Electrochromic polymer and large-scale purification method thereof
By using boron trifluoride ether complex electrochemical method, protonic acid doped polyaniline and polystyrene sulfonic acid doped poly3,4-ethylenedioxythiophene in electrochromic polymers, combined with magnetic force Cross-washing of stirring and methanol solves the problem of difficulty in redox reaction during polymer purification, and improves purification efficiency and conductivity.
Patent Information
- Application Number
- CN202411126887.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-01
AI Technical Summary
In the existing electrochromic polymer purification methods, the high chemical conductivity of the polymer leads to difficulty in redox reactions, affecting the effect of large-scale purification, and the low intensity after purification affects the conductivity.
The electrochemical method of the boron trifluoride ether complex was used to perform redox doped polythiophene, protonic acid doped polyaniline, polystyrene sulfonic acid doped poly3,4-ethylenedioxythiophene, and magnetic stirring Purification was carried out with methanol cross-wash to reduce polymerization potential and improve conductivity.
It shortens purification time, improves production efficiency, avoids the use of flammable and explosive chemicals during high-temperature reflux, enhances the strength and conductivity of the polymer, and improves purification degree and stability.
Smart Images

Figure CN118878795A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electrochromic polymers, in particular to an electrochromic polymer and a large-scale purification method thereof. Background Art
[0002] Electrochromic polymers are a type of conductive polymer that can undergo reversible redox under the action of an electric field and whose color changes reversibly in appearance. Conductive polymers such as polythiophene, polypyrrole, and polyacetylene can all be used as electrochromic materials. Unlike ordinary polymers, the main chain of this type of material is a conjugated structure formed by alternating single and double bonds, which makes it difficult for the polymer to be dissolved in commonly used organic solvents, increases the difficulty of polymer post-processing, and limits its subsequent application as a photoelectric material. In order to increase its solubility, it is necessary to introduce soluble groups into the side chains of the polymer to make the structure of the polymer more complex.
[0003] Soluble electrochromic polymers can be prepared in solution by means of chemical synthesis. These include: ferric chloride oxidation polymerization, Stille coupling polymerization, Suzuki coupling polymerization and direct arylation polymerization. However, these synthesis methods all require the introduction of inorganic metal-based catalysts (ferric chloride, palladium acetate, etc.) and specific inorganic metal salts (potassium carbonate, etc.) during the synthesis process to ensure the normal progress of the reaction. These inorganic components and oligomers and low molecular weight components produced by side reactions will significantly affect the photoelectric properties of the material during application. How to efficiently remove the above-mentioned inorganic substances and low molecular weight components has become one of the key points of the industrialization of electrochromic polymers.
[0004] In the existing electrochromic polymer purification method, such as an electrochromic polymer and a method for large-scale purification of electrochromic polymers with publication number CN111349216B, the technical scheme is as follows: the method comprises the following steps: pouring the unpurified electrochromic polymer obtained by the reaction into a methanol solution for precipitation, filtering and separating to obtain a crude electrochromic polymer, dissolving the crude product, and passing through a chromatography column, concentrating the polymer after chromatography, and performing secondary precipitation under stirring conditions, filtering and separating the precipitated polymer, and obtaining a purified electrochromic polymer after vacuum drying. The present invention is based on the principles of adsorption and polymer precipitation classification, replacing the original method for purifying electrochromic polymers based on liquid-solid extraction. The present invention can shorten the original purification process of 2 days to several weeks to 1 to 2 days, improve production efficiency, and avoid the process of using a variety of flammable and explosive chemicals under high temperature reflux when using a Soxhlet extractor.
[0005] In the prior art, during the reaction purification process of electrochromic polymers, the redox reaction is more difficult when the conductive polymerization potential of the chemical property of the polymer is high, which affects the purification of large-scale electrochromic polymers. The strength of the purified polymer is low, which affects the unsatisfactory conductive effect.
[0006] In view of this, we conducted in-depth research on the above issues, which led to the present case.
[0007] In view of the above problems, an innovative design was carried out based on the original electrochromic polymer purification method. Summary of the invention
[0008] The object of the present invention is to provide an electrochromic polymer and a large-scale purification method thereof, so as to solve the problem in the above background technology that the chemical polymerization potential of the polymer is relatively high, the redox reaction is difficult and affects the purification reaction.
