Cationic thickening agent and preparation method thereof
By introducing cationic monomers and double-stranded monomers into polyacrylamide, a thickener molecular structure with hydrophilic and hydrophobic groups is formed, which solves the problem of insufficient salt resistance and shear resistance in high-temperature and high-salt environments. The effective application of thickening agents in complex oil reservoirs has been achieved.
Patent Information
- Application Number
- CN202411389570.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-08
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-10-08
AI Technical Summary
The existing polyacrylamide thickening agents show insufficient salt resistance, temperature resistance and shear resistance in high temperature and high salt environments, and it is difficult to adapt to the development needs of complex reservoirs.
Develop a cationic thickening agent to form a molecular structure with hydrophilic and hydrophobic groups by introducing cationic monomers and double-stranded monomers into acrylamide, combined with surfactants and catalysts, using specific preparation methods. Enhance the electrostatic repulsion and hydrogen bonding between molecules, thereby forming a spatial network structure and improving the salt and shear resistance of the thickener.
In high temperature and high salt environment, the thickener exhibits good tackification enhancement effect, significantly improves salt resistance and shear resistance, ensures the temperature resistance of the thickener, and is suitable for the development of complex oil reservoirs.
Smart Images

Figure CN118878735A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of preparation of fracturing fluid thickeners, in particular to a cationic thickener and a preparation method thereof. Background Art
[0002] With the continuous exploitation of oil and gas resources, complex reservoirs such as deep well high temperature, high mineralization and low permeability reservoirs have become the main areas of oil field development. Chemical flooding, as one of the main measures to improve the recovery rate in the process of oil and gas exploitation, has been widely used in the direction of tertiary oil recovery. Among them, polymer flooding has become a widely used tertiary oil recovery technology in my country due to its direct effect, simple construction method and low cost. It has been industrially applied in oil fields such as Daqing, Shengli and Dagang. As the core technology of polymer drive, the research and development of oil displacement agents is very important. Among them, polyacrylamide and xanthan gum oil displacement agents are the two most important types of polymer flooding oil displacement agents. Since polyacrylamide polymers generally have good viscoelasticity and can significantly improve the recovery rate of residual oil, the application of polyacrylamide polymers is more extensive than that of xanthan gum polymers.
[0003] For conventional polyacrylamide (PAM), the amide group in the molecule hydrolyzes rapidly in an acidic or alkaline environment; in a neutral environment, increasing the temperature can accelerate the hydrolysis rate of the amide group. Therefore, ordinary PAM has poor temperature and salt resistance. Therefore, the molecular structure of conventional PAM determines that it can only be used in medium-low temperature and low-salinity reservoirs. Limited by the molecular structure and viscosity-increasing mechanism, the currently commonly used partially hydrolyzed polyacrylamide (HPAM) is a linear polymer. In the molecular chain of the salt solution, it is affected by the electrostatic shielding and dehydration of metal cations, causing the molecular chain to curl, the molecular size to decrease, and the solution viscosity to drop rapidly. At present, there are higher requirements for the performance of polymer fracturing fluids such as salt resistance, temperature resistance, shear resistance, reservoir contamination, and formation adaptability.
[0004] As a commonly used thickener in the field of chemical flooding, polyacrylamide has attracted widespread attention for its good performance and low cost. Currently, most of the commonly used thickeners in chemical flooding are anionic polyacrylamide thickeners, which are unanimously recognized by the market for their good solubility, high stability and low cost. However, they cannot be used in high-temperature and high-salinity oil fields. Summary of the invention
[0005] In response to the current application bottleneck of high-salt oil fields, the present application provides a new type of cationic functional thickener, which can achieve good viscosity increasing effect in high-temperature and high-salt environment, and has excellent salt resistance, shear resistance and temperature resistance.
