Water-based hydroxypropyl dispersion with high toughness, high solid content and zero VOC (volatile organic compound) as well as preparation method and application of water-based hydroxypropyl dispersion
By using caprolactone to modify hydroxyethyl acrylate monomer and grade glycidyl methacrylate, the problems of stability and environmental pollution of high solid content aqueous hydroxyacrylic acid dispersions in the prior art are solved, and high solid content and low viscosity are achieved and stable aqueous dispersions enhance the low temperature flexibility and gloss of the paint film.
Patent Information
- Application Number
- CN202410888320.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-11-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
It is difficult to prepare high solid content and stable aqueous hydroxyacrylic acid dispersions in the prior art, and organic solvents are often required to increase the risk of the production process and environmental pollution, and the polymerization reaction is unstable and difficult to control.
Using caprolactone modified hydroxyethyl acrylate monomer and grade glycidyl methacrylate as reactive monomers, a high toughness and high solids aqueous hydroxypropyl dispersion is formed through specific mass ratios and process steps, reducing or without the need for Use solvents to control the viscosity increase during the polymerization process and ensure the stability of the dispersion.
Aqueous hydroxypropylene dispersion with high solid content, low viscosity and stability is achieved, reducing environmental pollution, improving storage and use safety, and enhancing the low temperature flexibility and gloss of the paint film.
Smart Images

Figure QLYQS_1 
Figure BDA0004926700120000021 
Figure BDA0004926700120000091
Abstract
Description
Technical Field
[0001] The invention belongs to the field of chemical industry, and specifically relates to a high-toughness, high-solid content, zero-VOC aqueous hydroxypropyl dispersion and a preparation method and application thereof. Background Art
[0002] As one of the most commonly used water-based resins, water-based acrylic resin has been widely used in industrial paints. Due to its high gloss, good weather resistance, and good gloss and color retention, water-based (hydroxy) acrylic resin is often used in combination with isocyanate curing agent to prepare two-component polyurethane coatings. The cured paint film has the characteristics of both acrylic and polyurethane, with excellent performance and outstanding resistance. As one of the main varieties of water-based acrylic resins, hydroxy acrylic dispersion (secondary dispersion, referred to as hydroxy acrylic dispersion) has received widespread attention in recent years due to its excellent surface decorative properties. Compared with hydroxy acrylic emulsion, hydroxy acrylic dispersion has the characteristics of high gloss, good fullness, and better appearance decorative properties. It has been widely used in water-based industries.
[0003] However, the preparation of hydroxylated acrylic dispersions often requires the addition of a large amount of organic solvents to reduce viscosity. However, the use of organic solvents not only increases material costs and recycling costs, but also increases the danger of the production process and the harm to humans, while also causing certain pollution to the environment.
[0004] In addition, due to the presence of polar groups such as hydroxyl and carboxyl groups, the viscosity of hydroxylated acrylic dispersions first decreases, then increases, and finally decreases when dispersed in water. Therefore, in order to obtain a hydroxylated acrylic dispersion with suitable viscosity, it is usually necessary to add enough water to allow the dispersion to pass through the viscosity peak and reach a smaller viscosity. It is precisely based on this that the solid content of dispersion products currently sold on the market is often not high.
[0005] Chinese patent CN117946345 mentions a highly flexible zero-VOC low-hydroxy acrylic dispersion and its preparation method and application, which uses polycaprolactone polyol as an active solvent to reduce the viscosity of the system, and then uses a curing agent to react with the polycaprolactone polyol active solvent to achieve the purpose of zero solvent and zero VOC. However, the hydroxy dispersion prepared by this method is unstable and easily separated from water or thickened later.
[0006] Chinese patent CN110577614 mentions that the preparation of a high-solid hydroxy acrylic dispersion is to use tert-butyl glycidyl carbonate and monoglycidyl ether as active diluents to reduce the viscosity of the system, and then use the system-type carboxyl monomer and the active diluent to react, and then add a small amount of water to pass the viscosity peak, thereby obtaining a high-solid hydroxy acrylic dispersion with low viscosity. However, this reaction requires high temperature and the addition of a catalyst to react well, and the addition of a catalyst or the change of temperature will have a great influence on the polymerization reaction, resulting in uncontrollable polymerization.
[0007] Therefore, it is of great significance to provide a hydroxylated acrylic dispersion with high solid content and zero VOC, which is stable and controllable during production and stable in storage. Summary of the invention
[0008] In order to solve the above technical problems, the present invention discloses a preparation method and application of a high-toughness, high-solid content, zero-VOC aqueous hydroxypropyl dispersion.
