Acrylate-vinylidene chloride copolymer emulsion based on reversible addition fragmentation transfer reagent induction as well as preparation method and application thereof

Through the method of induction of reversible addition breakage transfer reagent, acrylate-vinylidene chloride copolymer emulsion with good compatibility and high stability was prepared, which solved the problem of breaking the emulsion when adding alcohol ether additives. The problem of high stability and suitable applications in the packaging field.

CN118878728APending Publication Date: 2024-11-01QINGHAI UNIV FOR NATITIES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410849796.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Acrylate-VDC copolymer emulsion is prone to demulsification when alcohol ether additives are added, resulting in the inability to obtain stable color paint. The reduction in the amount of small molecule emulsifier will deteriorate storage stability, affecting its application.

Method used

By using the method of induction of reversible addition break transfer reagent, acrylate-vinylidene chloride copolymer emulsion with good compatibility and high stability is prepared by producing large-molecular emulsifiers in situ and replacing small-molecular emulsifiers. Semi-continuous Emulsion polymerization is carried out by seed emulsion polymerization.

Benefits of technology

It has achieved a copolymer emulsion that maintains high stability and compatibility under the condition of small molecule emulsifier content, which is suitable for applications as high barrier film packaging materials, providing theoretical support.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118878728A_ABST
    Figure CN118878728A_ABST
Patent Text Reader

Abstract

The invention discloses an acrylate-vinylidene chloride copolymer emulsion based on reversible addition fragmentation transfer reagent induction as well as a preparation method and application thereof, and relates to the technical field of polyvinylidene chloride. The VDC-Acrylate copolymer emulsion is prepared by adopting a semi-continuous seed emulsion polymerization method, and the preparation method comprises the following steps: inducing to prepare an acrylate-vinylidene chloride copolymer by introducing a reversible addition fragmentation transfer reagent, and generating a macromolecular emulsifier in situ; the finally prepared copolymer has the characteristics of good compatibility and high stability while the content of the micromolecular emulsifier is low; by controlling the addition amount of the reversible addition fragmentation transfer reagent, the first auxiliary agent, the second auxiliary agent and the initiator, the influence of copolymerization reactivity rates of different acrylate monomers and VDC monomers on emulsion polymerization is researched. And theoretical support is provided for application of the copolymer in the packaging field.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polyvinylidene chloride, and in particular to an acrylate-vinylidene chloride copolymer emulsion induced by a reversible addition-fragmentation transfer reagent, and a preparation method and application thereof. Background Art

[0002] The molecular formula of polyvinylidene chloride (PVDC) is [CH2-CCl2]n. It has high structural symmetry, good stacking, dense structure and easy crystallization. PVDC homopolymer resin has no application value in actual production due to its processing difficulties. Its processing performance must be improved before it can be widely used. Commercialized PVDC is a type of PVDC copolymer that is copolymerized with VDC as the main component and other second monomers containing unsaturated double bonds (such as vinyl chloride and acrylate). The main types of PVDC copolymers are VDC-VC copolymers, VDC-AN copolymers and Acrylate-VDC copolymers. Acrylate-VDC copolymers are a type of more common PVDC copolymer material in which acrylate is copolymerized with VDC as the second monomer.

[0003] Acrylate-VDC copolymer emulsion has very good storage stability and can be used directly as a varnish. However, when used as a paint, the emulsion will quickly break when alcohol ether additives are added, resulting in the inability to obtain a stable paint. Studies have found that reducing the amount of small molecule emulsifier will make the storage stability of Acrylate-VDC copolymer emulsion worse. The contradiction between the amount of small molecule emulsifier in the stability of VDC-Acrylate copolymer emulsion and its barrier properties after film formation has become one of the main problems hindering its application.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] The object of the present invention is to provide an acrylate-vinylidene chloride copolymer emulsion induced by a reversible addition-fragmentation transfer reagent and a preparation method and application thereof, so as to solve the above technical problems.

[0006] The present invention is achieved in that:

[0007] In the first aspect, an embodiment of the present invention provides a method for preparing an acrylate-vinylidene chloride copolymer emulsion induced by a reversible addition-fragmentation transfer reagent, the preparation method comprising the following steps: reacting acrylate, vinylidene chloride and a first auxiliary agent in an ice-water bath to obtain a pre-emulsion; reacting a reversible addition-fragmentation transfer reagent and a second auxiliary agent at a reaction temperature of 30-40°C to obtain a seed emulsion; adding the pre-emulsion and an initiator to the seed emulsion to react at a reaction temperature of 30-40°C for a reaction time of 10-100 min to obtain a polymer emulsion.

[0008] In a second aspect, an embodiment of the present invention provides a copolymer prepared by the aforementioned preparation method.

[0009] In a third aspect, an embodiment of the present invention provides a use of a copolymer emulsion prepared by the aforementioned preparation method or a copolymer prepared by the aforementioned preparation method in preparing a copolymer film.

[0010] In a fourth aspect, an embodiment of the present invention provides a copolymer emulsion prepared by the aforementioned preparation method or a use of a copolymer prepared by the aforementioned preparation method in preparing packaging materials.