[0006] To this end, the first technical solution provided by the present invention is as follows: A cationic thickener, the structural formula of which is shown in Formula 1: ;
[0007] Formula 1 Where: x=1-98000, y=1-6000, z=1-2000; R 1 is one of (C1-C22) alkyl, (C1-C25) ethoxy, (C1-C25) hydroxyalkyl, (C1-C25) phenyl, and (C1-C25) sulfonic acid; R 2 It is one of (C1-C22) alkyl, (C1-C25) ethoxy, (C1-C25) hydroxyalkyl, (C1-C25) phenyl and (C1-C25) sulfonic acid.
[0008] The second technical solution provided by the present invention is as follows: A method for preparing a cationic thickener comprises the following steps in sequence: (1) Weigh acrylamide, cationic monomer A, cationic double-chain monomer B, and surfactant according to a certain mass, and dissolve them in a certain mass of deionized water; (2) adding the catalyst to the aqueous solution in (1) to dissolve, adjusting the pH of the solution to neutral with sodium carbonate, pouring it into a reactor and passing nitrogen for a period of time; (3) Weigh a certain amount of initiator and add a certain amount of deionized water to dissolve it; (4) After the air in the reaction kettle in step (2) is completely removed, the initiator solution in step (3) is added dropwise, and at the same time, the system temperature is raised to react for several hours; (5) The white colloidal substance was cut into pieces, washed several times with anhydrous ethanol, and then dried in a vacuum oven.
[0009] The total mass of raw materials is the total mass of acrylamide, cationic monomer A, cationic double-chain monomer B, surfactant, catalyst, initiator and deionized water.
[0010] Furthermore, in the above-mentioned method for preparing a cationic thickener, the mass of acrylamide accounts for 12.0-22.0% of the total mass of the raw materials; Furthermore, in the preparation method of the above-mentioned cationic thickener, the cationic monomer A is at least one of acryloyloxyethyl trimethyl ammonium chloride, dimethyl diallyl ammonium chloride, diallylamine chloride, diallyl-N-carbonyl butoxymethyl ammonium chloride, N,N-dimethyl-N-benzyl-acryloyloxy ammonium chloride, methacryloyloxyethyl trimethyl ammonium chloride, diallyl ethyl benzyl ammonium chloride, methacrylamide propyl trimethyl ammonium chloride, diallylamine, and acrylamide propyl trimethyl ammonium chloride, and the mass of the cationic monomer A accounts for 3.0-15.0% of the total mass of the raw materials; Furthermore, in the preparation method of the above-mentioned cationic thickener, the cationic double-chain monomer B is homemade in the laboratory, belongs to the diallyl quaternary ammonium salt derivative, and has the appearance of a light yellow oily liquid, and its mass accounts for 0.05-3.0% of the total mass of the raw materials; The specific preparation method is as follows: the preparation method of cationic double-chain monomer B comprises the following steps: weighing 1.0 mol of diallylamine, 1.0 mol of potassium carbonate and ethanol, mixing them evenly, stirring for 10-30 minutes, controlling the temperature to be 60-80°C, and then dropping 2.0-2.5 mol of bromoalkane into the solution. After the addition is completed, react for 6-10 hours, adjust the temperature to 40-60°C, react for 18-30 hours, cool to room temperature, filter, and rotary evaporate to obtain a light yellow associated active substance, which is then set aside for later use.