[0009] The present invention is achieved through the following technical solutions:
[0010] A high-toughness, high-solid content, zero-VOC aqueous hydroxypropylene dispersion comprises caprolactone-modified hydroxyethyl acrylate monomer, a neutralizer, an initiator, deionized water, a soft monomer, a hard monomer, a carboxyl monomer, a hydroxyl monomer, a chain transfer agent and glycidyl methacrylate; the mass ratio of the caprolactone-modified hydroxyethyl acrylate monomer, the neutralizer, the initiator, deionized water, the soft monomer, the hard monomer, the carboxyl monomer, the hydroxyl monomer, the chain transfer agent and glycidyl methacrylate is 20-30: 1-2: 0.5-0.8: 26.2-30: 4-5: 13-15: 5-8: 10-15: 0.5-2: 5-7.
[0011] As a further improvement, the structural formula of the caprolactone-modified hydroxyethyl acrylate monomer is as follows:
[0012]
[0013] Where R=H or CH 3 ; n = 1 or 2.
[0014] In a further improvement, the neutralizing agent is one or more of triethylamine, triethanolamine, NN-dimethylacetamide, and diethanolamine.
[0015] Further improvement, the initiator is one or more of azobisisobutyronitrile, di-tert-butyl dioxide, and benzoyl peroxide.
[0016] In a further improvement, the chain transfer agent is one or more of dodecyl mercaptan, aliphatic mercaptan, and α-methylstyrene dimer.
[0017] As a further improvement, the soft monomer is one or more of n-butyl acrylate, ethyl acrylate, isooctyl acrylate, isooctyl methacrylate, and dodecyl methacrylate; and the hard monomer is one or more of methyl acrylate, methyl methacrylate, styrene, ethyl methacrylate, propyl methacrylate, and vinyl acetate.
[0018] As a further improvement, the carboxyl monomer is one or more of acrylic acid, methacrylic acid, itaconic acid, maleic acid, cinnamic acid, and maleic anhydride, and the hydroxyl monomer is one or more of hydroxyethyl methacrylate, hydroxyethyl acrylate, hydroxypropyl methacrylate, and hydroxypropyl acrylate.
[0019] As a further improvement, the preparation method of the caprolactone-modified hydroxyethyl acrylate monomer is as follows:
[0020] Caprolactone-modified hydroxyethyl acrylate monomer can be prepared by reacting hydroxyethyl acrylate as an initiator with caprolactone monomer at 100-120°C for 4-6 hours, separating and purifying. The caprolactone repeating unit is 1-2, and the molar ratio of hydroxyethyl acrylate to caprolactone monomer is 1:1-2.
[0021] A method for preparing a high-toughness, high-solid content, zero-VOC aqueous hydroxypropyl dispersion comprises the following steps:
[0022] Step 1, preparing a core layer mixed solution: uniformly mixing caprolactone-modified hydroxyethyl acrylate monomer, soft monomer, hydroxyl monomer, hydrophilic monomer, initiator, and chain transfer agent in a mass ratio of 12-18:4-5:5-7.5:0.5-0.8:0.3-0.48:0.3-1.2 to obtain a core layer mixed solution;
[0023] Step 2, preparing a shell layer mixture: uniformly mix caprolactone-modified hydroxyethyl acrylate monomer, hard monomer, hydroxyl monomer, hydrophilic monomer, initiator, and chain transfer agent in a mass ratio of 8-12:13-15:5-7.5:4.5-7.2:0.2-0.32:0.2-0.8 to obtain a shell layer mixture; the mass ratio of the core layer mixture to the shell layer mixture is: 25.5-30.18:34.9-38.5;
[0024] Step 3, synthesizing the core structure: adding glycidyl methacrylate to a reaction kettle, heating to 90-150°C, and after the temperature in the kettle is stable, dripping the core layer mixture into the reaction kettle for 3-5 hours, and keeping the temperature for 30 minutes after the dripping; wherein the mass ratio of glycidyl methacrylate to the core layer mixture is 3-4.2:25.5-30.18;
[0025] Step 4, synthesizing the shell structure: continue to add glycidyl methacrylate to the reaction kettle, and then drop the shell layer mixture into the reaction kettle, the dropping time is 4 hours, and the temperature is kept for 30 minutes after the dropping is completed, wherein the mass ratio of glycidyl methacrylate to the shell layer mixture is 2-2.8:34.9-38.5;
[0026] Step 5: Neutralization to form salt: cool to 80°C, slowly add neutralizer, add over 15 minutes, stir for 30 minutes after addition; the mass ratio of neutralizer to shell mixture is 1-2:25.5-30.18;
[0027] Step 6, adding water to disperse: continue to cool to 50-80°C, gradually add deionized water, stir and disperse for 30 minutes after adding, and after dispersion, the high-toughness, high-solid content, zero-VOC aqueous hydroxypropylene dispersion is obtained; wherein the mass ratio of deionized water to the shell mixture is 26.2-30:25.5-30.18.
