Water-retaining agent and preparation method thereof

By introducing non-ionic monomers and salt-resistant functional additives into the soil water retention agent, and using photo-induced and high temperature to initiate polymerization reactions, the problems of low water absorption and poor salt resistance in the soil are solved, and high efficiency is achieved. Preparation of low-energy-consuming water retention agents, suitable for large-scale applications.

CN118878732AActive Publication Date: 2024-11-01JIANGSU SAILBOAT PETROCHEMICAL CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411108323.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-01
Estimated Expiration
2044-08-13

AI Technical Summary

Technical Problem

The existing soil water retention agent has low water absorption rate and poor salt resistance in soils with high ion concentrations, making it difficult to maintain good water absorption in a brine environment.

Method used

By combining acrylic acid with a nonionic monomer and a salt-resistant functional additive, polymerization reaction is carried out, and a two-step polymerization reaction is initiated by using photo-induced and high temperature to initiate a two-step polymerization reaction, a water retention agent with high salt resistance and water absorption is prepared.

Benefits of technology

It significantly improves the salt resistance and water absorption of water retention agents, reduces the energy consumption and cost of the preparation process, and is suitable for large-scale promotion and application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118878732A_ABST
    Figure CN118878732A_ABST
Patent Text Reader

Abstract

The invention provides a water-retaining agent and a preparation method thereof, and the preparation method at least comprises the following steps: dissolving acrylic acid in a solvent, and adding an alkaline solution and at least one nonionic monomer into the acrylic acid solution to obtain an intermediate solution; adding a cross-linking agent and an initiator into the intermediate solution; the initiator initiates the acrylic acid and the nonionic monomer to be subjected to a polymerization reaction, and gel is obtained; and drying, crushing and screening the gel to obtain the water-retaining agent. According to the water-retaining agent and the preparation method thereof provided by the invention, the salt tolerance and water absorption of the water-retaining agent can be improved, and the preparation process is simple, efficient, safe and low in energy consumption.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of soil water retaining agent, in particular to a water retaining agent and a preparation method thereof. Background Art

[0002] Soil water retainers are mostly based on acrylic acid as the main monomer. Although they have good water absorption performance, they are greatly affected by ionic strength and have poor salt resistance. The water absorption multiple of commercially available water retainers in 0.9wt% sodium chloride aqueous solution is generally lower than 40g / g, and soil water contains more ions, so the water absorption rate of water retainers in soil will be lower. Therefore, in order to achieve a certain water absorption effect of water retainers in soil, it is particularly important to improve the salt resistance of soil water retainers. Summary of the invention

[0003] In view of the above-mentioned shortcomings of the prior art, the object of the present invention is to provide a water-retaining agent and a preparation method thereof, which can significantly improve the salt resistance and water absorption of the water-retaining agent, and the preparation process is simple, efficient, safe and low in energy consumption.

[0004] To solve the above technical problems, the present invention is implemented through the following technical solutions.

[0005] The present invention provides a method for preparing a water-retaining agent, which comprises at least the following steps:

[0006] dissolving acrylic acid in a solvent, and adding an alkaline solution and at least one nonionic monomer to the acrylic acid solution to obtain an intermediate solution;

[0007] adding a crosslinking agent and an initiator to the intermediate solution;

[0008] The initiator initiates a polymerization reaction between the acrylic acid and the nonionic monomer to obtain a gel; and

[0009] The gel is dried, crushed and sieved to obtain a water retaining agent.

[0010] In one embodiment of the present invention, the nonionic monomer includes at least one of methyl methacrylate, ethyl acrylate, butyl acrylate, isooctyl acrylate, acrylamide and hydroxyethyl methacrylate.

[0011] In one embodiment of the present invention, the initiator includes a photoinitiator and a high temperature initiator.

[0012] In one embodiment of the present invention, a salt-resistant functional additive is further added to the intermediate solution.

[0013] In one embodiment of the present invention, the salt-resistant functional additive includes at least one of inorganic phosphates, and the inorganic phosphates include sodium hypophosphite, calcium hypophosphite, ammonium hypophosphite, nickel hypophosphite, cobalt hypophosphite and iron hypophosphite. The mass of the inorganic phosphate is 0.001%-0.1% of the total mass of the acrylic acid and the non-ionic monomer.