[0011] The present invention has the following beneficial effects:

[0012] An acrylate-vinylidene chloride copolymer emulsion induced by a reversible addition-fragmentation transfer reagent and its preparation method and application. The preparation method introduces a reversible addition-fragmentation transfer reagent to induce the preparation of acrylate-vinylidene chloride copolymers, generates a macromolecular emulsifier in situ, so that the final prepared copolymer has the characteristics of good compatibility and high stability while having a small content of small molecule emulsifiers; by controlling the addition amount of the reversible addition-fragmentation transfer reagent, the first auxiliary agent, the second auxiliary agent and the initiator, the influence of the copolymerization reactivity ratio of different acrylate monomers and VDC monomers on emulsion polymerization is studied. The theoretical support is provided for the application of copolymers in the packaging field. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0014] Figure 1 is the particle size distribution diagram of MA-VDC90;

[0015] Figure 2 As RAFT agent 1 HNMR spectrum;

[0016] Figure 3 The copolymers induced by different addition amounts of RAFT agents 1 HNMR spectrum;

[0017] Figure 4 Characterize the results for FTIR testing;

[0018] Figure 5 XRD test characterization results. DETAILED DESCRIPTION

[0019] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0020] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0021] Polyvinylidene chloride (PVDC) has strong intermolecular cohesion and high crystallinity. The chlorine atoms in the molecules are hydrophobic and will not form hydrogen bonds. Therefore, it is difficult for oxygen molecules and water molecules to move between PVDC macromolecular chains, which makes it have excellent oxygen and moisture barrier properties, and its oxygen barrier properties are not affected by the humidity of the surrounding environment. Due to the high chlorine content and high crystallinity of PVDC homopolymer resin, its melting temperature is high and the melting time is long. In addition, its melting and decomposition temperatures are very close, the melt viscosity is high, the fluidity is poor, and it is easy to degrade when heated; the processing cycle is short, the film is easy to change color, and the heat sealing strength is low; the elastic properties are poor and the processing properties are poor; these shortcomings make PVDC homopolymer resin have no application value in actual production, and its processing properties must be improved before it can be widely used.

[0022] At present, the polymerization methods of PVDC copolymers are mainly suspension polymerization and emulsion polymerization. The latex obtained by emulsion polymerization is convenient and quick to use, can be directly coated, and can effectively solve the problem that PVDC copolymers themselves are difficult to process and shape.

[0023] The study found that reducing the amount of small molecule emulsifier will make the storage stability of Acrylate-VDC copolymer emulsion worse. The contradiction between the amount of small molecule emulsifier in the stability of VDC-Acrylate copolymer emulsion and its barrier properties after film formation has become one of the main problems hindering its application. In view of this, the inventors adopted a strategy of partially replacing small molecule emulsifiers with macromolecular emulsifiers that are not easy to migrate to prepare Acrylate-VDC copolymer emulsions with less small molecule emulsifier content and higher stability, making it more suitable for use as a high barrier film packaging material.

[0024] In the first aspect, an embodiment of the present invention provides a method for preparing an acrylate-vinylidene chloride copolymer (Acrylate-VDC) emulsion induced by a reversible addition-fragmentation transfer reagent, the preparation method comprising the following steps: reacting acrylate, vinylidene chloride and a first auxiliary agent in an ice-water bath to obtain a pre-emulsion; reacting a reversible addition-fragmentation transfer reagent and a second auxiliary agent at a reaction temperature of 30-40°C to obtain a seed emulsion; adding the pre-emulsion and an initiator to the seed emulsion to react at a reaction temperature of 30-40°C for a reaction time of 10-100 min to obtain a copolymer emulsion.

[0025] It should be noted that after the reversible addition-fragmentation transfer reagent is introduced, a macromolecular emulsifier can be generated in situ, thereby partially replacing the small molecule emulsifier to prepare a highly stable copolymer emulsion. The preparation method is a semi-continuous seed emulsion polymerization method for preparing VDC-Acrylate copolymer emulsion.

[0026] In the process of preparing the pre-emulsion, acrylic acid (AA) is also added, and its main function is to help the formation of copolymer segments; in the process of preparing the polymer emulsion, ammonium bicarbonate is also added, and its main function is to provide a weakly acidic environment.

[0027] During the preparation of the seed emulsion, the container needs to be replaced by vacuum-nitrogen cycles three times so that the entire reaction system is finally under a nitrogen atmosphere. The machine speed is set to 250-300 r / min and the temperature is kept constant at 30-40°C in a water bath.

[0028] In an optional embodiment of the present invention, the raw materials of the copolymer emulsion include the following components by mass fraction:

[0029] The acrylate is 0.1%-5%, the vinylidene chloride is 70%-95%, the first auxiliary agent is 1%-10%, the reversible addition-fragmentation transfer agent is 0.03%-5%, the second auxiliary agent is 0.4%-5% and the initiator is 0.04%-5%.

[0030] Furthermore, the acrylate is 0.2%-0.7%, the vinylidene chloride is 70%-90%, the first auxiliary agent is 1.52%-5.53%, the reversible addition-fragmentation transfer agent is 0.031%-0.25%, the second auxiliary agent is 0.45%-0.74% and the initiator is 0.04%-0.4%.

[0031] In an optional embodiment of the present invention, the reversible addition-fragmentation transfer reagent is a RAFT containing a disulfide bond;

[0032] Furthermore, the reversible addition-fragmentation transfer reagent is 2-(dodecyl trithiocarbonate)-2-methylpropionic acid.

[0033] It should be noted that in other embodiments of the present invention, other suitable RAFT containing disulfide bonds can be selected according to actual needs.

[0034] In an optional embodiment of the present invention, the first auxiliary agent includes 2-acrylamide-2-methylpropanesulfonic acid (AMPS).

[0035] In an optional embodiment of the present invention, the second auxiliary agent includes sodium alcohol polyoxyethylene ether sulfate (AES) and sodium dodecyl sulfate (SDS).