[0028] A use of a high-toughness, high-solid, zero-VOC aqueous hydroxypropylene dispersion. The high-toughness, high-solid, zero-VOC aqueous hydroxypropylene dispersion is as described above, and the high-toughness, high-solid, zero-VOC aqueous hydroxypropylene dispersion is used as an additive to improve the low-temperature flexibility of a paint film.
[0029] The present invention has the following beneficial effects:
[0030] (1) The present invention has the following advantages by adding caprolactone to modify the hydroxyethyl acrylate monomer: first, the monomer itself has a carbon-carbon double bond, and can stably polymerize with other monomers at a suitable temperature, and can smoothly enter the molecular chain of the polymer, ensuring that the monomer can increase the storage stability of the hydroxy acrylic acid dispersion; second, the viscosity growth during the reaction can be controlled, because as the monomer enters the polymer molecular chain, it can play a role in reducing the viscosity, similar to the role of a reactive diluent, which allows the reaction system to be diluted with a small amount of solvent or without adding solvent to ensure the smooth progress of the reaction. Third, due to the low viscosity of the system, a small amount of water can be added to make the dispersion pass the viscosity peak, thereby preparing a high solid content and low viscosity dispersion.
[0031] (2) The present invention adds a small amount of methacrylate glycidyl ester or acrylate glycidyl ester as a reactive solvent. Since the solvent also has a carbon-carbon double bond, it can stably enter the polymer molecular chain as the polymerization reaction proceeds. Unlike many other patents that add polyols or tert-butyl glycidyl ester as diluents or solvents, which cannot enter the polymer molecular chain, this can also ensure the storage stability of the hydroxylated acrylic dispersion. Finally, as the reactive solvent is consumed by polymerization, a low-solvent or even solvent-free acrylic dispersion can be prepared.
[0032] (3) The performance of hydroxypropyl dispersion can be improved by adding caprolactone-modified hydroxyethyl acrylate monomer. Because the monomer contains caprolactone chain segments, it is of great help in impact resistance, flexibility, especially low-temperature flexibility, gloss, and fullness of the paint film. DETAILED DESCRIPTION
[0033] The technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0034] Example 1
[0035] (1) Preparation of caprolactone-modified hydroxyethyl acrylate monomer
[0036] Caprolactone-modified hydroxyethyl acrylate monomer can be prepared by reacting hydroxyethyl acrylate as an initiator with caprolactone at 120° C. for 4 hours. The number of caprolactone repeating units is 2 (determined by GPC distribution).
[0037] (2) Preparation of water-based hydroxylated acrylic dispersion
[0038] ① Prepare the core layer mixture: mix 18g of caprolactone-modified hydroxyethyl acrylate monomer, 5g of n-butyl acrylate, 5g of hydroxyethyl methacrylate, 0.5g of acrylic acid, 0.3g of azobisisobutyronitrile and 0.3g of α-methylstyrene dimer for 30 minutes and set aside.
[0039] ②Prepare the shell mixture: Mix 12g of caprolactone-modified hydroxyethyl acrylate monomer, 13g of methyl methacrylate, 5g of hydroxyethyl methacrylate, 4.5g of acrylic acid, 0.2g of azobisisobutyronitrile and 0.2g of α-methylstyrene dimer for 30 minutes and set aside.
[0040] ③ Synthesis of core structure: Add 3.6g of methacrylate into the reactor, heat it to 140℃, and after the temperature in the reactor stabilizes, add the core layer mixture dropwise into the reactor for 4 hours, and keep warm for 30 minutes after the addition is complete.
[0041] ④Synthesize shell structure: Continue to add 2.4 g of glycidyl methacrylate into the reactor, and then drop the shell layer mixture into the reactor for 4 hours. After the addition, keep warm for 30 minutes.
[0042] ⑤ Neutralization to salt: Cool down to 80℃, slowly add 2g triethylamine, add over 15min, stir for 30min after addition
[0043] ⑥ Dispersion by adding water: Continue to cool to 50°C, gradually add 28g of deionized water, stir and disperse for 30 minutes after adding, and obtain a zero-solvent high-solid content hydroxy acrylic acid dispersion after dispersion. This is called S1 hydroxy acrylic acid dispersion.
[0044] Example 2
[0045] (1) Preparation of caprolactone-modified hydroxyethyl acrylate monomer
[0046] Caprolactone-modified hydroxyethyl acrylate monomer can be prepared by reacting hydroxyethyl acrylate as an initiator with caprolactone at 120° C. for 4 hours. The number of caprolactone repeating units is 2 (determined by GPC distribution).
