Catalytic hydrogenation method of dicyclopentadiene resin

By screening high-efficiency catalysts and optimizing process conditions, the catalytic hydrogenation efficiency of dicyclopentadiene resin is improved, the problem of low catalytic hydrogenation efficiency in the existing technology is solved, and the efficient modification of the resin and the application of various industrial applications is realized. sex.

CN118878722APending Publication Date: 2024-11-01NANJING YUANGANG FINE CHEMICALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411106210.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

In the prior art, the catalytic hydrogenation efficiency of dicyclopentadiene resin is low, resulting in high unsaturation, deep hue and poor adhesion of the resin, making it difficult to be widely used in various applications.

Method used

By screening catalysts with high activity and good stability, combined with suitable process conditions such as catalyst content, stirring speed, temperature and time, preheating and high-pressure hydrogenation reaction processes are used to prepare dicyclopentadiene modified resin to improve hydrogenation conversion and the softening point of the resin.

Benefits of technology

It realizes efficient modification of resin, reduces unsaturation and color, and improves adhesion. It is suitable for a variety of industrial applications, especially hot melt road marking paint, shoe adhesives and food packaging supplies.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004990889790000091
    Figure BDA0004990889790000091
Patent Text Reader

Abstract

The invention discloses a catalytic hydrogenation method of dicyclopentadiene resin, which relates to the technical field of styrene modified resin, and comprises the following steps: raw material pretreatment: mixing a material composed of a dicyclopentadiene raw material and an organic solvent, and then continuously preheating through a preheating reactor, a polymerization reactor and a heat preservation reactor in sequence; and performing high-pressure hydrogenation on the resin: adding styrene, dicyclopentadiene, a catalyst and a solvent into a reaction kettle, mixing, vacuumizing, performing nitrogen displacement, performing thermal polymerization reaction, preparing dicyclopentadiene modified resin liquid, and then cooling. According to the method, the intermittent hydrogenation catalyst with high activity and good stability is screened out by comparing the performance of the resin hydrogenation catalyst, the hydrogenation conversion rate and the softening point of the resin are taken as main inspection indexes, and relatively proper hydrogenation process conditions are determined through solvent screening, process condition inspection and orthogonal optimization test; the hydrogenation conversion rate of the resin under the condition is maintained to be 93% or above.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of styrene modified resins, and in particular to a catalytic hydrogenation method for dicyclopentadiene resin. Background Art

[0002] Dicyclopentadiene petroleum resin is made by thermal polymerization of dicyclopentadiene with high purity, which is a by-product of petroleum cracking to produce ethylene. It is a thermoplastic hydrocarbon resin with relatively low number average molecular weight. This type of resin has defects such as dark hue, high content of unsaturated hydrocarbon bonds, low thermal stability and oxidation stability, and poor adhesion. It is not well compatible with many resin matrices and has poor effect as a tackifier. It is not often used directly and needs to be modified to prepare high-grade petroleum resin.

[0003] The simplest modification is resin hydrogenation. After hydrogenation, the unsaturation of petroleum resin is greatly reduced, the hue is light, and there is no special smell. In addition to being used in adhesives, hot melt adhesives, pressure-sensitive tapes, ink printing and rubber, it is particularly suitable for the manufacture of hot melt road marking paints that require pure color and good thermal stability, light-colored shoe adhesives and food packaging products, disposable paper diapers and sanitary napkins, etc. Special adhesives used in the manufacture of women's sanitary napkins.

[0004] The hydrogenation processes used for petroleum resin can be roughly summarized as: slurry hydrogenation, spray hydrogenation, and fixed bed hydrogenation. Slurry hydrogenation is generally intermittent, which is more suitable for smaller production scales or initial laboratory evaluations, but the operation is cumbersome and the catalyst loss is large; while fixed bed hydrogenation is suitable for large-scale continuous production, and currently the international market prefers the medium-pressure one-stage hydrogenation process.