[0009] To achieve the above object, the present invention provides the following technical solutions:
[0010] An electrochromic polymer and a large-scale purification method thereof, comprising an electrochromic polymer, wherein the electrochromic polymer comprises polythiophene, polyaniline and poly-3,4-ethylenedioxythiophene, wherein the polythiophene is a red amorphous solid, and the polythiophene comprises an organic hydrocarbon group, a halogen atom, a cyano group, an alkyl group, an ester group, an aryl group, an aralkyl group, an alkenyl group, a single bond, a double bond and a triple bond, and the polyaniline in the electrochromic polymer comprises a P electron conjugated structure. The large-scale purification method of the electrochromic polymer comprises the following steps:
[0011] Step 1, redox doping polythiophene using a boron trifluoride ether complex electrochemical method;
[0012] Step 2, redox doping of polyaniline using a protonic acid doping type;
[0013] Step 3, doping poly (3,4-ethylenedioxythiophene) with polystyrene sulfonic acid;
[0014] Step 4: magnetically stir the electrochromic polymer, add methanol, stir and filter, and dry to obtain a purified product.
[0015] Preferably, the specific steps of step one are: doping the polythiophene with a boron trifluoride ether complex solution, and synthesizing the polythiophene in the boron trifluoride ether complex solution by a constant potential method.
[0016] By adopting the above technical scheme, polythiophene is insoluble and has high strength. The strength of polythiophene obtained by electrochemical polymerization in a boron trifluoride ether complex is greater than that of metallic aluminum. The polymerization potential of polythiophene is very high, usually above 2.0V. Using a boron trifluoride ether complex as a solvent can greatly reduce the polymerization potential of thiophene, facilitating redox reactions.
[0017] Preferably, the specific steps of step 1 are: filtering the polythiophene and passing it through a chromatography column, placing the chromatographic polythiophene on a rotary evaporator for concentration, and then performing secondary precipitation in an isopropanol solution.
[0018] By adopting the above technical solution, the polymerization potential of the doped polythiophene is reduced, which is convenient for redox reaction and easier to purify during filtration and chromatography.
[0019] Preferably, the specific steps of step 2 are: polyaniline reacts from a reduced state to an oxidized state in a lithium perchlorate electrolyte solution with perchloric acid as a doping acid, until its color changes to yellow, green, blue and purple.
[0020] By adopting the above technical scheme, polyaniline belongs to the proton acid doping type. During the doping process with the lithium perchlorate electrolyte solution, there is no gain or loss of electrons, so that the main chain of the conductive polymer carries a positive charge during oxidation doping and carries a negative charge during reduction doping, thereby maintaining electrical neutrality.
[0021] Preferably, the specific steps of step 2 are: subjecting the polyaniline solution to activated carbon adsorption treatment for recrystallization.
[0022] By adopting the above technical solution, the activated carbon is used to adsorb the polyaniline solution, which has low cost, is convenient for preparing the motor, and improves the conductive property of the polyaniline.
[0023] Preferably, the specific steps of step three are: adding 100 ml of concentrated sulfuric acid and 0.2 g of silver sulfate into a flask, completely sealing the flask, adding 10 g of polystyrene ten times at 100° C., and stirring at intervals of 15 minutes.
[0024] By adopting the above technical solution, the sulfonation degree of the doped catalyst can be improved, and polystyrene sulfonic acid can be generated, thereby improving the conductive properties of poly (3,4-ethylenedioxythiophene).
[0025] Preferably, the specific steps of step three are: pouring the reaction mixture into deionized water at 5-10°C, stirring thoroughly to dissolve, placing it in a 2-10°C environment for refrigeration for 48 hours, using BaCl2 to test the dialyzate until there is no white precipitate, and placing it in a 90°C oven for drying to obtain polystyrene sulfonic acid doped with poly (3,4-ethylenedioxythiophene).
[0026] By adopting the above technical solution, since the rigidity of the molecular chain and the strong interaction between the chains make it less soluble, polystyrene sulfonic acid is doped into poly (3,4-ethylenedioxythiophene) to improve the stability of its conductive properties and provide catalytic assistance for purification treatment.
[0027] Preferably, the specific steps of step 4 are: placing the electrochromic polymer at 10-30° C., magnetically stirring for 24 hours, pouring the mixed solution after the reaction into methanol with a methanol content of 500 ml, magnetically stirring again for 60 minutes, and standing for 36 hours.