[0047] (2) Preparation of water-based hydroxylated acrylic dispersion
[0048] ① Prepare the core layer mixture: mix 15g of caprolactone-modified hydroxyethyl acrylate monomer, 5g of n-butyl acrylate, 6g of hydroxyethyl methacrylate, 0.6g of acrylic acid, 0.3g of azobisisobutyronitrile and 0.9g of α-methylstyrene dimer for 30 minutes and set aside.
[0049] ②Preparation of shell mixture: Mix 10g of caprolactone-modified hydroxyethyl acrylate monomer, 13g of methyl methacrylate, 6g of hydroxyethyl methacrylate, 5.4g of acrylic acid, 0.2g of azobisisobutyronitrile and 0.6g of α-methylstyrene dimer for 30 minutes and set aside.
[0050] ③ Synthesis of core structure: Add 4.2g of methacrylate into the reactor, heat it to 140℃, and after the temperature in the reactor stabilizes, add the core layer mixture dropwise into the reactor for 4 hours, and keep warm for 30 minutes after the addition is complete.
[0051] ④Synthesize shell structure: Continue to add 2.8g of glycidyl methacrylate into the reactor, and then drop the shell layer mixture into the reactor for 4 hours. After the addition, keep warm for 30 minutes.
[0052] ⑤ Neutralization to salt: Cool down to 80℃, slowly add 2g triethylamine, add over 15min, stir for 30min after addition
[0053] ⑥ Dispersion by adding water: Continue to cool to 50°C, gradually add 28g of deionized water, stir and disperse for 30 minutes after adding, and obtain zero-solvent high-solid content hydroxy acrylic acid dispersion after dispersion. Recorded as S2 hydroxy acrylic acid dispersion.
[0054] Example 3
[0055] (1) Preparation of caprolactone-modified hydroxyethyl acrylate monomer
[0056] Caprolactone-modified hydroxyethyl acrylate monomer can be prepared by reacting hydroxyethyl acrylate as an initiator with caprolactone at 120° C. for 4 hours. The number of caprolactone repeating units is 2 (determined by GPC distribution).
[0057] (2) Preparation of water-based hydroxylated acrylic dispersion
[0058] ① Prepare the core layer mixture: mix 12g of caprolactone-modified hydroxyethyl acrylate monomer, 4g of n-butyl acrylate, 7.5g of hydroxyethyl methacrylate, 0.8g of acrylic acid, 0.3g of azobisisobutyronitrile and 0.9g of α-methylstyrene dimer for 30 minutes and set aside.
[0059] ②Prepare the shell mixture: Mix 8g of caprolactone-modified hydroxyethyl acrylate monomer, 15g of methyl methacrylate, 7.5g of hydroxyethyl methacrylate, 7.2g of acrylic acid, 0.2g of azobisisobutyronitrile and 0.6g of α-methylstyrene dimer for 30 minutes and set aside.
[0060] ③ Synthesis of core structure: Add 3g of methacrylate into the reactor, heat it to 140℃, and after the temperature in the reactor stabilizes, add the core layer mixture dropwise into the reactor for 4 hours, and keep it warm for 30 minutes after the addition is completed.
[0061] ④Synthesize shell structure: Continue to add 2g of glycidyl methacrylate into the reactor, and then drop the shell layer mixture into the reactor for 4 hours. After the addition, keep warm for 30 minutes.
[0062] ⑤ Neutralization to salt: Cool down to 80℃, slowly add 1g triethylamine, add over 15min, stir for 30min after addition
[0063] ⑥ Dispersion by adding water: Continue to cool to 50°C, gradually add 30g of deionized water, stir and disperse for 30min after adding, and obtain zero-solvent high-solid content hydroxy acrylic acid dispersion after dispersion. This is called S3 hydroxy acrylic acid dispersion.
[0064] Example 4
[0065] (1) Preparation of caprolactone-modified hydroxyethyl acrylate monomer
[0066] Caprolactone-modified hydroxyethyl acrylate monomer can be prepared by reacting hydroxyethyl acrylate as an initiator with caprolactone at 120° C. for 4 hours. The number of caprolactone repeating units is 2 (determined by GPC distribution).
[0067] (2) Preparation of water-based hydroxylated acrylic dispersion
[0068] ① Prepare the core layer mixture: mix 18g of caprolactone-modified hydroxyethyl acrylate monomer, 5g of n-butyl acrylate, 5g of hydroxyethyl methacrylate, 0.5g of acrylic acid, 0.48g of azobisisobutyronitrile and 1.2g of α-methylstyrene dimer for 30 minutes and set aside.
