Modified maleimide resin composition containing POSS (Polyhedral Oligomeric Silsesquioxane) structure, prepreg and copper foil substrate

By introducing a bismaleimide compound with a POSS structure and a maleimide group, a modified maleimide resin composition was prepared, and the dielectric properties and peel strength of the existing bismaleimide resin were solved. The problem of insufficient results has achieved the effects of low dielectric constant, low dielectric loss and high glass transition temperature, and met the strict requirements of laminated plates for semiconductor packaging.

CN118878749AActive Publication Date: 2024-11-01广东伊帕思新材料科技有限公司
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411075309.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-01
Estimated Expiration
2044-08-07

AI Technical Summary

Technical Problem

The existing bismaleimide resins have insufficient dielectric properties and peel strength in printed circuit boards, and the glass transition temperature does not meet the requirements, making it difficult to meet the strict requirements of laminated plates for semiconductor packaging.

Method used

The bismaleimide compound with the POSS structure is introduced and the maleimide group is combined to prepare a modified maleimide resin composition containing the POSS structure, combining polyphenylene ether and hydrocarbon resin to form a low dielectric constant , compositions with low dielectric loss, extremely high glass transition temperature, low thermal expansion coefficient and low water absorption, and semi-cured sheets and copper foil substrates were prepared after stirring evenly.

Benefits of technology

It significantly improves the dielectric constant, dielectric loss, glass transition temperature, peel strength and thermal stability performance, meets the high requirements of laminated plates for semiconductor packaging, and provides better thermal expansion coefficient and low water absorption rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure QLYQS_2
    Figure QLYQS_2
  • Figure QLYQS_3
    Figure QLYQS_3
Patent Text Reader

Abstract

The invention discloses a modified maleimide resin composition containing a POSS (Polyhedral Oligomeric Silsesquioxane) structure, which comprises the following components in 100 parts by weight: 10 to 80 parts of bismaleimide compound containing the POSS structure, 10 to 60 parts of polyphenyl ether and 5 to 60 parts of 1, 2-bis (4-vinyl phenyl) ethane. The bismaleimide compound containing the POSS structure is introduced, the introduced POSS structure is matched with a maleimide group, the low dielectric constant and low dielectric loss of the composition are ensured, and meanwhile, the composition also has extremely high glass transition temperature, lower thermal expansion coefficient, very low water absorption rate and better thermal stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of resin compositions, in particular to a modified maleimide resin composition containing a POSS structure, a prepreg and a copper foil substrate. Background Art

[0002] In recent years, with the rapid development of mobile Internet technology, people's demand for mobile data has continued to increase, and the high integration and miniaturization of semiconductors used in electronic devices, communication devices, personal computers, etc. have been accelerating. Along with this, the various properties required of semiconductor package laminates (such as metal foil-clad laminates, etc.) used in printed circuit boards have become increasingly stringent.

[0003] Bismaleimide resin is a kind of high-performance thermosetting resin matrix with active double bonds, which has been widely used in transportation, aerospace, mechanical electronics and other fields. Moreover, bismaleimide resin has the characteristics of high heat resistance, oxidation resistance and difficulty in ablation. Therefore, most of the industries currently use bismaleimide as the raw material of the substrate. Although conventional bismaleimide has a higher glass transition temperature, the dielectric properties and peel strength are still lacking, and the glass transition temperature has not yet reached a higher requirement. Therefore, it is necessary to propose a new solution to improve the above problems. Summary of the invention

[0004] In view of this, the present invention aims at the deficiencies in the prior art, and its main purpose is to provide a modified maleimide resin composition, a semi-cured sheet and a copper foil substrate containing a POSS structure, which introduces a bismaleimide compound containing a POSS structure, and the introduced POSS structure cooperates with the maleimide group to ensure the low dielectric constant and low dielectric loss of the composition. At the same time, the composition also has an extremely high glass transition temperature, a relatively low thermal expansion coefficient, a very low water absorption rate and good thermal stability.