[0014] In one embodiment of the present invention, the salt-resistant functional additive comprises a hydrophilic polymer material, and the hydrophilic polymer material comprises at least one of 2,2,6,6-tetramethylpyridine-1-oxyl free radical oxidized cellulose, carboxymethyl cellulose, carboxymethyl starch, hydroxyethyl cellulose and carboxymethyl chitosan, and the mass of the hydrophilic polymer material is 0.005%-5% of the total mass of the acrylic acid and the non-ionic monomer.

[0015] In one embodiment of the present invention, the salt-resistant functional additive comprises a hydrophilic functional filler, the hydrophilic functional filler comprises at least water-absorbing resin particles, and the mass of the hydrophilic functional filler is 0.01%-5% of the total mass of the acrylic acid and the non-ionic monomer.

[0016] In one embodiment of the present invention, the preparation of the water-absorbent resin particles comprises at least the following steps:

[0017] adding an alkaline solution and at least one nonionic monomer to an acrylic acid solution to obtain an intermediate solution;

[0018] adding a crosslinking agent and an initiator to the intermediate solution;

[0019] The initiator initiates a polymerization reaction between the acrylic acid and the nonionic monomer to obtain a gel;

[0020] Drying, crushing and sieving the gel to obtain water-retaining agent powder; and

[0021] The water-absorbent resin particles are obtained by forming a coating layer on the surface of the water-retaining agent fine powder.

[0022] In one embodiment of the present invention, the coating at least includes propylene glycol, ethylene glycol diglycidyl ether, sorbitan glycidyl ether and metal ions.

[0023] The present invention also provides a water-retaining agent obtained by any of the above preparation methods.

[0024] In summary, the present invention provides a water-retaining agent and a preparation method thereof, which can significantly reduce the sensitivity of the water-retaining agent to salt and improve the salt resistance and water absorption of the water-retaining agent. Moreover, the preparation method of the water-retaining agent provided by the present invention has the advantages of simple process, efficient production and process safety, and can also make full use of the reaction heat in the preparation process, effectively reduce the energy consumption of the preparation process, thereby reducing the preparation cost of the water-retaining agent, and is suitable for large-scale promotion and application.

[0025] Of course, any method of implementing the present invention does not necessarily need to achieve all of the advantages mentioned above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0027] Figure 1 The present invention provides a schematic flow diagram of a method for preparing a water-retaining agent.

[0028] Figure 2 for Figure 1 Schematic diagram of the process for preparing a medium salt-tolerant functional additive. DETAILED DESCRIPTION

[0029] The following describes the embodiments of the present invention by specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. It should be noted that the following embodiments and features in the embodiments can be combined with each other without conflict.

[0030] It should be understood that the present invention can be implemented in different forms and should not be interpreted as limited to the embodiments set forth herein. On the contrary, these embodiments are provided to make the disclosure thorough and complete and to fully convey the scope of the present invention to those skilled in the art.

[0031] The technical solution of the present invention is further described in detail below in conjunction with the embodiments and drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0032] See also Figure 1As shown, the present invention provides a method for preparing a water-retaining agent, which at least includes steps S11-S14.

[0033] S11, dissolving acrylic acid in a solvent, and adding an alkaline solution and at least one non-ionic monomer to the acrylic acid solution to obtain an intermediate solution.

[0034] S12, adding a crosslinking agent and an initiator to the intermediate solution.

[0035] S13, the initiator initiates a polymerization reaction between acrylic acid and non-ionic monomers to obtain a gel.

[0036] S14, drying, crushing and sieving the gel to obtain a water-retaining agent.

[0037] See also Figure 1 As shown, in one embodiment of the present invention, in step S11, acrylic acid is dissolved in a solvent to obtain an acrylic acid solution. The solvent includes, for example, deionized water or purified water, etc., and the mass of acrylic acid in the acrylic acid solution accounts for, for example, 25%-35%. After acrylic acid is dissolved in the solvent, for example, the acrylic acid and the solvent are homogenized to obtain an acrylic acid solution with uniform composition. In this embodiment, the homogenization treatment is, for example, at least one of stirring and ultrasound.