[0069] ②Prepare the shell mixture: Mix 12g of caprolactone-modified hydroxyethyl acrylate monomer, 13g of methyl methacrylate, 5g of hydroxyethyl methacrylate, 4.5g of acrylic acid, 0.32g of azobisisobutyronitrile and 0.8g of α-methylstyrene dimer for 30 minutes and set aside.
[0070] ③ Synthesis of core structure: Add 3.6g of methacrylate into the reactor, heat it to 140℃, and after the temperature in the reactor stabilizes, add the core layer mixture dropwise into the reactor for 4 hours, and keep warm for 30 minutes after the addition is complete.
[0071] ④Synthesize shell structure: Continue to add 2.4 g of glycidyl methacrylate into the reactor, and then drop the shell layer mixture into the reactor for 4 hours. After the addition, keep warm for 30 minutes.
[0072] ⑤ Neutralization to salt: Cool down to 80℃, slowly add 2g triethylamine, add over 15min, stir for 30min after addition
[0073] ⑥ Dispersion by adding water: Continue to cool to 50°C, gradually add 26.2g of deionized water, stir and disperse for 30 minutes after adding, and obtain zero-solvent high-solid content hydroxy acrylic acid dispersion after dispersion. Recorded as S4 hydroxy acrylic acid dispersion.
[0074] Comparative Example 1
[0075] (1) Preparation of caprolactone-modified hydroxyethyl acrylate monomer
[0076] Caprolactone-modified hydroxyethyl acrylate monomer can be prepared by reacting hydroxyethyl acrylate as an initiator with caprolactone at 120° C. for 4 hours. The number of caprolactone repeating units is 2 (determined by GPC distribution).
[0077] (2) Preparation of water-based hydroxylated acrylic dispersion
[0078] ① Prepare the core layer mixture: mix 18g of caprolactone-modified hydroxyethyl acrylate monomer, 5g of n-butyl acrylate, 5g of hydroxyethyl methacrylate, 0.5g of acrylic acid, 0.72g of azobisisobutyronitrile and 1.8g of α-methylstyrene dimer for 30 minutes and set aside.
[0079] ②Prepare the shell mixture: Mix 12g of caprolactone-modified hydroxyethyl acrylate monomer, 13g of methyl methacrylate, 5g of hydroxyethyl methacrylate, 4.5g of acrylic acid, 0.48g of azobisisobutyronitrile and 1.2g of α-methylstyrene dimer for 30 minutes and set aside.
[0080] ③ Synthesis of core structure: Add 3.6g of methacrylate into the reactor, heat it to 140℃, and after the temperature in the reactor stabilizes, add the core layer mixture dropwise into the reactor for 4 hours, and keep warm for 30 minutes after the addition is complete.
[0081] ④Synthesize shell structure: Continue to add 2.4 g of glycidyl methacrylate into the reactor, and then drop the shell layer mixture into the reactor for 4 hours. After the addition, keep warm for 30 minutes.
[0082] ⑤ Neutralization to salt: Cool down to 80℃, slowly add 2g triethylamine, add over 15min, stir for 30min after addition
[0083] ⑥ Dispersion by adding water: Continue to cool to 50°C, gradually add 24.8g of deionized water, stir and disperse for 30 minutes after adding, and obtain a zero-solvent high-solid content hydroxy acrylic acid dispersion after dispersion. This is recorded as D1 hydroxy acrylic acid dispersion.
[0084] Comparative Example 2
[0085] (1) Preparation of caprolactone-modified hydroxyethyl acrylate monomer
[0086] Caprolactone-modified hydroxyethyl acrylate monomer can be prepared by reacting hydroxyethyl acrylate as an initiator with caprolactone at 120° C. for 4 hours. The number of caprolactone repeating units is 2 (determined by GPC distribution).
[0087] (2) Preparation of water-based hydroxylated acrylic dispersion
[0088] ① Prepare the core layer mixture: mix 6g of caprolactone-modified hydroxyethyl acrylate monomer, 6g of n-butyl acrylate, 12g of hydroxyethyl methacrylate, 0.4g of acrylic acid, 0.6g of azobisisobutyronitrile and 1.2g of α-methylstyrene dimer for 30 minutes and set aside.
[0089] ②Preparation of shell mixture: Mix 4g of caprolactone-modified hydroxyethyl acrylate monomer, 8g of methyl methacrylate, 12g of hydroxyethyl methacrylate, 3.6g of acrylic acid, 0.4g of azobisisobutyronitrile and 0.8g of α-methylstyrene dimer for 30 minutes and set aside.
