]
[0066] Add 5.78g of dipentaerythritol pentaacrylate (Mr = 578.56g / mol, about 10mmol) and 50g of DMF as solvent to a three-necked flask, place it in a heating mantle, start stirring, add 0.033g of KOH (Mr = 56g / mol, about 0.59mmol) to provide an alkaline environment for the system and as a catalyst, add 12.14g of dodecanethiol (Mr = 202.4g / mol, about 60mmol), stir for 30min, start heating, start timing when the reaction system reaches 80℃, and react for 40h under the same temperature conditions. Transfer the clear liquid obtained after the reaction to a single-necked flask and start rotary evaporation. Take out the target product and rinse it with ethanol 3 to 5 times to obtain a light yellow solid product.
[0067] The above product was added to the synthesis of red pigment CI254, and the addition ratio was 2.5% of the red pigment CI254.
[0068] 10.6g of metallic sodium was added to 150g of tert-amyl alcohol, and 1.5g of branched sulfide dispersant was added. When the temperature was raised to 80°C and the metallic sodium was completely dissolved, 34.08g of p-chlorobenzonitrile and 25.3g of diisopropyl succinate were added and reacted at 100°C until no raw material spot was found on the TLC plate. The material was discharged and the pigment was post-treated to obtain a nano-organic pigment with controlled particle size.
[0069] The obtained nano pigments were used to obtain a red filter according to a general method for manufacturing a color filter, and its photophysical properties were measured.
[0070] The general method of manufacturing color filters is as follows:
[0071] 5 g of pigment was placed in a 50 ml plastic bottle to prepare a pigment composition, and then 0.5 g of Efka PX 4700 (acrylic dispersant) was added, and then 20 g of propylene glycol monomethyl ether acetate (PMA) was added, and 12 g of dipentaerythritol hexaacrylate was added as a binder. The mixture was mixed with 100 g of zirconium oxide beads (particle size of 0.3 mm) and ball-milled on a ball mill for 48 hours. After filtering the zirconium oxide beads, 1.5 g of poly(propylene glycol) diglycerol diacrylate and 0.5 g of 1-benzyl-1-dimethylamino-1-(4-pentadiene-phenyl ketone) propane were added, and mixed on an oscillator for 30 minutes. The obtained product was then subjected to performance testing.
[0072] Example 2
[0073] Synthesis of Dipentaerythritol Pentaacrylate Phenyl Ethyl Sulfide
[0074]
[0075] Add 4.94g of dipentaerythritol hexaacrylate (Mr = 494.18g / mol, about 10mmol) and 50g of NMP as solvent to a three-necked flask, place it in a heating mantle, start stirring, add 0.09g of DBU (Mr = 152.24g / mol, about 0.59mmol) to provide an alkaline environment for the system and as a catalyst, add 2.76g of phenylethyl mercaptan (Mr = 138.23g / mol, about 20mmol), stir for 30min, start heating, start timing when the reaction system reaches 120℃, and react for 2h under the same temperature conditions. Transfer the clear liquid obtained after the reaction to a single-necked flask and start rotary evaporation. Take out the target product and rinse it with ethanol 3 to 5 times to obtain a light yellow solid product.
[0076] It was added into the synthesis of red pigment CI254, and the adding ratio was 0.5% of the red pigment CI254. The preparation process was the same as in Example 1 and will not be described in detail.
[0077] The obtained nano pigments were used to obtain a red filter according to a general method for manufacturing a color filter, and its photophysical properties were measured.
[0078] Example 3
[0079] Synthesis of Hyperbranched Homobenzyltrimethylacrylate Pentylene Disulfide
[0080]
[0081] Add 3.72g of benzyl trimethyl acrylate (Mr = 372.16g / mol, about 10mmol) to a three-necked flask, add 50g of toluene as a solvent, place it in a heating mantle, start stirring, add 0.09g of DBU (Mr = 152.24g / mol, about 0.59mmol) to provide an alkaline environment for the system and as a catalyst, add 2.72g of pentanedithiol (Mr = 136.04g / mol, about 20mmol), stir for 30min, start heating, start timing when the reaction system reaches 50℃, react for 4h under the same temperature conditions, continue to increase the temperature to 140℃, and continue to react for 4h. Transfer the clear liquid obtained after the reaction to a single-necked flask and start rotary evaporation. Take out the target and rinse it with ethanol 3 to 5 times to obtain a yellow solid product.
[0082] It was added into the synthesis of red pigment CI254, and the adding ratio was 10% of the red pigment CI254. The preparation process was the same as in Example 1 and will not be described in detail.
[0083] The obtained nano pigments were used to obtain a red filter according to a general method for manufacturing a color filter, and its photophysical properties were measured.
[0084] Example 4
[0085] Synthesis of 1,3-Diglycerol Alcohol Diacrylate Glycerol 2-Triazine Trisulfide
[0086]
[0087] Add 6.96g of 1,3-diglycerol alcohol diacrylate (Mr = 348.35g / mol, about 20mmol) to a three-necked flask, add 50g of DMSO as a solvent, place it in a heating mantle, start stirring, add 0.03g of sodium methoxide (Mr = 54.02g / mol, about 0.59mmol) to provide an alkaline environment for the system and as a catalyst, add 5.22g of 2,4,6-trimercapto-s-triazine (Mr = 261.04g / mol, about 20mmol), stir for 30min, start heating, and start timing when the reaction system reaches 80℃. React for 2h under the same temperature conditions, continue to heat to 100℃, react at this temperature for 10h, transfer the clear liquid obtained after the reaction to a single-necked flask and start rotary evaporation. Take out the target and rinse it with ethanol 3 to 5 times to obtain a yellow solid product.