[0038] See also Figure 1As shown, in one embodiment of the present invention, in step S11, after obtaining the acrylic acid solution, an alkaline solution and at least one non-ionic monomer are added to the acrylic acid solution to obtain an intermediate solution. Wherein, the mass of the non-ionic monomer in the intermediate solution accounts for 5%-15%, the mass of the alkaline solution accounts for 5%-30%, the mass of the alkaline solution and the non-ionic monomer in the intermediate solution accounts for 20%-35%, the alkaline solution includes at least one of potassium hydroxide aqueous solution and sodium hydroxide aqueous solution, the concentration of the alkaline solution is 40wt%-50wt%, the alkaline solution neutralizes 70wt%-80wt% of acrylic acid, the non-ionic monomer includes at least one of methyl methacrylate, ethyl acrylate, butyl acrylate, isooctyl acrylate, acrylamide and hydroxyethyl methacrylate, and the temperature of the intermediate solution is 15℃-20℃. Moreover, in the present embodiment, the alkaline solution and the nonionic monomer are added to the acrylic acid solution successively, for example, in the intermediate solution, the alkaline solution and the acrylic acid release heat due to the neutralization reaction, and the nonionic monomer dissolves and absorbs heat. By adding the alkaline solution and the nonionic monomer to the acrylic acid solution at the same time, the energy loss in the intermediate solution preparation process can be saved, the temperature of the intermediate solution can be better controlled, and the subsequent polymerization reaction can be ensured to proceed smoothly. By adding the nonionic monomer, the sensitivity of the water retaining agent to salt can be reduced, thereby significantly improving the salt resistance of the water retaining agent. Moreover, in the present embodiment, for example, two nonionic monomers are added to the acrylic acid solution, and the two nonionic monomers are added to the acrylic acid solution at the same time, forming a ternary copolymer system of acrylic acid-nonionic monomer-nonionic monomer. The ternary copolymer system has better salt resistance than the binary copolymer system, thereby further improving the salt resistance and water absorption of the water retaining agent.

[0039] See also Figure 1 As shown, in one embodiment of the present invention, in step S12, after obtaining the intermediate solution, a crosslinking agent and an initiator are added to the intermediate solution. The crosslinking agent includes, for example, at least one of ethylene glycol, ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, polyethylene glycol diacrylate, and N, N-methylenebisacrylamide, and the mass of the crosslinking agent is, for example, 0.01%-1% of the total mass of acrylic acid and non-ionic monomers. By adding the crosslinking agent, a strong chemical bond can be formed between the water retaining agent and the soil, and the adhesion of the water retaining agent can be improved, which is convenient for the molding of the water retaining agent.

[0040] See also Figure 1As shown, in one embodiment of the present invention, in step S12, the initiator includes, for example, a photoinitiator and a high-temperature initiator. The photoinitiator includes, for example, at least one of benzoin and its derivatives, benzil and its derivatives, acetophenone derivatives, α-hydroxyketone derivatives, α-aminoalkylacetophenone and acylphosphine oxide compounds, and the mass of the photoinitiator is, for example, 0.001%-1% of the total mass of acrylic acid and non-ionic monomers, and the high-temperature initiator includes, for example, sodium persulfate, potassium persulfate, ammonium persulfate, 2,2-azobisisobutylamidine dihydrochloride, 2,2'-azobis(2-methylpropylimidamide) dihydrochloride, and the mass of the high-temperature initiator is, for example, 0.01%-1% of the total mass of acrylic acid and non-ionic monomers.