[0005] Conventional technology does not add a catalyst to carry out conventional reactions, and the efficiency of catalytic hydrogenation is relatively low. Therefore, we propose a catalytic hydrogenation method for dicyclopentadiene resin. Summary of the invention

[0006] 1. Technical issues to be resolved

[0007] In view of the deficiencies in the prior art, the present invention provides a catalytic hydrogenation method for dicyclopentadiene resin, which solves the technical problem of low catalytic hydrogenation efficiency.

[0008] (II) Technical solution

[0009] To achieve the above objectives, the present invention is implemented through the following technical solutions:

[0010] A catalytic hydrogenation method for dicyclopentadiene resin, the steps are as follows:

[0011] Step 1, raw material pretreatment: mixing the material consisting of dicyclopentadiene raw material and organic solvent and then continuously passing through a preheating reactor, a polymerization reactor and a heat preservation reactor in sequence for preheating;

[0012] Step 2, high-pressure hydrogenation of the resin: Styrene, dicyclopentadiene, a catalyst and a solvent are added to a reaction kettle and mixed, and a vacuum is drawn and nitrogen is replaced to carry out a thermal polymerization reaction to prepare a dicyclopentadiene modified resin liquid, and then the temperature is reduced and cooled.

[0013] The preheating reactor is a shell-and-tube reactor with a static mixing element. In the shell-and-tube reactor, the tube-side medium is material, the shell-side medium is heat transfer oil for heat exchange and temperature control, the insulation reactor is a kettle reactor, the mass ratio of DCPD to solvent is 1:1-4, the preheating reaction temperature is 160-230°C, the preheating reaction pressure is 1.0-5.0MPa, and the preheating reaction residence time is 30-50min.

[0014] In the resin high pressure hydrogenation in step 2, styrene is 5-12%, dicyclopentadiene is 25-35%, catalyst is 2-5% and the rest is solvent.

[0015] The reactor is provided with a stirring paddle, which is turned on for heating, and a thermal polymerization reaction is carried out at 240-270° C. for 3-6 hours, and then the temperature is lowered to 120-150° C.

[0016] The styrene is analytical grade, wherein the mass concentration of styrene is above 99%, and the dicyclopentadiene is industrial grade dicyclopentadiene, wherein the mass concentration is 80-95%.

[0017] The solvent is one or a mixture of cyclohexane, n-hexane, n-heptane, methylcyclohexane and ethylcyclohexane.

[0018] The catalyst is Ni5388. By making Ni5388 into powder, the contact area is increased, the reaction efficiency is improved, and the resin obtained after removing the solvent from Ni5388 has a better softening point and color.

[0019] (III) Beneficial effects

[0020] 1. As can be seen from the above table, when the catalyst content is less than 2.0%, the hydrogenation conversion rate of the resin gradually increases with the increase of the added amount. At about 4.0%, the yield reaches the maximum. If the catalyst content continues to increase, the hydrogenation conversion rate of the resin does not change significantly, and the softening point also decreases slightly. This is because the initial catalyst content is too little, and the catalyst is not in sufficient contact with the material. The reaction rate increases with the increase in the amount of catalyst, and the hydrogenation conversion rate of the resin increases accordingly; but when the catalyst content reaches a certain level, the dynamic viscosity of the system increases, the mass transfer condition deteriorates, and the resin degradation reaction increases slightly. Therefore, the catalyst content should be about 4.0%.

[0021] 2. Under the conditions of catalyst content of about 3.0%, reaction pressure of 5.0MPa, reaction temperature of 250-260℃, the amount of solvent added and resin equal (mass ratio of 1:1), and reaction time of 4h, the effect of stirring speed on the reaction was investigated. Since the resin hydrogenation reaction is an exothermic reaction, the faster the stirring speed, the more conducive it is to mass transfer and diffusion, and the more beneficial it is to increasing the reaction rate.