[0005] To achieve the above purpose, the present invention adopts the following technical solutions:

[0006] A modified maleimide resin composition containing a POSS structure comprises the following components based on 100 parts by weight: 10-80 parts of a bismaleimide compound containing a POSS structure, 10-60 parts of polyphenylene ether, and 5-60 parts of 1,2-bis(4-vinylphenyl)ethane.

[0007] As a preferred embodiment, the general structural formula of the bismaleimide compound containing POSS structure is as follows:

[0008]

[0009] Among them, R1 is

[0010] As a preferred embodiment, the polyphenylene ether is a polyphenylene ether containing carbon-carbon unsaturated groups, and the polyphenylene ether containing carbon-carbon unsaturated groups contains at least any one of vinyl, allyl, propenyl, acrylate or methacrylate groups at one end, both ends or side chains.

[0011] As a preferred embodiment, the structural formula of the 1,2-bis(4-vinylphenyl)ethane is

[0012]

[0013] As a preferred embodiment, the invention further comprises 1-30 parts of hydrocarbon resin.

[0014] As a preferred embodiment, the hydrocarbon resin is at least one of polybutadiene, modified polybutadiene, polypentadiene, modified polypentadiene, polyisoprene, modified polyisoprene, polystyrene, butadiene-styrene copolymer, styrene-butadiene-styrene copolymer, hydrogenated diene-butadiene-styrene copolymer, maleic anhydride diene-butadiene-styrene copolymer, styrene-isoprene-styrene copolymer, styrene-butadiene-divinylbenzene copolymer, maleic anhydride styrene-butadiene copolymer, cyclopentadiene, modified cyclopentadiene, dicyclopentadiene, modified dicyclopentadiene, styrene-pentadiene copolymer, styrene-polypentadiene copolymer, butadiene-cyclopentadiene copolymer, ethylene-cyclopentadiene copolymer, norbornene polymer, and modified norbornene polymer.

[0015] A semi-cured sheet is prepared from the modified maleimide resin composition containing POSS structure.

[0016] A copper foil substrate is prepared from the aforementioned prepreg.

[0017] Compared with the prior art, the present invention has obvious advantages and beneficial effects. Specifically, it can be seen from the above technical solution that:

[0018] The present invention introduces a bismaleimide compound containing a POSS structure, and the introduced POSS structure cooperates with a maleimide group to ensure a low dielectric constant and a low dielectric loss of the composition. At the same time, the composition also has an extremely high glass transition temperature, a relatively low thermal expansion coefficient, a very low water absorption rate and good thermal stability.

[0019] In order to more clearly illustrate the structural features and effects of the present invention, the present invention is described in detail below in conjunction with specific embodiments. DETAILED DESCRIPTION

[0020] The invention discloses a modified maleimide resin composition containing a POSS structure. The modified maleimide resin composition comprises the following components based on 100 parts by weight: 10-80 parts of a bismaleimide compound containing a POSS structure, 10-60 parts of polyphenylene ether, and 5-60 parts of 1,2-bis(4-vinylphenyl)ethane.

[0021] The general structural formula of the bismaleimide compound containing POSS structure is as follows:

[0022] Among them, R1 is

[0023]

[0024] The polyphenylene ether is a polyphenylene ether containing carbon-carbon unsaturated groups, and one end, two ends or a side chain of the polyphenylene ether containing carbon-carbon unsaturated groups contains at least any one of vinyl, allyl, propenyl, acrylate or methacrylate groups.

[0025] The structural formula of the 1,2-bis(4-vinylphenyl)ethane is

[0026]

[0027] And, further comprising 1-30 parts of a hydrocarbon resin, wherein the hydrocarbon resin is at least one of polybutadiene, modified polybutadiene, polypentadiene, modified polypentadiene, polyisoprene, modified polyisoprene, polystyrene, butadiene-styrene copolymer, styrene-butadiene-styrene copolymer, hydrogenated diene-butadiene-styrene copolymer, maleic anhydride diene-butadiene-styrene copolymer, styrene-isoprene-styrene copolymer, styrene-butadiene-divinylbenzene copolymer, maleic anhydride styrene-butadiene copolymer, cyclopentadiene, modified cyclopentadiene, dicyclopentadiene, modified dicyclopentadiene, styrene-pentadiene copolymer, styrene-polypentadiene copolymer, butadiene-cyclopentadiene copolymer, ethylene-cyclopentadiene copolymer, norbornene polymer, and modified norbornene polymer.