[0041] See also Figure 1 As shown, in another embodiment of the present invention, in step S12, a salt-resistant functional aid is also added to the intermediate solution. Wherein, the salt-resistant functional aid is, for example, a composite, and the salt-resistant functional aid includes, for example, at least one of inorganic phosphate, hydrophilic polymer material, and hydrophilic functional filler. By adding the salt-resistant functional aid, the water-retaining agent can have good salt resistance and gel strength. In this embodiment, the salt-resistant functional aid includes, for example, inorganic phosphate, hydrophilic polymer material, and hydrophilic functional filler. Wherein, the inorganic phosphate includes, for example, at least one of sodium hypophosphite, calcium hypophosphite, ammonium hypophosphite, nickel hypophosphite, cobalt hypophosphite, and iron hypophosphite, and the mass of the inorganic phosphate is, for example, 0.001%-0.1% of the total mass of acrylic acid and non-ionic monomers, and the inorganic phosphate group can enable the water-retaining agent to form a better three-dimensional network structure during the reaction. In this embodiment, the hydrophilic polymer material includes at least one of 2,2,6,6-tetramethylpyridine-1-oxyl free radical oxidized cellulose, carboxymethyl cellulose, carboxymethyl starch, hydroxyethyl cellulose and carboxymethyl chitosan, and the mass of the hydrophilic polymer material is, for example, 0.005%-5% of the total mass of acrylic acid and non-ionic monomers, and the hydrophilic polymer material has a high hydroxyl content. Since both the hydrophilic polymer material and the hydrophilic functional filler have hydrophilic groups, the salt resistance and water absorption of the water retaining agent can be improved.

[0042] See also Figure 1 to Figure 2 As shown, in one embodiment of the present invention, the hydrophilic functional filler includes at least water-absorbent resin particles, and the water-absorbent resin particles have a high degree of crosslinking, and the mass of the hydrophilic functional filler is, for example, 0.01%-5% of the total mass of acrylic acid and non-ionic monomers. In this embodiment, the preparation steps of the water-absorbent resin particles, for example, include steps S121-S125, wherein steps S121-S124 are the same as steps S11-S14, and are not further elaborated here.

[0043] See also Figure 1 to Figure 2As shown, in one embodiment of the present invention, after obtaining the water-retaining agent powder in step S124, in step S125, a coating is formed on the surface of the water-retaining agent powder to obtain water-absorbent resin particles. By subjecting the sieved water-retaining agent powder to surface cross-linking treatment and then reusing it as a hydrophilic functional filler, the gel strength of the water-retaining agent can be improved on the one hand, and the material loss can be reduced on the other hand, thereby improving the utilization rate of the water-retaining agent powder. The mesh size of the water-retaining agent powder is, for example, 100 meshes to 150 meshes, and the coating is, for example, a composite, and the coating includes, for example, at least propylene glycol, ethylene glycol diglycidyl ether, sorbitan glycidyl ether, and metal ions. Among them, in the coating, propylene glycol accounts for 37%-41%, ethylene glycol diglycidyl ether accounts for 9%-13%, sorbitan glycidyl ether accounts for 26%-30%, metal ions account for 19%-23%, and the metal ions include at least one of aluminum ions, etc., and the mass of the coating is 0.1%-3% of the mass of the water-retaining agent powder.

[0044] See also Figure 1 to Figure 2 As shown, in one embodiment of the present invention, in step S125, the method of forming a coating on the surface of the water retaining agent is, for example, at least one of spraying and immersion. In this embodiment, the method of forming the coating is, for example, spraying. Specifically, a coating liquid is prepared according to a preset ratio of propylene glycol, ethylene glycol diglycidyl ether, sorbitan glycidyl ether and metal ions, and then the coating liquid is sprayed on the surface of the water retaining agent. After spraying, the water retaining agent with the spraying liquid is placed in an oven at a preset temperature for surface cross-linking treatment. The preset temperature is, for example, 100°C-200°C.