[0028] Using the above technical solution, methanol is a polar solvent that can dissolve many organic and inorganic substances. Compared with other organic solvents, methanol has lower toxicity and will not cause great harm to the human body. The chemical properties of methanol are relatively stable, and it is not easily oxidized or decomposed, and it is not easily decomposed by water, which provides a role for the washing of electrochromic polymers.
[0029] Preferably, the specific steps of step 4 are: filtering the solution after standing, cross-washing with methanol and deionized water, placing in an oven for vacuum drying at 60° C. for 24 hours to obtain a purified product.
[0030] By adopting the above technical scheme, the mixed solution is cross-washed with deionized water by taking advantage of the fact that methanol is not easily decomposed by water, so as to improve the purity of the purified product and enhance the stability of the electrochromic effect.
[0031] Compared with the prior art, the present invention has the following beneficial effects: the electrochromic polymer and its large-scale purification method,
[0032] 1. The method comprises doping with a boron trifluoride ether complex solution, doping the polythiophene with the boron trifluoride ether complex solution, and synthesizing the polythiophene in the boron trifluoride ether complex solution by a constant potential method, doping the polythiophene with a boron trifluoride ether complex solution, and synthesizing the polythiophene in the boron trifluoride ether complex solution by a constant potential method;
[0033] 2. A method of doping with a lithium perchlorate electrolyte solution is provided, wherein the polyaniline reacts from a reduced state to an oxidized state in the lithium perchlorate electrolyte solution with perchloric acid as the doping acid, until the color thereof changes to yellow, green, blue and purple. The method of doping with a lithium perchlorate electrolyte solution with perchloric acid as the doping acid reacts from a reduced state to an oxidized state, until the color thereof changes to yellow, green, blue and purple.
[0034] 3. The method is provided with polystyrene sulfonic acid doping, the reaction mixture is poured into deionized water at 5-10°C, fully stirred and dissolved, placed in a 2-10°C environment for refrigeration for 48 hours, the dialyzate is tested with BaCl2 until there is no white precipitate, and placed in a 90°C oven for drying to obtain polystyrene sulfonic acid doped with poly (3,4-ethylenedioxythiophene). Due to the rigidity of the molecular chain and the strong interaction between the chains, its solubility is poor. The polystyrene sulfonic acid doped with poly (3,4-ethylenedioxythiophene) improves the stability of its conductive properties and performs catalytic auxiliary effect for purification treatment;
[0035] 4. Place the electrochromic polymer at 10-30°C and stir magnetically for 24 hours. Pour the mixed solution after the reaction into methanol with a methanol content of 500 ml. Stir magnetically for 60 minutes again and let it stand for 36 hours. Filter the solution after standing, cross-wash with methanol and deionized water, and place in an oven for vacuum drying at 60°C for 24 hours to obtain a purified product. By taking advantage of the fact that methanol is not easily decomposed by water, the mixed solution is cross-washed with deionized water to improve the purity of the purified product and improve the stability of the electrochromic effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 is the chemical structural formula of the polythiophene of the present invention. DETAILED DESCRIPTION
[0037] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0038] See also Figure 1 , the present invention provides a technical solution:
[0039] An electrochromic polymer and a large-scale purification method thereof, comprising an electrochromic polymer, wherein the electrochromic polymer comprises polythiophene, polyaniline and poly-3,4-ethylenedioxythiophene, wherein the polythiophene is a red amorphous solid, and the polythiophene comprises an organic hydrocarbon group, a halogen atom, a cyano group, an alkyl group, an ester group, an aryl group, an aralkyl group, an alkenyl group, a single bond, a double bond and a triple bond, and the polyaniline in the electrochromic polymer comprises a P electron conjugated structure. The large-scale purification method of the electrochromic polymer comprises the following steps:
[0040] Step 1, redox doping polythiophene using a boron trifluoride ether complex electrochemical method;
[0041] Step 2, redox doping of polyaniline using a protonic acid doping type;
[0042] Step 3, doping poly (3,4-ethylenedioxythiophene) with polystyrene sulfonic acid;
[0043] Step 4: magnetically stir the electrochromic polymer, add methanol, stir and filter, and dry to obtain a purified product.