[0011] Furthermore, in the preparation method of the above-mentioned cationic thickener, the surfactant is at least one of dodecylaminopropionic acid, octadecylamidopropylamine oxide, dodecyldimethylsulfopropyl betaine, hexadecyltrimethylammonium chloride, dodecylethoxysulfobetaine, tetradecylamidopropylhydroxypropylsulfobetaine, octadecyldihydroxyethylamine oxide, sodium lauryl sulfate, dodecyldimethylhydroxypropylsulfobetaine, hexadecyldimethylhydroxypropylphosphate betaine, dodecanol polyoxyethylene ether 2-acrylamido-2-dimethylpropanesulfonic acid, decyldimethylhydroxypropylsulfobetaine, and sodium dodecylsulfonate, and the mass thereof accounts for 0.5-3.0% of the total mass of the raw materials; Furthermore, in the preparation method of the above-mentioned cationic thickener, the catalyst is at least one of 1,4-butanediol, 1,6-hexanediol, bis-hydroxyethyl (or hydroxypropyl) bisphenol A, ethylene glycol, glycerol, propylene glycol, 1,4-bis(hydroxyethyl) hydroquinone, hydrogenated bisphenol A, 1,4-cyclohexanediol, 1,4-bis(hydroxyethyl) piperazine, pentaerythritol, trimethylolpropane, tetramethylethylenediamine, diethylamine, diethylene glycol, dimethylaminopropionitrile, triethylene glycol, neopentyl glycol, hydrogenated bisphenol A, 1,4-cyclohexanediol, sorbitol, diethylamino anhydrous ethanol, N,N'-methylenebisacrylamide, and sodium formate, and the mass of the catalyst accounts for 0.005-0.1% of the total mass of the raw materials; Furthermore, the preparation method of the above-mentioned cationic thickener is characterized in that the initiator is at least one of sodium bisulfite, sodium thiosulfate, dicyclohexyl peroxydicarbonate, ammonium persulfate, azobisisobutyronitrile, azobisisobutylimidazoline hydrochloride, azobisisobutylamidine hydrochloride, potassium persulfate, azobiscyanovaleric acid, azobisisopropylimidazoline, and sodium persulfate, and its mass accounts for 0.001-0.1% of the total mass of the raw materials; Furthermore, the method for preparing the above-mentioned cationic thickener is characterized in that the reaction temperature in step (4) is 30-80°C and the reaction time is 2-20h; Furthermore, the preparation method of the above-mentioned cationic thickener is characterized in that the mixture is washed with anhydrous ethanol, the vacuum drying temperature is 50-100° C., and the drying time is 6-48 hours.
[0012] Compared with the prior art, the technical solution provided by the present invention has the following technical advantages: The cationic functional thickener prepared by the present invention can achieve a good thickening effect in a high temperature and high salt environment, and has excellent salt resistance, shear resistance and temperature resistance. The thickener structure contains both hydrophilic groups and hydrophobic groups. The hydrophilic groups in the molecules, such as amide groups, form hydrogen bond association after contact with water, and the hydrophobic groups, due to the hydrophobic effect, aggregate and entangle with each other in the thickener molecules. They work together to form a macromolecular network with a spatial mesh structure in water. In addition, due to the presence of dicationic groups, there is an electrostatic repulsion between them, and the thickener molecular chain is more stretched, which is conducive to the association between the thickener molecules and improves the salt resistance of the thickener molecules. The hydrogen bond, van der Waals force, electrostatic repulsion, and hydrophobic association work together to increase the fluid mechanics volume of the thickener, thereby improving the apparent viscosity and shear resistance of the thickener aqueous solution. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 This is an infrared spectrum of the structure of thickener molecule Q3 in Example 3 of the present invention; Figure 2 is the NaCl resistance of the thickener molecule Q5 in Example 4 of the present invention; Figure 3 The MgCl resistance of the thickener molecule Q5 in Example 4 of the present invention is 2 sex; Figure 4 The CaCl resistance of thickener molecule Q5 in Example 4 of the present invention is 2 sex; Figure 5 This is the shear resistance of the thickener molecule Q4 in Example 5 of the present invention. DETAILED DESCRIPTION
[0014] The claims of the present invention are further described in detail below in conjunction with specific embodiments, but do not constitute any limitation to the present invention. Any limited modifications made by anyone within the scope of the claims of the present invention are still within the scope of the claims of the present invention.