[0028] The invention also discloses a prepreg, which is prepared from the modified maleimide resin composition containing the POSS structure. The preparation process is as follows: firstly, the raw material components are mixed with fillers and catalysts according to the components, and the mixture is uniformly mixed by stirring, so as to obtain the modified maleimide resin composition containing the POSS structure; then, the modified bismaleimide resin composition is placed in an appropriate amount of butanone solvent, and the mixture is uniformly mixed by stirring to obtain a glue solution with a solid weight percentage of 65%; the glue solution is impregnated and coated on an E glass fiber cloth with a model of 7628, and the mixture is baked in an oven at 160° C. for 5 minutes, so as to obtain the prepreg.

[0029] The present invention also discloses a copper foil substrate, which is prepared from the above-mentioned prepreg; the manufacturing process is as follows: a metal copper foil with a thickness of 18 μm is placed on the upper and lower surfaces of the prepreg, and then placed in a vacuum hot press, and pressed for 4 hours at a pressure of 1.5 MPa and a temperature of 180-220° C. to obtain a laminate. This preparation method is used in the subsequent embodiments.

[0030] The raw materials used in the following examples and comparative examples are shown in Table 1:

[0031]

[0032] Table 1

[0033] The preparation method of BMI-P is as follows:

[0034] First, under an atmosphere of nitrogen, 1.903g (11.2mmol) silicon tetrachloride and 3.572g (35.3mmol) triethylamine are dissolved in 20ml THF, obtain a mixed THF solution of silicon tetrachloride and triethylamine, then the mixed THF solution of silicon tetrachloride and triethylamine obtained is added drop-wise to a 70ml THF solution containing 9.965g (10.7mmol) heptaphenyltrisilanol-POSS (Xi'an Qiyue Biology), stirred at room temperature overnight, the suspension is filtered, and the mixed solid of Ph7CI-POSS and triethylamine hydrochloride is obtained and dissolved in a mixed solvent of 20ml, the mixed solvent being composed of 5ml THF and 15ml chloroform, then hydrolyzed for 90min with 15ml water and 2ml hydrochloric acid;

[0035] Next, remove the water layer, extract twice with chloroform, combine the organic layers, extract with water, dilute hydrochloric acid, water and saturated sodium chloride solution in turn, dry with magnesium sulfate, filter, remove most of the solvent, precipitate in methanol, filter, and vacuum dry overnight at 40° C. to obtain 9.37 g of Ph7OH-POSS, the purity of which is 90%; then, dissolve 1.701 g (3.08 mmol) of di(N-trimethylsilyl)-2-phenylamine-4,4'-chloromethylsilane and 0.314 g (3.1 mmol) of triethylamine in water; The mixture was dissolved in 5 ml of ether to obtain a mixed solution of di(N-trimethylsilyl)-2-phenylamine-4,4'-chloromethylsilane and triethylamine, and then the mixed solution was added dropwise to 17 ml of a solution containing 2.92 g (3.00 mmol) of Ph7OH-POSS, the solvent of which consisted of 15 ml of ether and 2 ml of THF, and stirred overnight at room temperature. After filtering off triethylamine hydrochloride and removing most of the solvent, 50 ml of acidified methanol was added, stirred for 1 hour, filtered, and dried in vacuo at 60°C to obtain phenylmonosiloxymethyldiphenylamine;

[0036] Then, 14.78 g of maleic anhydride was dissolved in 80 ml of acetone, cooled to below 20° C., added to 80 ml of acetone solution containing 15 g of phenylmonosilyloxymethyldiphenylamine, and reacted at below 20° C., and then the amic acid I generated by the reaction was filtered out, washed with acetone, and dried at 60-70° C.;