[0022] As can be seen from the table above, if the stirring speed is too low, the hydrogenation rate is slow and the reaction is uneven, local overheating will cause the resin color to darken. When the stirring speed is greater than 300r / min, the resin hydrogenation conversion rate has no obvious change. At the same time, the reaction intensifies, causing the side reaction of hydrogenation degradation to increase, and the resin softening point decreases more. Therefore, the following tests were carried out at a stirring speed of about 300r / min.

[0023] 3. As can be seen from the table above, temperature has a great influence on the hydrogenation rate. When the temperature is low, the reaction speed is slow, the hydrogenation is insufficient, and the resin color is dark. However, when the temperature is greater than 260°C, the hydrogenation conversion rate of the resin changes little, while the side reaction of hydrogenation degradation increases, and the decrease in the resin softening point increases. Carrying out the hydrogenation reaction at a relatively low temperature will help delay coking and maintain the activity and stability of the catalyst. Therefore, the reaction temperature is best controlled at 260°C.

[0024] 4. Under the conditions of catalyst content of about 3.0%, reaction pressure of 5.0 MPa, stirring speed of 300 r / min, reaction temperature of 250-260°C, and equal amount of solvent added to resin (mass ratio of 1:1), the effect of time on the reaction was investigated.

[0025] It can be seen from the above table that in the initial stage of the reaction, the hydrogenation conversion rate gradually increases with the extension of time. When the reaction time exceeds 5h, the hydrogenation conversion rate no longer increases, and it can be considered that the hydrogenation is basically completed. At the same time, the degradation side reaction continues and the softening point is slightly reduced. Therefore, a reaction time of about 5h is more appropriate.

[0026] In summary: by comparing the performance of resin hydrogenation catalysts, intermittent hydrogenation catalysts with high activity and good stability were screened out, and the hydrogenation conversion rate and the softening point of the resin were taken as the main investigation indicators. Through the screening of solvents, the investigation of process conditions and orthogonal optimization experiments, the more suitable hydrogenation process conditions were determined: toluene (with a mass ratio of 1:1 to the hydrogenation raw material) as the solvent, a catalyst addition amount of about 4.0%, a stirring rate of 300r / min, a reaction temperature of 260°C, and a reaction time of 5h. Under these conditions, the hydrogenation conversion rate of the resin was maintained above 93%. DETAILED DESCRIPTION

[0027] The embodiment of the present application solves the problem of low catalytic efficiency in the prior art by providing a catalytic hydrogenation method for dicyclopentadiene resin. By comparing the performance of resin hydrogenation catalysts, an intermittent hydrogenation catalyst with high activity and good stability is screened out. The hydrogenation conversion rate and the softening point of the resin are taken as the main investigation indicators. By screening the solvent, investigating the process conditions and conducting orthogonal optimization experiments, more suitable hydrogenation process conditions are determined.

[0028] Example 1

[0029] The technical solution in the embodiment of the present application is to solve the above-mentioned problem of low catalytic efficiency, and the overall idea is as follows:

[0030] In view of the problems existing in the prior art, the present invention provides a catalytic hydrogenation method for dicyclopentadiene resin, the steps of which are as follows:

[0031] Step 1, raw material pretreatment: mixing the material consisting of dicyclopentadiene raw material and organic solvent and then continuously passing through a preheating reactor, a polymerization reactor and a heat preservation reactor in sequence for preheating;

[0032] The preheating reactor is a shell-and-tube reactor with a static mixing element. In the shell-and-tube reactor, the tube-side medium is material, the shell-side medium is heat transfer oil for heat exchange and temperature control, the insulation reactor is a kettle reactor, the mass ratio of DCPD to solvent is 1:1, and the preheating reaction temperature is 160°C.