[0036] In an optional embodiment of the present invention, the initiator is a redox system, and the initiator includes an oxidant solution and a reducing agent solution in a volume ratio of (1:0.5)-(1:2); the mass concentration of the oxidant solution is 0.04%-0.2%; the mass concentration of the reducing agent solution is 0.05%-0.2%.

[0037] Furthermore, the initiator includes an oxidant solution and a reductant solution in a volume ratio of (1:0.5)-(1:1).

[0038] It should be noted that in an optional embodiment of the present invention, the initiator is prepared as follows: prepare the oxidant solution and the reductant solution of the corresponding mass concentrations as required. In the process of preparing the copolymer emulsion, the initiator is a redox system, and the initiator of the redox system is added in batches according to proportion for reaction. Adding the initiator in batches is conducive to uniform dispersion of the copolymer emulsion; if all of it is added at once, it will cause the emulsion to agglomerate, thereby causing the emulsion to become unstable.

[0039] Furthermore, the oxidant is a peroxide; further, the oxidant used is tert-butyl peroxide; and the reducing agent includes sodium formaldehyde sulfoxylate.

[0040] It should be noted that in other embodiments of the present invention, the material types of the oxidant and the reductant can be reasonably replaced according to actual needs.

[0041] In an optional embodiment of the present invention, the acrylic acid ester is selected from at least one of methyl acrylate (MA), ethyl acrylate (EA) and butyl acrylate (BA).

[0042] In an optional embodiment of the present invention, when preparing the copolymer emulsion, the pre-emulsion is added in multiple times; by weight, the first pre-emulsion is 1%-4%, the second pre-emulsion is 5%-8%, the third pre-emulsion is 2%-5%, and the fourth pre-emulsion is the balance.

[0043] Furthermore, the amount of the first pre-emulsion is 1.6%-3.2%, the amount of the second pre-emulsion is 5.6%-7.2%, the amount of the third pre-emulsion is 2%-3.6%, and the amount of the fourth pre-emulsion is the remainder.

[0044] It should be noted that adding the pre-emulsion in batches is beneficial to the uniform dispersion of the copolymer emulsion; if it is added all at once, the emulsion will agglomerate, thereby causing the emulsion to become unstable.

[0045] In an optional embodiment of the present invention, when preparing the copolymer emulsion, the initiator is added in multiple times; by volume, the first initiator amount is 18%-35%, the second initiator amount is 40%-60%, the first initiator amount is 6%-15%; the fourth initiator amount is 6%-15%.

[0046] Furthermore, the first initiator dosage is 18.75%-31.25%, the second initiator dosage is 43.75%-56.25%, the first initiator dosage is 6.25%-12.5%; and the fourth initiator dosage is 6.25%-12.5%.

[0047] The structure of the copolymer emulsion prepared in the present application is composed of the polymerizable monomer AMPS constituting the hydrophilic unit of the macromolecular emulsifier and the constituent monomers VDC and acrylate as the hydrophobic unit of the macromolecular emulsifier, ensuring that the macromolecular emulsifier has good compatibility with the Acrylate-VDC copolymer emulsion, so that it is not easily replaced by alcohol ethers, and high stability is achieved.

[0048] Acrylate-VDC copolymer emulsion was prepared by semi-continuous seed emulsion polymerization, with a solid content of 55-59wt%; the initial molecular particle size of the prepared copolymer emulsion was 193-249nm, and the molecular particle size after 7 days was 190-250nm. The particle size was almost unchanged, which also shows that the polymer emulsion prepared by the new synthesis scheme has good stability.

[0049] The naming of the compounds in the present invention is as follows: the copolymer emulsion is represented as Acrylate-VDC copolymer emulsion, wherein Acrylate represents acrylate, such as methyl acrylate (MA), ethyl acrylate (EA) and butyl acrylate (BA). It is specifically divided into two categories: one is a copolymer with high VDC content but different acrylate monomers, namely MA-VDC90, EA-VDC90 and BA-VDC90; the other is a copolymer with the same acrylate monomer unit but different VDC content, namely MA-VDC90, MA-VDC85 and MA-VDC80.

[0050] Specifically, the method for preparing an acrylate-vinylidene chloride copolymer emulsion based on reversible addition-fragmentation transfer reagent induction provided in an embodiment of the present invention comprises the following steps:

[0051] Preparation of pre-emulsion: add 0.43%-0.49% fatty alcohol polyoxyethylene ether sodium sulfate aqueous solution (AES) and water according to the ratio and place them in a pear-shaped bottle, place it in an ice water bath and stir vigorously with a magnetic bar to fully emulsify; then add 0.063%-0.25% sodium dodecyl sulfate (SDS), 70%-90% VDC monomer, 0.2%-0.7% acrylate and acrylic acid (AA), and continue to fully emulsify.

[0052] Preparation of initiator: prepare an oxidant solution with a mass concentration of 0.04%-0.2%, wherein the oxidant is tert-butyl peroxide; prepare a reducing agent solution with a mass concentration of 0.05%-0.2%, wherein the reducing agent is sodium formaldehyde sulfoxylate. Mix the oxidant solution and the reducing agent solution in a volume ratio of (1:0.5)-(1:2) to form a redox system for standby use.