[0045] See also Figure 1As shown, in one embodiment of the present invention, after adding the crosslinking agent and the initiator, in step S13, the initiator initiates a polymerization reaction of acrylic acid and non-ionic monomers to obtain a gel. Specifically, the polymerization reaction includes the following steps. First, the photoinitiator initiates a photo-initiated polymerization reaction of acrylic acid and non-ionic monomers under light. After the reaction system reaches the preset reaction temperature, the light is stopped, and then the high-temperature initiator initiates a high-temperature initiated polymerization reaction of acrylic acid and non-ionic monomers to obtain a gel. Among them, the light is, for example, UV ultraviolet light, the ultraviolet light is, for example, a band ultraviolet light, the ultraviolet light is, for example, a long-wave ultraviolet light, the wavelength of the ultraviolet light is, for example, 300nm-400nm, and the acrylic acid and non-ionic monomers can be photo-initiated for 40s-60s to undergo a polymerization reaction, the preset reaction temperature is, for example, 50℃-60℃, and the total time of the photo-initiated polymerization reaction and the high-temperature initiated polymerization reaction is, for example, 10min-20min. By continuously performing the polymerization reaction in step S13, the polymerization reaction time can be shortened, the preparation process can be simplified, and the preparation efficiency of the water-retaining agent can be improved. Moreover, the polymerization reaction is quickly initiated by the photoinitiator. After the polymerization reaction releases enough heat, the light is turned off and the polymerization reaction is continued to be initiated by the high-temperature initiator. The two-step polymerization reaction fully utilizes the heat released by the polymerization reaction without the need for additional heat, which can effectively reduce energy consumption and thus reduce the cost of the preparation process, making it suitable for large-scale promotion and application. At the same time, the photoinitiated polymerization reaction can be completed at room temperature and pressure without the need for pressure equipment, making the preparation process extremely low in risk.

[0046] See also Figure 1 As shown, in one embodiment of the present invention, after obtaining the gel, in step S14, the gel is dried, crushed and sieved to obtain a water retaining agent. Specifically, a cutting aid is added to the gel during the crushing process to facilitate the molding of the water retaining agent. The cutting aid, for example, includes at least anhydrous sodium sulfite, etc., and the mass of the cutting aid is, for example, 0.01%-2% of the total mass of acrylic acid and non-ionic monomers.

[0047] See also Figure 1 to Figure 2 The present invention also provides a water retaining agent obtained by the above-mentioned water retaining agent preparation method. The water retaining agent provided by the present invention can reduce the sensitivity of the water retaining agent to salt and improve the salt resistance and water absorption of the water retaining agent by introducing non-ionic monomers and salt-resistant functional additives during the preparation process.

[0048] The technical scheme of the present invention is described in detail below through several specific examples and comparative examples. Unless otherwise specified, the raw materials and reagents used in the following examples and comparative examples are all commercially available products, or can be prepared by conventional methods in the art, and the instruments used in the examples can all be commercially available.

[0049] Example 1

[0050] Dissolve 200g of acrylic acid in 424g of deionized water, then add 276g of 45wt% potassium hydroxide aqueous solution and neutralize in an ice water bath. Then add 100g of acrylamide monomer to obtain an intermediate solution, and control the temperature of the intermediate solution to 20°C. Add 0.09g of N,N-methylenebisacrylamide, 0.12g of sodium persulfate and 0.018g of α-aminoalkyl acetophenone to the intermediate solution to obtain a reaction solution. After deoxygenating the reaction solution for 3min, pour it into a UV reaction tank and turn on the ultraviolet lamp to initiate the polymerization reaction. When the reaction reaches 60°C, turn off the ultraviolet lamp and the high-temperature initiator continues to initiate the reaction. React for 12min to obtain a water retainer gel. The obtained water retainer gel is crushed by an extruder, and 6g of sodium sulfite solution is added during the crushing process. The colloid particles are dried and sieved to obtain a water retainer, and the water retainer is sieved into 150 mesh or more and 100 mesh-150 mesh according to the mesh number. Among them, sodium sulfite is a 20wt% solution.

[0051] Example 2

[0052] 0.7 g of propylene glycol, 0.2 g of ethylene glycol diglycidyl ether, 0.375 g of aluminum sulfate and 0.5 g of sorbitan glycidyl ether were mixed to obtain a surface crosslinking liquid, which was sprayed onto the surface of the 100-150 mesh water retaining agent in Example 1, and then the water retaining agent was placed in an oven at 150° C. for surface crosslinking treatment to obtain a hydrophilic functional filler. The mass of the 100-150 mesh water retaining agent was 100 g.