[0033] Step 2, high-pressure hydrogenation of the resin: styrene, dicyclopentadiene, a catalyst and a solvent are added to a reaction kettle and mixed, and then vacuumed and nitrogen replaced to perform a thermal polymerization reaction to prepare a dicyclopentadiene modified resin liquid, and then cooled;

[0034] In the resin high pressure hydrogenation in step 2, styrene is 5%, dicyclopentadiene is 25%, catalyst is 2% and the rest is solvent.

[0035] The reactor is provided with a stirring paddle, which is turned on to heat the reactor, and a thermal polymerization reaction is carried out at 240° C. The reaction time is 3 hours, and then the temperature is lowered to 120° C.;

[0036] The styrene is analytically pure, wherein the mass concentration of styrene is above 99%;

[0037] The dicyclopentadiene is industrial grade dicyclopentadiene with a mass concentration of 80%;

[0038] The solvent is one or a mixture of cyclohexane, n-hexane, n-heptane, methylcyclohexane and ethylcyclohexane.

[0039] The catalyst is Ni5388. By making Ni5388 into powder, the contact area is increased, the reaction efficiency is improved, and the resin obtained after removing the solvent from Ni5388 has a better softening point and color.

[0040] Example 2

[0041] The technical solution in the embodiment of the present application is to solve the above-mentioned problem of low catalytic efficiency, and the overall idea is as follows:

[0042] In view of the problems existing in the prior art, the present invention provides a catalytic hydrogenation method for dicyclopentadiene resin, the steps of which are as follows:

[0043] Step 1, raw material pretreatment: mixing the material consisting of dicyclopentadiene raw material and organic solvent and then continuously passing through a preheating reactor, a polymerization reactor and a heat preservation reactor in sequence for preheating;

[0044] The preheating reactor is a shell-and-tube reactor with a static mixing element. In the shell-and-tube reactor, the tube-side medium is material, the shell-side medium is heat transfer oil for heat exchange and temperature control, the insulation reactor is a kettle reactor, the mass ratio of DCPD to solvent is 1:2, and the preheating reaction temperature is 170°C.

[0045] Step 2, high-pressure hydrogenation of the resin: styrene, dicyclopentadiene, a catalyst and a solvent are added to a reaction kettle and mixed, and then vacuumed and nitrogen replaced to perform a thermal polymerization reaction to prepare a dicyclopentadiene modified resin liquid, and then cooled;

[0046] In the resin high pressure hydrogenation in step 2, styrene is 7%, dicyclopentadiene is 27%, catalyst is 3% and the rest is solvent.

[0047] The reactor is provided with a stirring paddle, the stirring paddle is turned on for heating, a thermal polymerization reaction is carried out at 250° C., the reaction time is 4 hours, and then the temperature is lowered to 130° C.;

[0048] The styrene is analytically pure, wherein the mass concentration of styrene is above 99%;

[0049] The dicyclopentadiene is industrial grade dicyclopentadiene with a mass concentration of 83%;

[0050] The solvent is one or a mixture of cyclohexane, n-hexane, n-heptane, methylcyclohexane and ethylcyclohexane.

[0051] The catalyst is Ni5388. By making Ni5388 into powder, the contact area is increased, the reaction efficiency is improved, and the resin obtained after removing the solvent from Ni5388 has a better softening point and color.

[0052] Example 3

[0053] The technical solution in the embodiment of the present application is to solve the above-mentioned problem of low catalytic efficiency, and the overall idea is as follows:

[0054] In view of the problems existing in the prior art, the present invention provides a catalytic hydrogenation method for dicyclopentadiene resin, the steps of which are as follows:

[0055] Step 1, raw material pretreatment: mixing the material consisting of dicyclopentadiene raw material and organic solvent and then continuously passing through a preheating reactor, a polymerization reactor and a heat preservation reactor in sequence for preheating;

[0056] The preheating reactor is a shell-and-tube reactor with a static mixing element. In the shell-and-tube reactor, the tube-side medium is material, the shell-side medium is heat transfer oil for heat exchange and temperature control, the insulation reactor is a kettle reactor, the mass ratio of DCPD to solvent is 1:3, and the preheating reaction temperature is 210°C.