[0053] Preparation of seed emulsion: Add 1.52%-5.53% of 2-acrylamide-2-methylpropanesulfonic acid (AMPS) and water in a four-necked flask according to the ratio, and continue to add 0.031%-0.25% of RAFT agent and ammonium bicarbonate (NH4HCO3). Install a polytetrafluoroethylene stirring paddle to the middle mouth of the four-necked flask, install a dropping funnel and a condenser (with a nitrogen balloon at the mouth of the tube) at the other two sides, and seal the other small mouth with a rubber stopper to facilitate the injection of initiator later. The four-necked flask is subjected to three vacuum-nitrogen cycle replacements, and finally placed in a nitrogen atmosphere, the mechanical speed is set to 250-300r / min, and the temperature is constant in a 30-40°C water bath.

[0054] The four-necked flask was subjected to three vacuum-nitrogen cycle replacements and finally placed in a nitrogen atmosphere. The machine speed was set to 250-300 r / min and the temperature was kept constant at 30-40° C. in a water bath.

[0055] Preparation of polymer emulsion: first, by volume fraction, add 1%-4% of pre-emulsion and 18%-35% of initiator to a four-necked bottle kept at a constant temperature in a water bath at 30-40°C; after reacting for 15-20 minutes, add 5%-8% of pre-emulsion; after continuing to react for 0.5-1.5 hours, add 2%-5% of pre-emulsion and 40%-60% of initiator to the seed emulsion; after reacting for 8-15 minutes, add the remaining pre-emulsion; after reacting for 3-4 hours, add 6.25%-12.5% ​​of initiator to continue the reaction; after 3-4 hours, add 6.25%-12.5% ​​of initiator; after 3-5 hours, gradually start to heat up, and the reaction ends when the temperature reaches 50°C and there is no reflux.

[0056] In a second aspect, an embodiment of the present invention provides a copolymer prepared by the aforementioned preparation method.

[0057] In a third aspect, an embodiment of the present invention provides a use of a copolymer emulsion prepared by the aforementioned preparation method or a copolymer prepared by the aforementioned preparation method in preparing a copolymer film.

[0058] In a fourth aspect, an embodiment of the present invention provides a copolymer emulsion prepared by the aforementioned preparation method or a use of a copolymer prepared by the aforementioned preparation method in preparing packaging materials.

[0059] In an optional embodiment of the present invention, the packaging material comprises a copolymer film;

[0060] The initial water permeability of the copolymer film is 1-30g / m 2 ·day, the water permeability after 7 days is 0.8-27g / m 2 ·day; the initial oxygen permeability of the copolymer film is 0-43mL / m 2 day, oxygen permeability after 7 days is 0-40mL / m 2 ·day.

[0061] Furthermore, the initial water permeability of the copolymer film is 1-2.5 g / m 2 ·day, the water permeability after 7 days is 0.8-2g / m 2 ·day; the initial oxygen permeability of the copolymer film is 0-9mL / m 2 day, oxygen permeability after 7 days is 0-6mL / m 2 ·day.

[0062] Example 1

[0063] This embodiment provides an acrylate-vinylidene chloride copolymer emulsion induced by a reversible addition-fragmentation transfer reagent, and the preparation method thereof is as follows:

[0064] Preparation of pre-emulsion: Weigh 2.8 g of 13% fatty alcohol polyoxyethylene ether sodium sulfate aqueous solution (AES) and 44.1 g of deionized water into a 250 mL pear-shaped bottle, place it in an ice-water bath and stir vigorously with a magnetic bar to fully emulsify; then add 0.135 g of sodium dodecyl sulfate (SDS), 66.1 g of VDC monomer, 7.0 g of methyl acrylate (MA), and 1.5 g of acrylic acid (AA), continue to fully emulsify, and prepare a pre-emulsion.

[0065] Preparation of initiator: Weigh 0.160g of tert-butyl peroxide and dissolve it in 2.1g of deionized water to prepare an oxidant solution; weigh 0.100g of sodium formaldehyde sulfoxylate (Diaobaikuai) and dissolve it in 2.2g of deionized water to prepare a reducing agent solution. The oxidant solution and the reducing agent solution are mixed in a volume ratio of 1:1 to form a redox system for later use.

[0066] Preparation of seed emulsion: Weigh 1.6g of 2-acrylamide-2-methylpropanesulfonic acid (AMPS) and 16.2g of water into a 250mL four-necked flask, and continue to add 0.050g of RAFT agent and 0.570g of ammonium bicarbonate (NH4HCO3). Install a polytetrafluoroethylene stirring paddle to the middle of the four-necked flask, install a dropping funnel and a condenser (with a nitrogen balloon at the mouth of the tube) on the other two sides, and seal the other small mouth with a rubber stopper to facilitate the later injection of the initiator (composed of the previous oxidant solution and the reductant solution, with a ratio of 1:1). Prepare the bottom of the pot.

[0067] The four-necked flask was subjected to three vacuum-nitrogen cycle replacements and finally placed in a nitrogen atmosphere. The mechanical speed was set to 280 r / min and the temperature was kept constant at 36° C. in a water bath.

[0068] First, add 6 mL of pre-emulsion and 0.5 mL of initiator to a four-necked bottle kept at a constant temperature in a 36°C water bath; after reacting for 20 minutes, add another 16 mL of pre-emulsion; after continuing to react for 1 hour, add 7 mL of pre-emulsion and 1 mL of initiator to the bottom of the pot; after reacting for 10 minutes, slowly add the remaining pre-emulsion dropwise for about 50 minutes; after 2.5 hours, add an additional 0.125 mL of initiator; after 3.5 hours, add an additional 0.125 mL of initiator; after 4 hours, gradually start to heat up, and the reaction is completed when the temperature reaches 50°C and there is no reflux.