[0090] ③ Synthesis of core structure: Add 4.8g of methacrylate into the reactor, heat it to 140℃, and after the temperature in the reactor stabilizes, add the core layer mixture dropwise into the reactor for 4 hours, and keep warm for 30 minutes after the addition is complete.
[0091] ④Synthesize shell structure: Continue to add 3.2g of glycidyl methacrylate into the reactor, and then drop the shell layer mixture into the reactor for 4 hours. After the addition, keep warm for 30 minutes.
[0092] ⑤ Neutralization to salt: Cool down to 80℃, slowly add 2g triethylamine, add over 15min, stir for 30min after addition
[0093] ⑥ Dispersion by adding water: Continue to cool to 50°C, gradually add 35g of deionized water, stir and disperse for 30 minutes after adding, and obtain zero-solvent high-solid content hydroxy acrylic acid dispersion after dispersion. Recorded as D2 hydroxy acrylic acid dispersion.
[0094] Comparative Example 3
[0095] (1) Preparation of caprolactone-modified hydroxyethyl acrylate monomer
[0096] Caprolactone-modified hydroxyethyl acrylate monomer can be prepared by reacting hydroxyethyl acrylate as an initiator with caprolactone at 120° C. for 4 hours. The number of caprolactone repeating units is 2 (determined by GPC distribution).
[0097] (2) Preparation of water-based hydroxylated acrylic dispersion
[0098] ① Prepare the core layer mixture: mix 12g of caprolactone-modified hydroxyethyl acrylate monomer, 4g of n-butyl acrylate, 6g of hydroxyethyl methacrylate, 0.8g of acrylic acid, 0.3g of azobisisobutyronitrile and 0.9g of α-methylstyrene dimer for 30 minutes and set aside.
[0099] ②Prepare the shell mixture: Mix 8g of caprolactone-modified hydroxyethyl acrylate monomer, 11g of methyl methacrylate, 6g of hydroxyethyl methacrylate, 7.2g of acrylic acid, 0.2g of azobisisobutyronitrile and 0.6g of α-methylstyrene dimer for 30 minutes and set aside.
[0100] ③ Synthesis of core structure: Add 7.8g of methacrylate into the reactor, heat it to 140℃, and after the temperature in the reactor stabilizes, add the core layer mixture dropwise into the reactor for 4 hours, and keep warm for 30 minutes after the addition is completed.
[0101] ④Synthesize shell structure: Continue to add 5.2g of glycidyl methacrylate into the reactor, and then drop the shell layer mixture into the reactor for 4 hours. After the addition, keep warm for 30 minutes.
[0102] ⑤ Neutralization to salt: Cool down to 80℃, slowly add 1g triethylamine, add over 15min, stir for 30min after addition
[0103] ⑥ Dispersion by adding water: Continue to cool to 50°C, gradually add 29g of deionized water, stir and disperse for 30 minutes after adding, and obtain zero-solvent high-solid content hydroxy acrylic acid dispersion after dispersion. Recorded as D3 hydroxy acrylic acid dispersion.
[0104] Performance Testing
[0105] The aqueous acrylic dispersions in Examples 1-4 and Comparative Examples 1-3 were tested as follows:
[0106] (1) Solid content: Dry in an oven at 150°C for 20 minutes and record the weight change before and after drying
[0107] (2) Viscosity: measured at 25°C using a rotational viscometer.
[0108] (3) Stability after 30-day heat storage at 50°C: After baking in a 50°C oven for 30 days, observe whether there is water separation and thickening, and test its viscosity.
[0109] The test results are summarized in the following table:
[0110]
[0111] From Examples 1-3, it can be seen that the caprolactone-modified hydroxyethyl acrylate monomer can reduce the viscosity of the system. As the amount of the monomer added increases, the viscosity of the system will be lower. Moreover, due to the addition and reaction of the caprolactone-modified hydroxyethyl acrylate monomer and the glycidyl methacrylate monomer, both enter the polymer molecular chain, which can ensure the storage stability of the dispersion.
[0112] It can be seen from Examples 1, 4 and Comparative Example 1 that the initiator and chain transfer agent also have a certain influence on the viscosity of the system. As the amount of the two is added, the viscosity of the system will first decrease and then remain basically stable. Further increase in amount will lead to an increase in viscosity. Therefore, it is sufficient to keep the amount of chain transfer agent in this system at about 2%, and the amount of initiator at about 0.8%.
[0113] It can be seen from Comparative Example 2 and Examples 1-3 that although the dispersion in Comparative Example 2 has a high hydroxyl content, due to the small amount of caprolactone-modified hydroxyethyl acrylate monomer added, the viscosity of the system does not decrease significantly, and more water is needed for dilution later. Therefore, the dispersion has a high viscosity and a lower solid content than that of the examples.