[0057] Step 2, high-pressure hydrogenation of the resin: styrene, dicyclopentadiene, a catalyst and a solvent are added to a reaction kettle and mixed, and then vacuumed and nitrogen replaced to perform a thermal polymerization reaction to prepare a dicyclopentadiene modified resin liquid, and then cooled;

[0058] In the resin high pressure hydrogenation in step 2, styrene is 10%, dicyclopentadiene is 32%, catalyst is 2-5% and the rest is solvent.

[0059] The reactor is provided with a stirring paddle, the stirring paddle is turned on for heating, a thermal polymerization reaction is carried out at 260° C., the reaction time is 5 hours, and then the temperature is lowered to 140° C.;

[0060] The styrene is analytically pure, wherein the mass concentration of styrene is above 99%;

[0061] The dicyclopentadiene is industrial grade dicyclopentadiene with a mass concentration of 92%;

[0062] The solvent is one or a mixture of cyclohexane, n-hexane, n-heptane, methylcyclohexane and ethylcyclohexane.

[0063] The catalyst is Ni5388. By making Ni5388 into powder, the contact area is increased, the reaction efficiency is improved, and the resin obtained after removing the solvent from Ni5388 has a better softening point and color.

[0064] Example 4

[0065] The technical solution in the embodiment of the present application is to solve the above-mentioned problem of low catalytic efficiency, and the overall idea is as follows:

[0066] In view of the problems existing in the prior art, the present invention provides a catalytic hydrogenation method for dicyclopentadiene resin, the steps of which are as follows:

[0067] Step 1, raw material pretreatment: mixing the material consisting of dicyclopentadiene raw material and organic solvent and then continuously passing through a preheating reactor, a polymerization reactor and a heat preservation reactor in sequence for preheating;

[0068] The preheating reactor is a shell-and-tube reactor with a static mixing element. In the shell-and-tube reactor, the tube-side medium is material, the shell-side medium is heat transfer oil for heat exchange and temperature control, the insulation reactor is a kettle reactor, the mass ratio of DCPD to solvent is 1:1-4, and the preheating reaction temperature is 160-230°C.

[0069] Step 2, high-pressure hydrogenation of the resin: styrene, dicyclopentadiene, a catalyst and a solvent are added to a reaction kettle and mixed, and then vacuumed and nitrogen replaced to perform a thermal polymerization reaction to prepare a dicyclopentadiene modified resin liquid, and then cooled;

[0070] In the resin high pressure hydrogenation in step 2, styrene is 5-12%, dicyclopentadiene is 25-35%, catalyst is 2-5% and the rest is solvent.

[0071] The reactor is provided with a stirring paddle, which is turned on for heating, and a thermal polymerization reaction is carried out at 240-270° C. for 3-6 hours, and then the temperature is lowered to 120-150° C.;

[0072] The styrene is analytically pure, wherein the mass concentration of styrene is above 99%;

[0073] The dicyclopentadiene is industrial grade dicyclopentadiene with a mass concentration of 80-95%;

[0074] The solvent is one or a mixture of cyclohexane, n-hexane, n-heptane, methylcyclohexane and ethylcyclohexane.

[0075] The catalyst is Ni5388. By making Ni5388 into powder, the contact area is increased, the reaction efficiency is improved, and the resin obtained after removing the solvent from Ni5388 has a better softening point and color.

[0076] Through the above experimental data, the increase in the amount of catalyst added is beneficial to accelerate the reaction rate, but when the amount added is too large, a considerable part of the catalyst will not be suspended in the reaction liquid in an ideal state, resulting in a decrease in the effective utilization rate of the catalyst. Moreover, when the amount is too large, the dynamic viscosity of the system will increase, which is not conducive to mass transfer.