[0015] Example 1
[0016] The present embodiment provides a method for preparing a cationic thickener, which specifically comprises the following steps: (1) Weigh 12.06 g of acrylamide, 15.53 g of methacryloyloxyethyl trimethyl ammonium chloride, 0.05 g of cationic double-chain monomer B, and 1.42 g of sodium dodecyl sulfate, and dissolve them in 55 mL of deionized water; (2) Add 0.005 g of tetramethylethylenediamine to the aqueous solution in (1) to dissolve, adjust the pH of the solution to neutral with sodium carbonate, pour it into a reactor and pass nitrogen for 40 minutes; (3) Weigh 0.05 g of azobisisobutyronitrile and add it to 15 mL of deionized water to dissolve it to obtain an initiator solution; (4) The air in the reactor in step (2) was removed and the initiator solution in step (3) was added dropwise. At the same time, the system temperature was raised to 60 ° C and the reaction was carried out for 10 h; (5) The white colloidal substance was cut into pieces, washed three times with anhydrous ethanol, and then dried in a vacuum oven at 75 °C for 24 h.
[0017] Wherein: the preparation method of cationic double-chain monomer B comprises the following steps: weighing 1.0 mol of diallylamine and 1.0 mol of potassium carbonate, adding 50 ml of ethanol and mixing evenly, stirring for 10 min, controlling the temperature to 70°C, and then dropping 2.2 mol of tetradecane bromide into the solution. After the addition is completed, react for 8 h, adjust the temperature to 50°C, react for 24 h, cool to room temperature, filter, and rotary evaporate to obtain a light yellow associated active substance, which is set aside for later use.
[0018] The thickener prepared in this example is recorded as Q1, and its molecular weight can reach about 4.436 million. The test method refers to the national standard "GB / T 12005.1-1989 Polyacrylamide intrinsic viscosity determination method" and "GB / T 12005.10-1992 Polyacrylamide molecular weight determination viscosity method".
[0019] Example 2
[0020] The present embodiment provides a method for preparing a cationic thickener, which specifically comprises the following steps: (1) Weigh 22.07 g of acrylamide, 2.98 g of methacryloyloxyethyl trimethyl ammonium chloride, 1.60 g of cationic double-chain monomer B, and 0.49 g of sodium dodecyl sulfate, and dissolve them in 55 mL of deionized water; (2) Add 0.049 g of N,N'-methylenebisacrylamide to the aqueous solution in (1) to dissolve, adjust the pH of the solution to neutral with sodium carbonate, pour it into the reactor and pass nitrogen for 40 minutes; (3) Weigh 0.001 g of ammonium persulfate and add it to 18 mL of deionized water to dissolve it to obtain an initiator solution; (4) The air in the reactor in step (2) was removed and the initiator solution in step (3) was added dropwise, and at the same time the system temperature was raised to 80 ° C for 2h; (5) The white colloidal substance was cut into pieces, washed three times with anhydrous ethanol, and then dried in a vacuum oven at 100 °C for 6 h.
[0021] Wherein: the preparation method of cationic double-chain monomer B comprises the following steps: weighing 1.0 mol of diallylamine and 1.0 mol of potassium carbonate, adding 50 ml of ethanol and mixing evenly, stirring for 15 min, controlling the temperature at 60°C, and then dropping 2.0 mol of dodecane bromide into the solution. After the addition is completed, react for 10 h, adjust the temperature to 40°C, react for 30 h, cool to room temperature, filter, and rotary evaporate to obtain a light yellow associated active substance, which is set aside for later use.
[0022] The thickener prepared in this example is recorded as Q2, and its molecular weight can reach about 3.264 million. The test method refers to the national standard "GB / T 12005.1-1989 Polyacrylamide intrinsic viscosity determination method" and "GB / T 12005.10-1992 Polyacrylamide molecular weight determination viscosity method".