[0069] The prepared polymer emulsion was recorded as MA-VDC90.

[0070] Example 2

[0071] This embodiment provides an acrylate-vinylidene chloride copolymer emulsion induced by a reversible addition-fragmentation transfer agent, and the preparation method thereof is different from that of embodiment 1 only in that:

[0072] Preparation of pre-emulsion: 62.3 g of VDC monomer.

[0073] The prepared polymer emulsion was recorded as MA-VDC85.

[0074] Example 3

[0075] This embodiment provides an acrylate-vinylidene chloride copolymer emulsion induced by a reversible addition-fragmentation transfer agent, and the preparation method thereof is different from that of embodiment 1 only in that:

[0076] Preparation of pre-emulsion: 58.6 g of VDC monomer.

[0077] The prepared polymer emulsion was recorded as MA-VDC80.

[0078] Example 4

[0079] This embodiment provides an acrylate-vinylidene chloride copolymer emulsion induced by a reversible addition-fragmentation transfer agent, and the preparation method thereof is different from that of embodiment 1 only in that:

[0080] Preparation of pre-emulsion: ethyl acrylate (EA) 7.0 g.

[0081] The prepared polymer emulsion was recorded as EA-VDC90.

[0082] Example 5

[0083] This embodiment provides an acrylate-vinylidene chloride copolymer emulsion induced by a reversible addition-fragmentation transfer agent, and the preparation method thereof is different from that of embodiment 2 only in that:

[0084] Preparation of pre-emulsion: ethyl acrylate (EA) 7.0 g.

[0085] The prepared polymer emulsion was recorded as EA-VDC85.

[0086] Example 6

[0087] This embodiment provides an acrylate-vinylidene chloride copolymer emulsion induced by a reversible addition-fragmentation transfer reagent, and the preparation method thereof is different from that of embodiment 3 only in that:

[0088] Preparation of pre-emulsion: ethyl acrylate (EA) 7.0 g.

[0089] The prepared polymer emulsion was recorded as EA-VDC80.

[0090] Example 7

[0091] This embodiment provides an acrylate-vinylidene chloride copolymer emulsion induced by a reversible addition-fragmentation transfer agent, and the preparation method thereof is different from that of embodiment 1 only in that:

[0092] Preparation of pre-emulsion: 7.0 g of butyl acrylate (BA).

[0093] The prepared polymer emulsion was recorded as BA-VDC90.

[0094] Example 8

[0095] This embodiment provides an acrylate-vinylidene chloride copolymer emulsion induced by a reversible addition-fragmentation transfer agent, and the preparation method thereof is different from that of embodiment 2 only in that:

[0096] Preparation of pre-emulsion: 7.0 g of butyl acrylate (BA).

[0097] The prepared polymer emulsion was recorded as BA-VDC85.

[0098] Example 9

[0099] This embodiment provides an acrylate-vinylidene chloride copolymer emulsion induced by a reversible addition-fragmentation transfer reagent, and the preparation method thereof is different from that of embodiment 3 only in that:

[0100] Preparation of pre-emulsion: 7.0 g of butyl acrylate (BA).

[0101] The prepared polymer emulsion was recorded as BA-VDC80.

[0102] Comparative Example 1

[0103] This comparative example provides an acrylate-vinylidene chloride copolymer emulsion, which differs from Example 1 only in that:

[0104] Preparation of initiator: Dissolve 0.2 g of ammonium disulfate in 2 mL of secondary water to prepare an oxidant solution, and dissolve 0.14 g of sodium bisulfite in 2 mL of secondary water to prepare a reducing agent solution.

[0105] The reaction rate of this preparation method is slower than that of Example 1.

[0106] Test Example 1

[0107] This test example is used to optimize the amount of raw materials used in the preparation of acrylate-vinylidene chloride copolymer emulsion. The specific formula and related data are shown in Table 1.

[0108] Table 1

[0109]

[0110]

[0111] Note: "○" indicates no precipitation or good stability; "×" indicates precipitation or poor stability (appearing below, indicating the same).

[0112] As can be seen from Table 1, in formula 1, which contains 2.53% AMPS, 0.25% RAFT, 0.49% AES and 0.25% SDS, there is no precipitation in the obtained copolymer emulsion. After adding ethylene glycol butyl ether, the emulsion breaks and becomes unstable; in formulas 2 and 3, as the amount of AMPS decreases, the emulsion still becomes unstable; starting from formula 4, as the amount of AMPS in the bottom of the pot continues to decrease, precipitation will occur; the results of formula 5 are similar to those of formula 4. From formulas 1-5, it can be concluded that although the amount of AMPS in the bottom of the pot can be reduced, there is a lower limit, that is, the minimum amount of 2.03% can ensure that there is no coagulation during the emulsion polymerization process. Formulas 6-10 are the optimization of the amount of SDS. As the amount of SDS decreases, coagulation begins to occur in the emulsion; as in formulas 9 and 10, the emulsion has coagulation. From formulas 6-10, it can be seen that the amount of SDS in the pre-emulsion also has a lower limit, and its lower limit is 0.17%. This conclusion can also be verified by experimental observation: as the amount of SDS in the pre-emulsified liquid decreases, the pre-emulsification effect of VDC and MA in the ice bath becomes significantly worse, resulting in the inability to observe the blueing of the emulsion in the four-necked flask during polymerization. This further indicates that the number of nuclei in the polymerization process is relatively small, the particle size of the resulting copolymer latex particles is large, and finally coagulation occurs. Formulas 11-14 studied the effect of the amount of RAFT agent on the properties of the emulsion. As can be seen from Table 1, the reason why formulas 1-10 can partially show no coagulation phenomenon is attributed to the addition of sufficient RAFT agents. Similar to the rules of other emulsifiers, as the amount of RAFT agent decreases, the coagulation of the emulsion occurs in formula 14, and it is also concluded that the minimum lower limit of the amount of RAFT agent is 0.063%. Formulas 15 and 16 mainly study the effect of the AES content in the pre-emulsified liquid. As can be seen from the table, the optimal amount of AES is 0.46%. In the optimized formula 15, the total amount of AES and SDS small molecule emulsifiers is 0.73%, which is only about one-fourth of the small molecule emulsifier in the previous formula. It can be further inferred that the introduction of the macromolecular emulsifier with good compatibility with the Acrylate-VDC copolymer latex particles and low mobility is the main reason for the high stability of the Acrylate-VDC copolymer emulsion.