[0077] Therefore, under the premise of ensuring smooth mass transfer, the amount of catalyst has an optimal value. The test catalyst amount is 2-5%, the stirring speed is 100-400r / min, the reaction temperature is 240-270℃, the amount of solvent added is equal to the resin (mass ratio is 1:1), and the reaction time is 3-6h. The effects of catalyst addition, stirring speed, reaction temperature and reaction time on the hydrogenation conversion amount of the resin are investigated. The experimental data are as follows:

[0078]

[0079] 1. As can be seen from the above table, when the catalyst content is less than 2.0%, the hydrogenation conversion rate of the resin gradually increases with the increase of the added amount. At about 4.0%, the yield reaches the maximum. If the catalyst content continues to increase, the hydrogenation conversion rate of the resin does not change significantly, and the softening point also decreases slightly. This is because the initial catalyst content is too little, and the catalyst is not in sufficient contact with the material. The reaction rate increases with the increase in the amount of catalyst, and the hydrogenation conversion rate of the resin increases accordingly; but when the catalyst content reaches a certain level, the dynamic viscosity of the system increases, the mass transfer condition deteriorates, and the resin degradation reaction increases slightly. Therefore, the catalyst content should be about 4.0%.

[0080] 2. Under the conditions of catalyst content of about 3.0%, reaction pressure of 5.0MPa, reaction temperature of 250-260℃, the amount of solvent added and resin equal (mass ratio of 1:1), and reaction time of 4h, the effect of stirring speed on the reaction was investigated. Since the resin hydrogenation reaction is an exothermic reaction, the faster the stirring speed, the more conducive it is to mass transfer and diffusion, and the more beneficial it is to increasing the reaction rate.

[0081] As can be seen from the table above, if the stirring speed is too low, the hydrogenation rate is slow and the reaction is uneven, local overheating will cause the resin color to darken. When the stirring speed is greater than 300r / min, the resin hydrogenation conversion rate has no obvious change. At the same time, the reaction intensifies, causing the side reaction of hydrogenation degradation to increase, and the resin softening point decreases more. Therefore, the following tests were carried out at a stirring speed of about 300r / min.

[0082] 3. As can be seen from the table above, temperature has a great influence on the hydrogenation rate. When the temperature is low, the reaction speed is slow, the hydrogenation is insufficient, and the resin color is dark. However, when the temperature is greater than 260°C, the hydrogenation conversion rate of the resin changes little, while the side reaction of hydrogenation degradation increases, and the decrease in the resin softening point increases. Carrying out the hydrogenation reaction at a relatively low temperature will help delay coking and maintain the activity and stability of the catalyst. Therefore, the reaction temperature is best controlled at 260°C.

[0083] 4. Under the conditions of catalyst content of about 3.0%, reaction pressure of 5.0 MPa, stirring speed of 300 r / min, reaction temperature of 250-260°C, and equal amount of solvent added to resin (mass ratio of 1:1), the effect of time on the reaction was investigated.

[0084] It can be seen from the above table that in the initial stage of the reaction, the hydrogenation conversion rate gradually increases with the extension of time. When the reaction time exceeds 5h, the hydrogenation conversion rate no longer increases, and it can be considered that the hydrogenation is basically completed. At the same time, the degradation side reaction continues and the softening point is slightly reduced. Therefore, a reaction time of about 5h is more appropriate.

[0085] In summary: by comparing the performance of resin hydrogenation catalysts, intermittent hydrogenation catalysts with high activity and good stability were screened out, and the hydrogenation conversion rate and the softening point of the resin were taken as the main investigation indicators. Through the screening of solvents, the investigation of process conditions and orthogonal optimization experiments, the more suitable hydrogenation process conditions were determined: toluene (with a mass ratio of 1:1 to the hydrogenation raw material) as the solvent, a catalyst addition amount of about 4.0%, a stirring rate of 300r / min, a reaction temperature of 260°C, and a reaction time of 5h. Under these conditions, the hydrogenation conversion rate of the resin was maintained above 93%.