[0114] From Example 3 and Comparative Example 3, it can be seen that the viscosity of Comparative Example 3 is significantly higher than that of Example 3. This is because when the amount of reactive solvent increases, the epoxy groups in the reactive solvent will react too much with the carboxyl monomer, resulting in excessive viscosity of the system. Moreover, the thickening will affect the storage stability of the dispersion, so the amount of reactive solvent added must be controlled, and 5%-10% is the most appropriate.
[0115] This application provides a water-based industrial varnish, and the formula of the water-based industrial varnish is as follows:
[0116]
[0117] The coatings described in Application Examples 1-4 and Application Comparative Examples 1-3 were tested according to the implementation standard "HG / T 5176-2017" for surface coatings in water-based anti-corrosion coatings for steel structures, as follows:
[0118] 1) Pencil hardness: Tested according to GB / T 6739-2006; measured with a pencil hardness tester.
[0119] 2) Room temperature flexibility: Referring to the national standard "GB-1731-2020 Determination of paint film flexibility", the paint films applied on the tinplate are placed in a room temperature environment (about 25°C) for 1 hour, and then compared and measured according to the national standard paint film flexibility. The results are expressed as the minimum shaft rod diameter (mm) where no reticulation, cracks or peeling are observed in at least two tests.
[0120] 3) Low temperature flexibility: Referring to the national standard "GB-1731-2020 Determination of paint film flexibility", the paint films applied on the tinplate are placed in a -15°C environment for 1 hour in turn, and then quickly compared and measured according to the national standard paint film flexibility. The results are expressed as the minimum shaft rod diameter (mm) where no reticulation, cracks or peeling are observed in at least two tests. 4) Early water resistance: After the paint film applied on the steel plate is cured in a standard environment for 24 hours, half of the sample is immersed in water for 5 hours. Then take it out and observe whether there is blistering, peeling, cracking or rust in the immersed area. Moreover, after the test plate is restored under standard conditions for 2 hours, no obvious discoloration is observed between the immersed area and the non-immersed area, which is considered to be normal. The test results are as follows:
[0121]
[0122] It can be seen from Examples 1-3 that as the amount of caprolactone-modified hydroxyethyl acrylate monomer added increases, the low-temperature flexibility of the paint film becomes better and better, but the hardness gradually decreases, and the early water resistance is basically normal in this application formulation system.
[0123] It can be seen from Comparative Example 2 that the room temperature flexibility of the hydroxyl dispersion is closely related to the amount of soft monomer added. The more soft monomer is added, the better the room temperature flexibility is. In this formulation system, the low temperature flexibility (-15°C) needs to be adjusted by caprolactone-modified hydroxyethyl acrylate monomer.
[0124] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all details in detail, nor do they limit the invention to only the specific implementation methods described.
Claims
1. A high-toughness, high-solid content, zero-VOC aqueous hydroxypropyl dispersion, characterized in that: The invention comprises caprolactone-modified hydroxyethyl acrylate monomer, neutralizer, initiator, deionized water, soft monomer, hard monomer, carboxyl monomer, hydroxyl monomer, chain transfer agent and glycidyl methacrylate; the mass ratio of the caprolactone-modified hydroxyethyl acrylate monomer, neutralizer, initiator, deionized water, soft monomer, hard monomer, carboxyl monomer, hydroxyl monomer, chain transfer agent and glycidyl methacrylate is 20-30: 1-2: 0.5-0.8: 26.2-30: 4-5: 13-15: 5-8: 10-15: 0.5-2: 5-7.
2. The high-toughness, high-solid, zero-VOC aqueous hydroxypropyl dispersion according to claim 1, characterized in that: The structural formula of the caprolactone-modified hydroxyethyl acrylate monomer is as follows: Wherein, R=H or CH3; n=1 or 2.
3. The high-toughness, high-solid, zero-VOC aqueous hydroxypropyl dispersion according to claim 1, characterized in that: The neutralizing agent is one or more of triethylamine, triethanolamine, NN dimethylacetamide and diethanolamine.
4. The high-toughness, high-solid, zero-VOC aqueous hydroxypropyl dispersion according to claim 1, characterized in that: The initiator is one or more of azobisisobutyronitrile, di-tert-butyl dioxide and benzoyl peroxide.
5. The high-toughness, high-solid, zero-VOC aqueous hydroxypropyl dispersion according to claim 1, characterized in that: The chain transfer agent is one or more of dodecyl mercaptan, aliphatic mercaptan, and α-methylstyrene dimer.