[0113] Test Example 2

[0114] In order to reduce the generation of inorganic salts, the embodiment of the present invention replaces the redox initiator, the new oxidant is tert-butyl peroxide solution, and the reducing agent is bleaching solution. Because the emulsion polymerization is semi-continuous seed emulsion polymerization, the amount of initiator added will have a greater impact on the polymerization reaction. In the emulsion polymerization process, the initiator is added 4 times. This test example is used to optimize the amount of initiator used each time in the preparation of acrylate-vinylidene chloride copolymer emulsion. The specific formula and related data are shown in Table 2.

[0115] Table 2

[0116]

[0117] As can be seen from Table 2, the main difference in formula 1-2 is the amount of initiator added for the first time. Compared with formula 7, if the amount of initiator added increases, coagulation is likely to occur in the emulsion. If the amount of initiator added is reduced, a stable emulsion without coagulation can be obtained, but the emulsion polymerization reaction time will be prolonged. Formula 3-4 mainly studies the effect of the second amount of initiator added on the emulsion polymerization reaction. The amount of initiator added this time is the largest, so it has a greater impact on the entire reaction. Compared with formula 7, the emulsion in formula 3 coagulates and has poor stability. Although there is no coagulation phenomenon and the emulsion is stable in formula 4, the polymerization reaction time is extended by 1.5h. Compared with formula 7, formulas 5 and 6 increase the third and fourth amounts of initiator added, respectively, and the emulsions coagulate and have poor stability. After optimization, formula 7 is the optimal amount of initiator added.

[0118] In summary, based on the addition amount of the auxiliary agent formula 15 in Test Example 1 and the initiator formula 7 in Test Example 2, a series of Acrylate-VDC copolymer emulsions were prepared, including methyl acrylate-vinylidene chloride (MA-VDC), ethyl acrylate-vinylidene chloride (EA-VDC) and butyl acrylate-vinylidene chloride (BA-VDC).

[0119] Test Example 3

[0120] This test example is used to analyze the copolymerization reactivity ratios of different acrylate monomers and VDC monomers.

[0121] When preparing Acrylate-VDC copolymer, the feed amount of VDC monomer is much larger than that of acrylate monomer, so as to ensure that the obtained Acrylate-VDC copolymer has a high VDC unit content, and there will be many VDC homopolymer segments in its microstructure. By analyzing the copolymerization reactivity data of different acrylate monomers and VDC monomers, we can understand the influence of different acrylate monomers on the microstructure of Acrylate-VDC copolymer, especially the influence on the length of VDC homopolymer segments in the copolymer. The relevant data are summarized in Table 3.

[0122] Table 3

[0123] Acrylate copolymer <![CDATA[r Acrylate ]]> <![CDATA[r VDC ]]> <![CDATA[r Acrylate r VDC ]]> MA 0.900 0.950 0.855 EA 0.580 0.720 0.418 BA 0.870 0.940 0.818

[0124] As can be seen from Table 3, the reactivity ratio values ​​of all acrylate monomers and VDC monomers are less than 1, indicating that the copolymerization tendency between different monomers when acrylate monomers and VDC monomers are copolymerized is greater than the homopolymerization tendency between the same monomers. When the reactivity ratio product of different monomers of Acrylate-VDC copolymer (racrylaterVDC) is 1, the composition of the two monomer units in the copolymer is completely consistent with the feed ratio of the two monomers, and the fewer acrylate monomer units will be evenly dispersed in the molecular chain mainly composed of more VDC monomer units. When the reactivity ratio product of different monomers of Acrylate-VDC copolymer (racrylaterVDC) is 0, the acrylate monomers and VDC monomers tend to be alternately polymerized. All racrylaterVDC values ​​are between 0 and 1. When the acrylate is MA and BA, the racrylaterVDC is greater than 0.8, closer to 1, indicating that MA or BA can be more evenly distributed in the PVDC chain segment after polymerization as a small amount of comonomers, resulting in a relatively uniform length of the VDC homopolymer segment in the MA-VDC or BA-VDC copolymer. When EA is used as a comonomer, racrylaterVDC is around 0.4, closer to 0. This indicates that EA is unevenly distributed in the PVDC chain segment after polymerization as a small amount of comonomer, that is, the average distance between EA units is smaller than the average distance between MA or BA units, which results in not only short VDC homopolymer segments but also long VDC homopolymer segments that are easier to crystallize in the EA-VDC copolymer.