[0053] Place a beaker containing 50 mL of deionized water on a magnetic stirrer at a speed of 300 rpm, slowly add 0.5 g of hydroxyethyl cellulose into the deionized water, and then add 0.5 g of a hydrophilic functional filler and 0.015 g of sodium hypophosphite into the above solution respectively, stir evenly, and obtain a salt-resistant functional additive.

[0054] Dissolve 200g of acrylic acid in 424g of deionized water, then add 276g of 45wt% potassium hydroxide aqueous solution and neutralize in an ice water bath. Then add 100g of acrylamide monomer to obtain an intermediate solution, and control the temperature of the intermediate solution to 20°C. Add 0.09g of N,N-methylenebisacrylamide, 0.12g of sodium persulfate, 0.018g of α-aminoalkyl acetophenone and 25g of salt-resistant functional additive to the intermediate solution to obtain a reaction solution. After deoxygenating the reaction solution for 3min, pour it into a UV reaction tank and turn on the ultraviolet lamp to initiate the polymerization reaction. When the reaction reaches 60°C, turn off the ultraviolet lamp and the high-temperature initiator continues to initiate the reaction. React for 12min to obtain a water-retaining agent gel. The obtained water-retaining agent gel is crushed by an extruder, and 6g of sodium sulfite solution is added during the crushing process. The gel particles are dried and sieved to obtain a water-retaining agent. The sodium sulfite is a 20wt% solution.

[0055] Example 3

[0056] The difference between this embodiment and embodiment 2 is that the mass of acrylic acid is 175 g, 100 g of acrylamide monomer is added, and 25 g of hydroxyethyl methacrylate monomer is also added, and the rest is the same.

[0057] Example 4

[0058] The difference between this embodiment and embodiment 3 is that hydroxyethyl cellulose is not added during the preparation of the salt-tolerant functional additive, and the rest is the same.

[0059] Example 5

[0060] The difference between this embodiment and embodiment 3 is that no hydrophilic functional filler is added during the preparation of the salt-resistant functional additive, and the rest is the same.

[0061] Example 6

[0062] The difference between this embodiment and embodiment 3 is that sodium hypophosphite is not added during the preparation of the salt-tolerant functional additive, and the rest is the same.

[0063] Comparative Example 1

[0064] Dissolve 200g of acrylic acid in 424g of deionized water, then add 276g of 45wt% potassium hydroxide aqueous solution, neutralize in an ice-water bath to obtain an intermediate solution, and control the temperature of the intermediate solution to 20°C. Add 0.09g of N,N-methylenebisacrylamide and 0.018g of α-aminoalkylacetophenone to the intermediate solution to obtain a reaction solution. After deoxygenating the reaction solution for 3 minutes, pour it into a UV reaction tank and turn on the ultraviolet lamp to initiate the polymerization reaction. When the temperature no longer changes during the reaction, turn off the ultraviolet lamp to obtain a water-retaining agent gel. The obtained water-retaining agent gel is crushed by an extruder, and 6g of sodium sulfite solution is added during the crushing process. The gel particles are dried and sieved to obtain a water-retaining agent. The sodium sulfite is a 20wt% solution.

[0065] The water retaining agents prepared in Examples 1-6 and Comparative Example 1, as well as commercially available water retaining agents, were tested under the conditions specified in the industry standard NY / T886-2022 "Agricultural and Forestry Water Retaining Agents". The test results are shown in Table 1. The commercially available water retaining agent is, for example, the HD204 water retaining agent of Jinan Huadi Industry and Trade Co., Ltd.

[0066] Table 1. Test results of Examples 1-6, Comparative Example 1 and commercially available water-retaining agents

[0067]

[0068] As can be seen from Table 1, the water absorption multiples and salt water absorption multiples of the water retaining agents of Examples 2-6 are much higher than those of Example 1, the comparative example and the commercially available water retaining agents, indicating that the water retaining agents of Examples 2-6 have higher salt tolerance and water absorption. Therefore, the preparation method of the water retaining agent provided by the present invention can improve the salt tolerance and water absorption of the water retaining agent by introducing non-ionic monomers and salt-resistant functional additives into acrylic acid. Moreover, the preparation method provided by the present invention can reduce the energy consumption of the preparation process and reduce the cost of the preparation process by initiating polymerization reaction by light and initiating polymerization reaction at high temperature and utilizing the reaction heat of polymerization reaction to complete the polymerization reaction.