[0023] Example 3
[0024] The present embodiment provides a method for preparing a cationic thickener, which specifically comprises the following steps: (1) Weigh 19.32 g of acrylamide, 2.38 g of methacryloyloxyethyl trimethyl ammonium chloride, 3.00 g of cationic double-chain monomer B, and 3.02 g of sodium dodecyl sulfate, and dissolve them in 60 mL of deionized water; (2) Add 0.10 g of tetramethylethylenediamine to the aqueous solution in (1) to dissolve, adjust the pH of the solution to neutral with sodium carbonate, pour it into a reactor and pass nitrogen for 40 minutes; (3) Weigh 0.10 g of potassium persulfate and sodium thiosulfate and add them to 12 mL of deionized water to dissolve them to obtain an initiator solution; (4) After the air in the reactor in step (2) is completely removed, the initiator solution in step (3) is added dropwise, and at the same time, the system temperature is raised to 30°C and the reaction is carried out for 20 hours; (5) The white colloidal substance was cut into pieces, washed three times with anhydrous ethanol, and then dried in a 50°C vacuum oven for 48 h.
[0025] Wherein: the preparation method of cationic double-chain monomer B comprises the following steps: weighing 1.0 mol of diallylamine and 1.0 mol of potassium carbonate, adding 50 ml of ethanol and mixing evenly, stirring for 30 min, controlling the temperature to 80°C, and then dropping 2.5 mol of hexadecane bromide into the solution, reacting for 6 h after the addition is completed, adjusting the temperature to 60°C, reacting for 18 h, cooling to room temperature, filtering, and rotary evaporating to obtain a light yellow associated active substance, which is set aside for later use.
[0026] The thickener prepared in this example is denoted as Q3, and its molecular weight can reach about 2.868 million. The test method refers to the national standard "GB / T 12005.1-1989 Polyacrylamide intrinsic viscosity determination method" and "GB / T 12005.10-1992 Polyacrylamide molecular weight determination viscosity method". The infrared spectrum of the thickener molecule is shown in Figure 1 .
[0027] Example 4
[0028] The present embodiment provides a method for preparing a cationic thickener, which specifically comprises the following steps: (1) Weigh 16.46 g of acrylamide, 7.25 g of methacryloyloxyethyl trimethyl ammonium chloride, 2.02 g of cationic double-chain monomer B, and 2.39 g of sodium dodecyl sulfate, and dissolve them in 55 mL of deionized water; (2) Add 0.072 g of tetramethylethylenediamine to the aqueous solution in (1) to dissolve, adjust the pH of the solution to neutral with sodium carbonate, pour it into a reactor and pass nitrogen for 40 minutes; (3) Weigh 0.054 g of azobisisobutylamidine hydrochloride and add it to 14 mL of deionized water to dissolve it to obtain an initiator solution; (4) After the air in the reactor in step (2) is completely removed, the initiator solution in step (3) is added dropwise, and at the same time, the system temperature is raised to 50°C and the reaction is carried out for 16 hours; (5) The white colloidal substance was cut into pieces, washed three times with anhydrous ethanol, and then dried in a vacuum oven at 80 °C for 18 h.
[0029] The preparation method of the cationic double-chain monomer B in this embodiment is the same as the preparation method of the cationic double-chain monomer B described in Example 2.
[0030] The thickener prepared in this example is recorded as Q4, and its molecular weight can reach about 5.543 million. The test method refers to the national standard "GB / T 12005.1-1989 Polyacrylamide intrinsic viscosity determination method" and "GB / T 12005.10-1992 Polyacrylamide molecular weight determination viscosity method".
[0031] Example 5
[0032] The present embodiment provides a method for preparing a cationic thickener, which specifically comprises the following steps: (1) Weigh 15.09 g of acrylamide, 10.47 g of methacryloyloxyethyl trimethyl ammonium chloride, 1.04 g of cationic double-chain monomer B, and 1.54 g of sodium dodecyl sulfate, and dissolve them in 57 mL of deionized water; (2) Add 0.04 g of diethylamine to the aqueous solution in (1) to dissolve, adjust the pH of the solution to neutral with sodium carbonate, pour it into a reactor and pass nitrogen for 40 minutes; (3) Weigh 0.05 g of potassium persulfate and add it to 14 mL of deionized water to dissolve it to obtain an initiator solution; (4) After the air in the reactor in step (2) is completely removed, the initiator solution in step (3) is added dropwise, and at the same time, the system temperature is raised to 65°C and the reaction is carried out for 8 hours; (5) The white colloidal substance was cut into pieces, washed three times with anhydrous ethanol, and then dried in a vacuum oven at 60 °C for 32 h.