6. The high-toughness, high-solid, zero-VOC aqueous hydroxypropyl dispersion according to claim 1, characterized in that: The soft monomer is one or more of n-butyl acrylate, ethyl acrylate, isooctyl acrylate, isooctyl methacrylate, and dodecyl methacrylate; the hard monomer is one or more of methyl acrylate, methyl methacrylate, styrene, ethyl methacrylate, propyl methacrylate, and vinyl acetate.
7. The high-toughness, high-solid, zero-VOC aqueous hydroxypropyl dispersion according to claim 1, characterized in that: The carboxyl monomer is one or more of acrylic acid, methacrylic acid, itaconic acid, maleic acid, cinnamic acid, and maleic anhydride; the hydroxyl monomer is one or more of hydroxyethyl methacrylate, hydroxyethyl acrylate, hydroxypropyl methacrylate, and hydroxypropyl acrylate.
8. The high-toughness, high-solid, zero-VOC aqueous hydroxypropyl dispersion according to claim 1, characterized in that: The preparation method of the caprolactone-modified hydroxyethyl acrylate monomer is as follows: Caprolactone-modified hydroxyethyl acrylate monomer can be prepared by reacting hydroxyethyl acrylate as an initiator with caprolactone monomer at 100-120°C for 4-6 hours, separating and purifying. The caprolactone repeating unit is 1-2, and the molar ratio of hydroxyethyl acrylate to caprolactone monomer is 1:1-2.
9. A method for preparing a high-toughness, high-solid content, zero-VOC aqueous hydroxypropyl dispersion, characterized in that: The steps include: Step 1, preparing a core layer mixed solution: uniformly mixing caprolactone-modified hydroxyethyl acrylate monomer, soft monomer, hydroxyl monomer, hydrophilic monomer, initiator, and chain transfer agent in a mass ratio of 12-18:4-5:5-7.5:0.5-0.8:0.3-0.48:0.3-1.2 to obtain a core layer mixed solution; Step 2, preparing a shell layer mixture: uniformly mix caprolactone-modified hydroxyethyl acrylate monomer, hard monomer, hydroxyl monomer, hydrophilic monomer, initiator, and chain transfer agent in a mass ratio of 8-12:13-15:5-7.5:4.5-7.2:0.2-0.32:0.2-0.8 to obtain a shell layer mixture; the mass ratio of the core layer mixture to the shell layer mixture is: 25.5-30.18:34.9-38.5; Step 3, synthesizing the core structure: adding glycidyl methacrylate to a reaction kettle, heating to 90-150°C, and after the temperature in the kettle is stable, dripping the core layer mixture into the reaction kettle for 3-5 hours, and keeping the temperature for 30 minutes after the dripping; wherein the mass ratio of glycidyl methacrylate to the core layer mixture is 3-4.2:25.5-30.18; Step 4, synthesizing the shell structure: continue to add glycidyl methacrylate to the reaction kettle, and then drop the shell layer mixture into the reaction kettle, the dropping time is 4 hours, and the temperature is kept for 30 minutes after the dropping is completed, wherein the mass ratio of glycidyl methacrylate to the shell layer mixture is 2-2.8:34.9-38.5; Step 5: Neutralization to form salt: cool to 80°C, slowly add neutralizer, add over 15 minutes, stir for 30 minutes after addition; the mass ratio of neutralizer to shell mixture is 1-2:25.5-30.18; Step 6, adding water to disperse: continue to cool to 50-80°C, gradually add deionized water, stir and disperse for 30 minutes after adding, and after dispersion, the high-toughness, high-solid content, zero-VOC aqueous hydroxypropylene dispersion is obtained; wherein the mass ratio of deionized water to the shell mixture is 26.2-30:25.5-30.
18.
10. Use of a high-toughness, high-solid content, zero-VOC aqueous hydroxypropyl dispersion, characterized in that: The high-toughness, high-solid, zero-VOC aqueous hydroxypropylene dispersion is as described in any one of claims 1 to 8, and the high-toughness, high-solid, zero-VOC aqueous hydroxypropylene dispersion is used as an additive to improve the low-temperature flexibility of the paint film.
Citation Information
Patent Citations
Method for producing crosslinked polymer, crosslinked polymer, and coating composition containing the same
CN103897096A
Glycidyl methacrylate modified hydroxy acrylate dispersion and new synthesis technology thereof
CN108383939A
Acrylate emulsion with core-shell structure and preparation method thereof
CN115124657A
Water-based hydroxyl acrylic acid dispersion as well as preparation method and application thereof
CN117567677A
Aqueous dispersion and method for producing the same
JP2017155126A
Cited By
A polyester-modified waterborne hydroxy acrylic acid dispersion, its preparation method and application
CN123083035A