[0037] Finally, 18 g of amic acid I, 16 g of acetic anhydride, 0.09 g of nickel acetate and 3.43 g of 2,4,6-tris(dimethylaminomethyl)phenol were mixed and heated to 65-73°C, stirred for 1 hour, the product was filtered out, and after the generated water was evaporated, the product was added to 30 ml of methanol, the precipitate was filtered out, and then the precipitate was washed with a 50% methanol aqueous solution, a 20% methanol aqueous solution and water, and then recrystallized from methanol, dried at 70-100°C, mp 155-157°C, to obtain the product BMI-P. The preparation process of BMI-P is as follows:

[0038]

[0039] The raw material ratios of Examples 1-6 and Comparative Examples 1-7 are shown in Table 2:

[0040] Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Comparative Example 6 Comparative Example 7 BMI-P 60 45 70 10 20 35 BMI-1000 70 BMI-7000 60 70 BMI-2000 60 70 BMI-4000 60 70 SA90000 20 35 10 70 60 45 20 20 20 35 35 10 10 Ricon100 15 15 15 15 15 15 15 15 15 15 15 15 15 BVPE 5 5 5 5 5 5 5 5 5 5 5 5 5 DCP 2 2 2 2 2 2 2 2 2 2 2 2 2 SC-2050-KD 255 255 255 255 255 255 255 255 255 255 255 255 255

[0041] Table 2

[0042] The above multiple embodiments and comparative examples were subjected to performance tests, and the test results are shown in Table 3:

[0043] Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Comparative Example 6 Comparative Example 7 Dielectric constant SFDR(10C) 3.3 3.32 3.26 3.55 3.43 3.39 3.64 3.5 3.42 3.42 3.43 3.52 3.48 Dielectric loss SPDR(10G) 0.002 0.0026 0.0018 0.0035 0.0033 0.003 0.0036 0.0039 0.0033 0.0035 0.0038 0.0035 0.0028 Glass transition temperature ℃ 278 262 295 237 238 246 237 253 242 253 245 258 246 Water absorption % 0.18 0.20 0.12 0.32 0.25 0.22 0.23 0.24 0.23 0.25 0.28 0.32 0.37 X / Y axis CTE ppc / ℃ 8 11 7 15 13 13 11 10 12 12 11 12 12 Peel strength N / mm 0.72 0.6 0.75 0.4 0.42 0.56 0.52 0.51 0.52 0.45 0.45 0.41 0.51

[0044] Table 3

[0045] Analyzing the above data, compared with Comparative Examples 1-3, Example 1 uses the same proportion of raw materials, but Example 1 uses a homemade bismaleimide compound BMI-P, while Comparative Examples 1-3 use common commercially available bismaleimide resins. The finished product prepared in Example 1 is significantly superior to the finished products prepared in Comparative Examples 1-3 in terms of dielectric constant, dielectric loss, glass transition temperature, peel strength, water absorption rate and thermal expansion coefficient, and the glass transition temperature can be increased by up to 41°C, and the dielectric loss is reduced by nearly half.

[0046] At the same time, compared with Comparative Examples 4 and 5, the finished product prepared in Example 2 is superior to the finished products prepared in Comparative Examples 4 and 5 in terms of dielectric constant, dielectric loss, glass transition temperature, peel strength, water absorption rate and thermal expansion coefficient. Compared with Example 1 and Example 2, the ratio of bismaleimide compound to polyphenylene ether in Example 2 is smaller, and the dielectric constant, peel strength and water absorption rate of the two are roughly the same, but the finished product prepared in Example 2 is slightly inferior to the finished product prepared in Example 1 in terms of glass transition temperature, dielectric loss and thermal expansion coefficient. The finished products are as follows, while the ratio of the bismaleimide compound to the polyphenylene ether in Comparative Examples 4 and 5 is smaller than that in Comparative Examples 1-3, but the finished products obtained have substantially the same performance as those in Comparative Examples 1-3. When the ratio of the bismaleimide compound to the polyphenylene ether is reduced, different results are obtained by selecting different bismaleimide compounds. It can be seen that the role of the BMI-P in the present invention in the reaction system is completely different from that of the commercially available bismaleimide in the reaction system.