[0033] The preparation method of the cationic double-chain monomer B in this embodiment is the same as the preparation method of the cationic double-chain monomer B described in Example 2.
[0034] The thickener prepared in this example is recorded as Q5, and its molecular weight can reach about 6.011 million. The test method refers to the national standard "GB / T 12005.1-1989 Polyacrylamide intrinsic viscosity determination method" and "GB / T 12005.10-1992 Polyacrylamide molecular weight determination viscosity method".
[0035] Comparative Example 1 The preparation process of this embodiment is exactly the same as that of the above-mentioned embodiment 1, except that the cationic double-chain monomer B is not added.
[0036] (1) Weigh 13.82 g of acrylamide, 13.46 g of methacryloyloxyethyl trimethyl ammonium chloride, 0.00 g of cationic double-chain monomer B, and 0.96 g of sodium dodecyl sulfate, and dissolve them in 56 mL of deionized water; (2) Add 0.019 g of tetramethylethylenediamine to the aqueous solution in (1) to dissolve, adjust the pH of the solution to neutral with sodium carbonate, pour it into a reactor and pass nitrogen for 40 minutes; (3) Weigh 0.027 g of potassium persulfate and dissolve it in 16 mL of deionized water; (4) After the air in the reactor in step (2) is completely removed, the initiator solution in step (3) is added dropwise, and at the same time, the system temperature is raised to 75°C and the reaction is carried out for 5 hours; (5) The white colloidal substance was cut into pieces, washed three times with anhydrous ethanol, and then dried in a vacuum oven at 80 °C for 18 h.
[0037] The thickener prepared in this example is recorded as P1, and its molecular weight can reach about 4.624 million. The test method refers to the national standard "GB / T 12005.1-1989 Polyacrylamide intrinsic viscosity determination method" and "GB / T 12005.10-1992 Polyacrylamide molecular weight determination viscosity method".
[0038] In order to demonstrate the advantages of the technical solution provided by the present application, the following is a cationic thickener detection experiment provided by the present application: 1. Infrared spectrum Infrared spectrum test method: Take a small amount of the thickener prepared in Example 3 and mix it evenly with the dried KBr, grind the thickener and KBr solid into powder with a mortar, adopt the tableting method, and use an infrared spectrometer to perform infrared spectrum test on the thickener, and the test wavelength range is 500~4000nm.
[0039] Test results reference Figure 1 ,from Figure 1 The infrared spectrum shows that 2923 cm -1 and 2853 cm -1 The peak at is attributed to the long-chain alkane -CH 2 - stretching vibration, 3181 cm -1 、3401 cm -1 and 1680 cm -1 The peaks are attributed to NH and C=O in the amide group, 1045 cm -1 The peak at is attributed to N + (CH 3 ) 3 The characteristic absorption peak of -1 The peak at 1453 cm is attributed to the stretching vibration absorption peak of CO. -1 The peaks were assigned to -CH 2 -N + The bending vibration of -CH2- in the mixture indicated that the thickener was successfully synthesized.
[0040] 2. Salt tolerance Test method: 50 mL of Example Q5 thickener solution was prepared with distilled water, with a mass concentration of 0.6 wt% for standby use. The test instrument was a rotational rheometer (MCR 702e), the test temperature was 25 °C, the rotor model was CP40-1, and the constant shear rate was 170 s -1 Under the conditions of , the apparent viscosity of the thickener solution of Example Q5 was tested.