[0125] Test Example 4

[0126] This test example is used to analyze the particle size distribution of the polymer emulsion prepared in Examples 1-9. Specifically, the particle size of the emulsion is tested using a nanometer particle size analyzer and a zeta potential analyzer. Each particle size is tested 5 times and the average value is taken. The specific results are shown in Tables 4 and Figure 1 .

[0127] It should be noted that the copolymer emulsion was left for 7 days to reach equilibrium.

[0128] Table 4

[0129]

[0130] As shown in Table 4, at the same VDC content, the particle size of the polymer latex particles obtained by copolymerization of ethyl acrylate is the largest. The particle size of the latex particles obtained by polymerization of the same acrylate decreases with the increase of VDC content. After the emulsion is placed for 7 days, the change of the particle size of the polymer latex particles before and after is compared, and it is found that it is almost unchanged, which also shows that the polymer latex emulsion prepared by the new synthesis scheme has good stability.

[0131] In addition, MA-VDC90 (wherein the VDC content is 90%) is taken as an example. Figure 1 It can be seen that the maximum particle size of the emulsion is distributed at 203nm, which is similar to the particle size of the latex synthesized by the research group in the early stage (208nm). This shows that the emulsion obtained by the emulsion polymerization formula induced by the RAFT agent can meet the evaluation requirements of the early coating-grade emulsion, which further illustrates the feasibility of the new synthesis method.

[0132] Test Example 5

[0133] This test example is used to verify whether RAFT is synthesized or not, and the effect of different RAFT agent dosages on the stability of the polymer emulsion. Specifically, the copolymer emulsion induced by different RAFT agent addition amounts is subjected to NMR testing. 1 HNMR spectrum: Figure 2 A typical RAFT agent 1 HNMR spectra and Figure 3 Typical copolymers induced by different RAFT agent addition amounts 1 HNMR spectrum.

[0134] from Figure 2 It can be seen that the peaks at h, g, i, and j are clearly found in the spectrum, and the integral ratio is consistent with the ratio of hydrogen in the structural formula, proving that the RAFT agent was successfully synthesized.

[0135] from Figure 3 It can be seen that a is the characteristic peak corresponding to AMPS, b, c, d are the characteristic peaks corresponding to MA, and e is the characteristic peak corresponding to VDC. Based on this, when the RAFT agent content is 0.031%, the ratio of AMPS, MA and VDC is: 1:2.1:0.32; when the RAFT agent content is 0.063%, the ratio of AMPS, MA and VDC is: 1:2:1.2; when the RAFT agent content is 0.19%, the ratio of AMPS, MA and VDC is: 1:1.46:0.33. In summary, when the RAFT agent content is 0.063%, the hydrophobic blocks VDC and MA are longer, making their hydrophilicity worse and eventually completely fixed on the surface of the formed polymer latex, so that they will not be replaced by other substances and cause the polymer latex emulsion to become unstable.

[0136] Test Example 6

[0137] This test example is used to test the water and oxygen permeability of the copolymer film prepared by the copolymer emulsion of Examples 1-9. The specific test method is as follows: Oxygen permeability test parameter settings: carrier gas: 99.999% N2, 99.999% O2, test area: 25 cm 2 , oxygen concentration: 100%;

[0138] Water vapor transmission rate test parameter settings: carrier gas: 99.999% N2, temperature: 38°C, humidity: 100% RH, test area: 25 cm 2 .

[0139] The relevant results are shown in Table 5.

[0140] Table 5

[0141]

[0142] From the data in Table 5, it can be seen that the water permeability and oxygen permeability values ​​of the same type of acrylic copolymers increase with the decrease of VDC content. After 7 days of aging, the water permeability and oxygen permeability values ​​of the films decrease. This shows that the crystallinity of the aging film is enhanced, which is conducive to better water and oxygen barrier properties of the film. Among the different acrylic copolymers, VDC-MA has the best water and oxygen barrier properties, and VDC-BA has the worst barrier properties.

[0143] Test Example 7

[0144] This test example is used to verify the crystallinity of the copolymer emulsion prepared in Examples 1-9, wherein the chemical structure of the film is characterized using a Thermo Fisher (IS50) Fourier transform infrared spectrometer. The parameters are set as follows: scanning range 500-4500nm. The copolymer film is tested using a German BRUKER D8 Focus X-ray diffractometer (Cu target). The parameters are set as follows: scanning speed 4° / min, sampling step width 0.02°, and scanning angle 5°≤2θ≤40°.

[0145] The test results are as follows: Figure 4 The results of FTIR test are as follows: Figure 5 XRD test characterization results.

[0146] exist Figure 4 (A) 1070cm -1 and 1044cm -1 They correspond to the C-Cl vibration peaks in the amorphous and crystalline states of the copolymer, and are also the infrared characteristic peaks of the copolymer. When the mass fraction of VDC is 90%, the characteristic peak will not change with the change of acrylic acid type. Figure 4 (B) It can be seen that for the same type of acrylates, the characteristic peaks will weaken as the VDC content decreases, especially the characteristic peaks corresponding to the crystalline region change more obviously, indicating that the presence of VDC has a huge contribution to the crystallinity of the entire copolymer matrix.

[0147] from Figure 5(A) It can be seen that the VDC-Acrylate copolymer has characteristic crystallization peaks in the XRD spectrum, which are located at 15.5°, 24.6° and 31.0°~35.0°, and the crystallization peaks do not change with the change of the type of acrylate. Figure 5 (B) It can be seen that in the VDC-MA copolymer, the characteristic peaks weaken with the decrease of VDC content, especially when the VDC content drops to 80%, the peaks at 24.6° and 31.0°~35.0° disappear, which is consistent with the peak at 1044cm in the infrared spectrum. -1 The peak weakening of the crystalline state is consistent with that of the copolymer film, which will also lead to the weakening of the rigidity of the copolymer film.