[0088] It was added into the synthesis of red pigment CI254, and the addition ratio was 6% of the red pigment CI254. The preparation process was the same as in Example 1 and will not be described in detail.
[0089] The obtained nano pigments were used to obtain a red filter according to a general method for manufacturing a color filter, and its photophysical properties were measured.
[0090] Comparative Example 1:
[0091] 5 g of pigment CI254 (the branched sulfide dispersant of the present invention is not added during the synthesis process) is placed in a 50 ml plastic bottle to prepare a pigment composition, and then 0.5 g of Efka PX 4700 (acrylic dispersant) is added, and then 20 g of propylene glycol monomethyl ether acetate (PMA) is added, and 12 g of dipentaerythritol hexaacrylate is added as a binder. The mixture is mixed with 100 g of zirconium oxide beads (particle size is 0.3 mm), and then ball-milled on a ball mill for 48 hours. After filtering the zirconium oxide beads, 1.5 g of poly(propylene glycol) diglycerol diacrylate and 0.5 g of 1-benzyl-1-dimethylamino-1-(4-pentadiene-phenyl ketone) propane are added, and mixed on an oscillator for 30 minutes. The obtained product is then subjected to performance testing.
[0092] Table 1 Photophysical properties test
[0093] name x y Y Contrast Comparative Example 1 0.6500 0.2915 12.91 3100 Example 1 0.6500 0.2933 13.97 7800 Example 2 0.6500 0.2941 13.88 8100 Example 3 0.6500 0.2928 13.76 7900 Example 4 0.6500 0.2965 13.57 8300
[0094] From the optical physical performance test table 1, it can be seen that, under the premise of ensuring a relatively accurate cursor table (x, y) of the filter, the brightness of embodiments 1 to 4 is increased by more than 5% and the contrast is more than doubled compared with comparative example 1, thus meeting the performance index requirements of modern LCD panel technology for high transmittance and high contrast of the filter.
[0095] from Figure 3 and Figure 4 It can be seen from the particle size diagrams of the embodiments and comparative examples (wherein the curve with a peak is the particle size distribution curve and the other is the cumulative integral curve of the particle size) that after adding the branched sulfide dispersant of the present invention during the preparation of the nanopigment, a CI254 pigment with uniform particle size and significantly improved particle size can be obtained.
[0096] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a branched sulfide dispersant, characterized in that: A monomer having a branched or long-chain carbon-carbon unsaturated bond is added to a solvent, and a catalyst and a thiol compound are added under heating conditions. Under the catalytic action of the catalyst, the monomer having a branched or long-chain carbon-carbon unsaturated bond and the thiol compound undergo a click chemical reaction to obtain the branched sulfide dispersant.
2. The method for preparing a branched sulfide dispersant according to claim 1, characterized in that: The monomer having branched or long-chain carbon-carbon unsaturated bonds is selected from aliphatic compounds and their derivatives or (heterocyclic) aromatic compounds and their derivatives.
3. The method for preparing a branched sulfide dispersant according to claim 2, characterized in that: The aliphatic compound and its derivatives are selected from the following general formula I: Where n is an integer ≥ 1, R1, R2, and R3 are independently selected from hydrogen atoms, methyl groups, C2-C20 alkyl groups and their derivatives, or aromatic rings and their derivatives, or propylene oxide groups, or heterocyclic structure derivatives containing O, N or S elements, or alicyclic groups and their derivatives, R4 is methyl or hydrogen, X is one of O, N or S elements.
4. The method for preparing a branched sulfide dispersant according to claim 2, characterized in that: The (heterocyclic) aromatic compound and its derivatives are selected from the following general formula II: Wherein, m is an integer ≥ 1, R4 is methyl or hydrogen, R5, R6, R7, R8, and R9 are independently selected from hydrogen atoms, methyl groups, C2-C20 alkyl groups and their derivatives, or aromatic rings and their derivatives, or propylene oxide groups, or heterocyclic structure derivatives containing O, N or S elements, or alicyclic groups and their derivatives. X is one of O, N or S elements, Y is C, or one or two of O, N or S elements.
5. The method for preparing a branched sulfide dispersant according to claim 1, characterized in that: The thiol compound is selected from one or more of dodecanethiol, mercapto-hexaethylene glycol-tert-butyl propionate, 1,6-hexanedithiol, 2,3-pentanedithiol, n-octyl mercaptan, 4-fluorobenzyl mercaptan, 3,4-hexanedithiol, 1.2-octanedithiol, 1,9-nonanedithiol, octadecanethiol, 1-hexadecanethiol, n-tetradecanethiol, phenylethanethiol, 3-(pyridin-2-yl)propane-1-thiol, 2-(pyrrolidin-1-yl)ethanethiol, 1,10-decanethiol, 2,4,6-trimercapto-s-triazine, and 2,2-bis(mercaptomethyl)-1,3-propanethiol.
6. The method for preparing a branched sulfide dispersant according to any one of claims 1 to 5, characterized in that: The molar ratio of the monomer having a branched or long-chain carbon-carbon unsaturated bond to the thiol compound is 1:1-10.
7. The method for preparing a branched sulfide dispersant according to claim 6, characterized in that: The catalyst is an inorganic base or an organic base.
8. The method for preparing a branched sulfide dispersant according to claim 1, characterized in that: The reaction temperature is between 10°C and 140°C, and the reaction time is between 1h and 48h.
9. A branched sulfide dispersant, characterized in that: The method for preparing the branched sulfide dispersant is adopted as claimed in any one of claims 1 to 8.