[0047] In addition, the finished product prepared in Example 3 is the best in dielectric constant, dielectric loss, glass transition temperature, peel strength, water absorption and thermal expansion coefficient. Compared with Comparative Examples 6 and 7, Example 3 uses the same proportion of raw materials, but uses different bismaleimide compounds. The finished product prepared in Example 3 is significantly better than the finished products prepared in Comparative Examples 6 and 7 in dielectric constant, dielectric loss, glass transition temperature, peel strength, water absorption and thermal expansion coefficient, and the glass transition temperature can be increased by up to 49°C, and the dielectric loss is reduced by nearly half.

[0048] Also, from the perspective of Examples 1-6, the performance of the finished products obtained in Examples 1-6 is affected by the ratio of the bismaleimide compound to the polyphenylene ether, while in Comparative Examples 1-7, the performance of the finished products obtained in Comparative Examples 1-7 is roughly the same and is not affected by the ratio of the bismaleimide compound to the polyphenylene ether. It can be seen that the bismaleimide compound selected by the present invention, after the introduction of the POSS structure, the POSS structure and the maleimide group are used in combination, which produces a very positive effect, and the performance of the final finished product is further optimized.

[0049] The above description is only a preferred embodiment of the present invention and does not limit the technical scope of the present invention. Therefore, any slight modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention are still within the scope of the technical solution of the present invention.

Claims

1. A modified maleimide resin composition containing a POSS structure, characterized in that: The invention comprises the following components based on 100 parts by weight: 10-80 parts of a modified bismaleimide compound containing a POSS structure, 10-60 parts of polyphenylene ether, and 5-60 parts of 1,2-bis(4-vinylphenyl)ethane.

2. The modified maleimide resin composition containing POSS structure according to claim 1, characterized in that: The general structural formula of the bismaleimide compound containing POSS structure is as follows: Among them, R1 is 3. The modified maleimide resin composition containing POSS structure according to claim 1, characterized in that: The polyphenylene ether is a polyphenylene ether containing carbon-carbon unsaturated groups, and one end, two ends or a side chain of the polyphenylene ether containing carbon-carbon unsaturated groups contains at least any one of vinyl, allyl, propenyl, acrylate or methacrylate groups.

4. The modified maleimide resin composition containing POSS structure according to claim 1, characterized in that: The structural formula of the 1,2-bis(4-vinylphenyl)ethane is 5. The modified maleimide resin composition containing POSS structure according to claim 1, characterized in that: The invention further comprises 1-30 parts of hydrocarbon resin.

6. The modified maleimide resin composition containing POSS structure according to claim 5, characterized in that: The hydrocarbon resin is at least one of polybutadiene, modified polybutadiene, polypentadiene, modified polypentadiene, polyisoprene, modified polyisoprene, polystyrene, butadiene-styrene copolymer, styrene-butadiene-styrene copolymer, hydrogenated diene-butadiene-styrene copolymer, maleic anhydride diene-butadiene-styrene copolymer, styrene-isoprene-styrene copolymer, styrene-butadiene-divinylbenzene copolymer, maleic anhydride styrene-butadiene copolymer, cyclopentadiene, modified cyclopentadiene, dicyclopentadiene, modified dicyclopentadiene, styrene-pentadiene copolymer, styrene-polypentadiene copolymer, butadiene-cyclopentadiene copolymer, ethylene-cyclopentadiene copolymer, norbornene polymer, and modified norbornene polymer.

7. A prepreg, characterized in that: The invention is prepared from the modified maleimide resin composition containing POSS structure as described in any one of claims 1 to 6.

8. A copper foil substrate, characterized in that: Prepared from the prepreg according to claim 7.

Citation Information

Patent Citations

  • Maleimide with cage-type silsesquioxane structure and synthesis method thereof

    CN101723968A

  • Modified maleimide resin composition and prepreg and laminate prepared therefrom

    CN109054381A

  • Vinyl POSS (Polyhedral Oligomeric Silsesquioxane) modified bismaleimide resin condensate as well as preparation method and application thereof

    CN118240375A

  • Low dielectric constant, low dielectric dissipation factor coatings, films and adhesives

    US20160237311A1