[0069] In summary, the present invention provides a water-retaining agent and a preparation method thereof. By introducing a nonionic monomer and a salt-resistant functional auxiliary agent into acrylic acid, the salt resistance and water absorption of the water-retaining agent can be improved. Moreover, the preparation method provided by the present invention completes the polymerization reaction by two steps of light initiation and high temperature initiation, fully utilizes the reaction heat of the polymerization reaction, can save energy consumption in the preparation process, reduce the cost of the preparation process, and is suitable for large-scale promotion and application. At the same time, the preparation method provided by the present invention has the advantages of simple process, high efficiency and safety.

[0070] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A method for preparing a water-retaining agent, characterized in that: At least the following steps are included: dissolving acrylic acid in a solvent, and adding an alkaline solution and at least one nonionic monomer to the acrylic acid solution to obtain an intermediate solution; adding a crosslinking agent and an initiator to the intermediate solution; The initiator initiates a polymerization reaction between the acrylic acid and the nonionic monomer to obtain a gel; as well as The gel is dried, crushed and sieved to obtain a water retaining agent.

2. The preparation method according to claim 1, characterized in that: The nonionic monomer includes at least one of methyl methacrylate, ethyl acrylate, butyl acrylate, isooctyl acrylate, acrylamide and hydroxyethyl methacrylate.

3. The preparation method according to claim 1, characterized in that: The initiator includes a photoinitiator and a high temperature initiator.

4. The preparation method according to claim 1, characterized in that: A salt-resistant functional auxiliary agent is also added to the intermediate solution.

5. The preparation method according to claim 4, characterized in that: The salt-resistant functional auxiliary agent includes at least one of inorganic phosphates, including sodium hypophosphite, calcium hypophosphite, ammonium hypophosphite, nickel hypophosphite, cobalt hypophosphite and iron hypophosphite. The mass of the inorganic phosphate is 0.001%-0.1% of the total mass of the acrylic acid and the non-ionic monomer.

6. The preparation method according to claim 4, characterized in that: The salt-resistant functional additive includes at least one of the hydrophilic polymer materials, and the hydrophilic polymer materials include 2,2,6,6-tetramethylpyridine-1-oxyl free radical oxidized cellulose, carboxymethyl cellulose, carboxymethyl starch, hydroxyethyl cellulose and carboxymethyl chitosan. The mass of the hydrophilic polymer material is 0.005%-5% of the total mass of the acrylic acid and the non-ionic monomer.

7. The preparation method according to claim 4, characterized in that: The salt-resistant functional auxiliary agent includes a hydrophilic functional filler, which includes at least water-absorbing resin particles. The mass of the hydrophilic functional filler is 0.01%-5% of the total mass of the acrylic acid and the non-ionic monomer.

8. The preparation method according to claim 7, characterized in that: The preparation of the water-absorbent resin particles comprises at least the following steps: adding an alkaline solution and at least one nonionic monomer to an acrylic acid solution to obtain an intermediate solution; adding a crosslinking agent and an initiator to the intermediate solution; The initiator initiates a polymerization reaction between the acrylic acid and the nonionic monomer to obtain a gel; Drying, crushing and sieving the gel to obtain water-retaining agent powder; and The water-absorbent resin particles are obtained by forming a coating layer on the surface of the water-retaining agent fine powder.

9. The preparation method according to claim 8, characterized in that: The coating at least comprises propylene glycol, ethylene glycol diglycidyl ether, sorbitan glycidyl ether and metal ions.

10. A water-retaining agent, characterized in that: The method is obtained by the preparation method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Preparation method of salt-tolerance controlled-release high-water-absorption resin with hydrophobic chain segments

    CN102633944A

  • Soil water-retaining agent and preparation method thereof

    CN109705874A

  • Super absorbent resin and preparation method thereof

    CN112442152A

  • Manufacture of high water absorptive polymer

    JP1999255837A

  • Production method for hydrophilic polymer

    US20070149701A1