[0041] Table 1
[0042] Poor salt resistance of thickeners is a pain point in the application of thickeners in oil fields. By introducing hydrophobic monomers to form a spatial network structure of the thickener, the hydrodynamic volume of the thickener in water can be increased, the viscosity of the thickener solution can be increased, and thus its salt resistance can be improved. As can be seen from Table 1, with the increase of salt concentration, the apparent viscosity of Q5 and P1 decreases, but the apparent viscosity of Q5 is much greater than that of P1, indicating that the salt resistance of Q5 is better than that of P1. The thickener solutions of Q5 and P1 in MgCl 2 The apparent viscosity of the solution is higher than that of CaCl 2 In solution. Figure 2-Figure 4 It can be seen that with the increase of salt concentration, the thickener molecular chain curls, the solubility decreases, and the viscosity decreases. The salt tolerance of Q5 is better than that of P1. When the concentration of NaCl reaches 20000mg / L, the apparent viscosity of Q5 can still reach 61mPa·s, while the apparent viscosity of P1 is only 33mPa·s; MgCl 2 When the concentration of CaCl reaches 2000 mg / L, the apparent viscosity of Q5 can still reach 62 mPa·s, while the apparent viscosity of P1 is only 31 mPa·s; 2 When the concentration reaches 2000 mg / L, the apparent viscosity of Q5 can still reach 60 mPa·s, while the apparent viscosity of P1 is only 28 mPa·s.
[0043] 3. Shear resistance Shear resistance test method: A rotational rheometer (MCR 702e) was used at a constant temperature of 25°C. The thickener molecule solution of Example Q4 was 0.6 wt %. The effect of shear rate on the shear stress of the thickener solution at different shear rates was tested.
[0044] Test results see Figure 5 ,from Figure 5 It can be seen that under the action of external shear force, the thixotropic loop of the thickener solution is very small, the rate at which the thickener solution structure is destroyed is basically equal to the rate at which the structure recovers, the thickener solution structure has instantaneous recovery performance, and the hysteresis of recovery can be ignored. In addition, with the increase of shear rate, the shear stress of the thickener solution gradually increases, indicating that the energy required to destroy the thickener solution gradually increases, and the spatial interpenetrating network structure formed by the thickener solution Q4 is the most dense, and the network structure strength is the greatest.
Claims
1. A cationic thickener, characterized in that: The structural formula is shown in Formula 1: ; Formula 1 Where: x=1-98000, y=1-6000, z=1-2000; R1 is one of (C1-C22) alkyl, (C1-C25) ethoxy, (C1-C25) hydroxyalkyl, (C1-C25) phenyl, and (C1-C25) sulfonic acid; R2 is one of (C1-C22) alkyl, (C1-C25) ethoxy, (C1-C25) hydroxyalkyl, (C1-C25) phenyl and (C1-C25) sulfonic acid.
2. The method for preparing a cationic thickener according to claim 1, characterized in that: The steps are as follows: (1) Weigh acrylamide, cationic monomer A, cationic double-chain monomer B, and surfactant, and dissolve them in deionized water; (2) adding the catalyst to the aqueous solution in (1) to dissolve, adjusting the pH of the solution to neutral, and pouring it into a reactor and introducing nitrogen; (3) Weigh the initiator and add deionized water to dissolve it; (4) After the air in the reaction kettle in step (2) is completely removed, the initiator solution in step (3) is added dropwise, and at the same time, the system is heated to 30-80°C and reacted for 2-20 hours; (5) The white colloidal substance is cut into pieces, washed several times with anhydrous ethanol, and then dried in a vacuum oven; The mass ratio of acrylamide, cationic monomer A, cationic double-chain monomer B, surfactant, catalyst and initiator is: 12.0-22.0: 3.0-15.0: 0.05-3.0: 0.5-3.0: 0.005-0.1: 0.001-0.
1.