[0086] Finally, it should be noted that: Obviously, the above embodiments are only examples for clearly explaining the present invention, and are not intended to limit the implementation methods. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from this are still within the scope of protection of the present invention.

Claims

1. A catalytic hydrogenation method for dicyclopentadiene resin, characterized in that: Here are the steps: Step 1, raw material pretreatment: mixing the material consisting of dicyclopentadiene raw material and organic solvent and then continuously passing through a preheating reactor, a polymerization reactor and a heat preservation reactor in sequence for preheating; Step 2, high-pressure hydrogenation of the resin: Styrene, dicyclopentadiene, a catalyst and a solvent are added to a reaction kettle and mixed, and a vacuum is drawn and nitrogen is replaced to carry out a thermal polymerization reaction to prepare a dicyclopentadiene modified resin liquid, and then the temperature is reduced and cooled.

2. A catalytic hydrogenation method for dicyclopentadiene resin as claimed in claim 1, characterized in that: The preheating reactor is a shell-and-tube reactor with a static mixing element. In the shell-and-tube reactor, the tube-side medium is material, the shell-side medium is heat transfer oil for heat exchange and temperature control, the insulation reactor is a kettle reactor, the mass ratio of DCPD to solvent is 1:1-4, the preheating reaction temperature is 160-230°C, the preheating reaction pressure is 1.0-5.0MPa, and the preheating reaction residence time is 30-50min.

3. A catalytic hydrogenation method for dicyclopentadiene resin as claimed in claim 2, characterized in that: The preheating reactor is a shell-and-tube reactor with a static mixing element. In the shell-and-tube reactor, the tube-side medium is material, the shell-side medium is heat transfer oil for heat exchange and temperature control, the insulation reactor is a kettle reactor, the mass ratio of DCPD to solvent is 1:1, the preheating reaction temperature is 160°C, the preheating reaction pressure is 1.0 MPa, and the preheating reaction residence time is 30 min.

4. A catalytic hydrogenation method for dicyclopentadiene resin as claimed in claim 2, characterized in that: The preheating reactor is a shell-and-tube reactor with a static mixing element. In the shell-and-tube reactor, the tube-side medium is material, the shell-side medium is heat transfer oil for heat exchange and temperature control, the insulation reactor is a kettle reactor, the mass ratio of DCPD to solvent is 1:4, the preheating reaction temperature is 230°C, the preheating reaction pressure is 5.0MPa, and the preheating reaction residence time is 50min.

5. A catalytic hydrogenation method for dicyclopentadiene resin as claimed in claim 1, characterized in that: In the resin high pressure hydrogenation in step 2, styrene is 5-12%, dicyclopentadiene is 25-35%, catalyst is 2-5% and the rest is solvent.

6. A catalytic hydrogenation method for dicyclopentadiene resin as claimed in claim 5, characterized in that: The reactor is provided with a stirring paddle, which is turned on for heating, and a thermal polymerization reaction is carried out at 240-270° C. for 3-6 hours, and then the temperature is lowered to 120-150° C.

7. A catalytic hydrogenation method for dicyclopentadiene resin as claimed in claim 6, characterized in that: The styrene is analytical grade, wherein the mass concentration of styrene is above 99%, and the dicyclopentadiene is industrial grade dicyclopentadiene, wherein the mass concentration is 80-95%.

8. A catalytic hydrogenation method for dicyclopentadiene resin as claimed in claim 7, characterized in that: The solvent is one or a mixture of cyclohexane, n-hexane, n-heptane, methylcyclohexane and ethylcyclohexane.

9. A catalytic hydrogenation method for dicyclopentadiene resin as claimed in claim 8, characterized in that: The catalyst is Ni5388. By making Ni5388 into powder, the contact area is increased, and the resin obtained after removing the solvent from Ni5388 has a better softening point and color.