[0148] In summary, the present invention provides an acrylate-vinylidene chloride copolymer emulsion induced by a reversible addition-fragmentation transfer reagent, and a preparation method and application thereof. The preparation method introduces a reversible addition-fragmentation transfer reagent to induce the preparation of an acrylate-vinylidene chloride copolymer, generates a macromolecular emulsifier in situ, and makes the final prepared copolymer have the characteristics of good compatibility and high stability while having a small content of a small molecule emulsifier; and controls the addition amount of the reversible addition-fragmentation transfer reagent, the first auxiliary agent, the second auxiliary agent and the initiator to study the influence of different copolymerization reactivity ratios of acrylate monomers and VDC monomers on emulsion polymerization. This provides theoretical support for the application of copolymers in the field of packaging.

[0149] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing an acrylate-vinylidene chloride copolymer emulsion induced by a reversible addition-fragmentation transfer reagent, characterized in that: The preparation method comprises the following steps: reacting acrylate, vinylidene chloride and the first auxiliary agent in an ice water bath to prepare a pre-emulsion; The reversible addition-fragmentation transfer reagent and the second auxiliary agent are reacted at a reaction temperature of 30-40° C. to obtain a seed emulsion; The pre-emulsion and the initiator are added to the seed emulsion for reaction at a temperature of 30-40° C. and a reaction time of 10-100 min to obtain the copolymer emulsion.

2. The preparation method according to claim 1, characterized in that: The raw materials of the copolymer emulsion include the following components by mass fraction: Acrylate is 0.1%-5%, vinylidene chloride is 70%-95%, the first auxiliary agent is 1%-10%, the reversible addition-fragmentation transfer agent is 0.03%-5%, the second auxiliary agent is 0.4%-5% and the initiator is 0.04%-5%; Preferably, the acrylate is 0.2%-0.7%, the vinylidene chloride is 70%-90%, the first auxiliary agent is 1.52%-5.53%, the reversible addition-fragmentation transfer agent is 0.031%-0.25%, the second auxiliary agent is 0.45%-0.74% and the initiator is 0.04%-0.4%.

3. The preparation method according to claim 1, characterized in that: The reversible addition-fragmentation transfer reagent is a RAFT containing a disulfide bond; Preferably, the reversible addition-fragmentation transfer reagent is 2-(dodecyl trithiocarbonate)-2-methylpropionic acid; Optionally, the first auxiliary agent includes 2-acrylamide-2-methylpropane sulfonic acid; Optionally, the second auxiliary agent includes sodium fatty alcohol polyoxyethylene ether sulfate and sodium dodecyl sulfate.

4. The preparation method according to claim 1, characterized in that: The initiator is a redox system, and the initiator comprises an oxidant solution and a reductant solution in a volume ratio of (1:0.5)-(1:2); The mass concentration of the oxidant solution is 0.04%-0.2%; the mass concentration of the reductant solution is 0.05%-0.2%; Preferably, the oxidizing agent is a peroxide; preferably tert-butyl peroxide; Reducing agents include sodium formaldehyde sulfoxylate.

5. The preparation method according to claim 1, characterized in that: The acrylic acid ester is selected from at least one of methyl acrylate, ethyl acrylate and butyl acrylate.

6. The preparation method according to claim 1, characterized in that: When preparing the copolymer emulsion, the pre-emulsion is added in multiple times; by weight, the first pre-emulsion is 1%-4%, the second pre-emulsion is 5%-8%, the third pre-emulsion is 2%-5%, and the fourth pre-emulsion is the balance; Preferably, the first pre-emulsion is used in an amount of 1.6%-3.2%, the second pre-emulsion is used in an amount of 5.6%-7.2%, the third pre-emulsion is used in an amount of 2%-3.6%, and the fourth pre-emulsion is the remainder; When preparing the copolymer emulsion, the initiator is added in multiple times; by weight, the first initiator dosage is 18%-35%, the second initiator dosage is 40%-60%, the third initiator dosage is 6%-15%; and the fourth initiator dosage is 6%-15%; Preferably, the first initiator dosage is 18.75%-31.25%, the second initiator dosage is 43.75%-56.25%, the third initiator dosage is 6.25%-12.5%; and the fourth initiator dosage is 6.25%-12.5%.

7. A copolymer obtained by the preparation method according to any one of claims 1 to 6.

8. Use of the copolymer emulsion prepared by the preparation method according to any one of claims 1 to 6 or the copolymer according to claim 7 in preparing a copolymer film.

9. Use of the copolymer emulsion obtained by the preparation method according to any one of claims 1 to 6 or the copolymer according to claim 7 in the preparation of packaging materials.

10. The use according to claim 9, characterized in that: The packaging material includes a copolymer film; The initial water permeability of the copolymer film is 1-30 g / m 2 ·day, the water permeability after 7 days is 0.8-27g / m 2 ·day; the initial oxygen permeability of the copolymer film is 0-43mL / m 2 day, oxygen permeability after 7 days is 0-40mL / m 2 day; Preferably, the initial water permeability of the copolymer film is 1-2.5 g / m 2 ·day, the water permeability after 7 days is 0.8-2g / m 2 ·day; the initial oxygen permeability of the copolymer film is 0-9mL / m 2 day, oxygen permeability after 7 days is 0-6mL / m 2 ·day.