3. The method for preparing a cationic thickener according to claim 2, characterized in that: The cationic monomer A is at least one of acryloyloxyethyl trimethyl ammonium chloride, dimethyl diallyl ammonium chloride, diallylamine chloride, diallyl-N-carbonyl butoxymethyl ammonium chloride, N,N-dimethyl-N-benzyl-acryloyloxy ammonium chloride, methacryloyloxyethyl trimethyl ammonium chloride, diallyl ethyl benzyl ammonium chloride, methacrylamide propyl trimethyl ammonium chloride, diallylamine, and acrylamide propyl trimethyl ammonium chloride.
4. The method for preparing a cationic thickener according to claim 2, characterized in that: The cationic double-chain monomer B is a diallyl quaternary ammonium salt derivative.
5. The method for preparing a cationic thickener according to claim 4, characterized in that: The cationic double-chain monomer B is prepared by the following method: weigh 1.0 mol of diallylamine, 1.0 mol of potassium carbonate and ethanol, mix them evenly, stir for 10-30 minutes, control the temperature value to 60-80°C, then add 2.0-2.5 mol of bromoalkane to the solution, react for 6-10 hours after the addition is completed, adjust the temperature to 40-60°C, react for 18-30 hours, cool to room temperature, filter, and rotary evaporate to obtain a light yellow associated active substance, which is placed for later use.
6. The method for preparing a cationic thickener according to claim 2, characterized in that: The surfactant is at least one of dodecylaminopropionic acid, octadecylamidopropylamine oxide, dodecyldimethylsulfopropyl betaine, hexadecyltrimethylammonium chloride, dodecylethoxysulfobetaine, tetradecylamidopropylhydroxypropylsulfobetaine, octadecyldihydroxyethylamine oxide, sodium lauryl sulfate, dodecyldimethylhydroxypropylsulfobetaine, hexadecyldimethylhydroxypropylphosphate betaine, lauryl alcohol polyoxyethylene ether 2-acrylamido-2-dimethylpropanesulfonic acid, and decyldimethylhydroxypropylsulfobetaine.
7. The method for preparing a cationic thickener according to claim 2, characterized in that: The catalyst is at least one of 1,4-butanediol, 1,6-hexanediol, bis-hydroxyethyl (or hydroxypropyl) bisphenol A, ethylene glycol, glycerol, propylene glycol, 1,4-bis(hydroxyethyl) hydroquinone, hydrogenated bisphenol A, 1,4-cyclohexanediol, 1,4-bis(hydroxyethyl) piperazine, pentaerythritol, trimethylolpropane, tetramethylethylenediamine, diethylamine, diethylene glycol, dimethylaminopropionitrile, triethylene glycol, neopentyl glycol, hydrogenated bisphenol A, 1,4-cyclohexanediol, sorbitol, diethylamino anhydrous ethanol, N,N'-methylenebisacrylamide, and sodium formate.
8. The method for preparing a cationic thickener according to claim 2, characterized in that: The initiator is at least one of sodium bisulfite, sodium thiosulfate, dicyclohexyl peroxydicarbonate, ammonium persulfate, azobisisobutyronitrile, azobisisobutylimidazoline hydrochloride, azobisisobutylamidine hydrochloride, potassium persulfate, azobiscyanovaleric acid, azobisisopropylimidazoline, and sodium persulfate.
9. The method for preparing a cationic thickener according to claim 2, characterized in that: The vacuum drying temperature in step (5) is 50-100°C, and the drying time is 6-48h.
10. The method for preparing a cationic thickener according to claim 2, characterized in that: The pH value of the solution in step (2) is adjusted by using sodium carbonate.
Citation Information
Patent Citations
Water dispersion dewatering cationic polymer and preparing method
CN101270178A
Thickening agent for high-temperature deep well acidification and preparation method thereof
CN112745454A
Cationic copolymer composition, amphoteric copolymer composition, and cosmetic and aromatic agent containing the cationic copolymer composition and / or the amphoteric copolymer composition
JP2017226713A