[0044] The specific steps of step one are: doping polythiophene with a boron trifluoride ether complex solution, and synthesizing polythiophene in the boron trifluoride ether complex solution by a constant potential method. The specific steps of step one are: filtering the polythiophene, passing it through a chromatography column, placing the chromatographic polythiophene on a rotary evaporator for concentration, and then performing secondary precipitation in an isopropanol solution. Polythiophene is insoluble and has high strength. The strength of the polythiophene obtained by electrochemical polymerization in a boron trifluoride ether complex is greater than that of metallic aluminum. The polymerization potential of polythiophene is very high, usually above 2.0V. Using a boron trifluoride ether complex as a solvent can greatly reduce the polymerization potential of thiophene, which is convenient for redox reactions. The polymerization potential of the doped polythiophene is reduced, which is convenient for redox reactions and easier to purify during filtration and chromatography.
[0045] The specific steps of step 2 are: polyaniline reacts from a reduced state to an oxidized state in an electrolyte solution of lithium perchlorate with perchloric acid as a doping acid, until its color changes to yellow, green, blue and purple. The specific steps of step 2 are: the polyaniline solution is treated by activated carbon adsorption and recrystallized. Polyaniline belongs to the proton acid doping type. During the doping process of the lithium perchlorate electrolyte solution, there is no gain or loss of electrons, so that the main chain of the conductive polymer is positively charged during oxidation doping, and the main chain of the conductive polymer is negatively charged during reduction doping, thereby maintaining electrical neutrality. Using activated carbon to adsorb polyaniline solution is low-cost, easy to prepare motors, and improves the conductive properties of polyaniline.
[0046] The specific steps of step three are: add 100ml concentrated sulfuric acid and 0.2g silver sulfate into a flask, seal the flask completely, add 10g polystyrene at 100°C in ten times, and stir at intervals of 15 minutes. The specific steps of step three are: pour the reaction mixture into 5-10°C deionized water, stir and dissolve it thoroughly, put it into a 2-10°C environment for refrigeration for 48 hours, use BaCl2 to check the dialyzate until there is no white precipitate, place it in a 90°C oven for drying, and obtain polystyrene sulfonic acid doped with poly 3,4-ethylenedioxythiophene. The sulfonation degree of the doped catalyst can be increased, and polystyrene sulfonic acid is generated to improve the conductive properties of poly 3,4-ethylenedioxythiophene. Due to the rigidity of the molecular chain and the strong interaction between the chains, its solubility is poor. Polystyrene sulfonic acid is doped with poly 3,4-ethylenedioxythiophene to improve its stability in conductive properties and perform catalytic auxiliary effects for purification treatment.
[0047] The specific steps of step four are: placing the electrochromic polymer at 10-30°C, magnetically stirring for 24 hours, pouring the mixed solution after the reaction into methanol, the methanol content is 500ml, magnetically stirring again for 60 minutes, and standing for 36 hours. The specific steps of step four are: filtering the solution after standing, cross-washing with methanol and deionized water, placing in an oven for vacuum drying at 60°C for 24 hours to obtain a purified product. Methanol is a polar solvent that can dissolve many organic and inorganic substances. Compared with other organic solvents, methanol has lower toxicity and will not cause great harm to the human body. The chemical properties of methanol are relatively stable, not easily oxidized or decomposed, and not easily decomposed by water, which provides a role for the washing of electrochromic polymers. Through the advantage of methanol's difficulty in water decomposition, the mixed solution is cross-washed with deionized water to improve the purity of the purified product and improve the stability of the electrochromic effect.
[0048] The contents not described in detail in this specification belong to the prior art known to professional and technical personnel in this field.
[0049] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. An electrochromic polymer and a large-scale purification method thereof, comprising an electrochromic polymer, characterized in that: The electrochromic polymer comprises polythiophene, polyaniline and poly (3,4-ethylenedioxythiophene), and the polythiophene is a red amorphous solid, and the polythiophene comprises an organic hydrocarbon group, a halogen atom, a cyano group, an alkyl group, an ester group, an aryl group, an aralkyl group, an alkenyl group, a single bond, a double bond and a triple bond, and the polyaniline in the electrochromic polymer comprises a P electron conjugated structure. The large-scale purification method of the electrochromic polymer comprises the following steps: Step 1, redox doping polythiophene using a boron trifluoride ether complex electrochemical method; Step 2, redox doping of polyaniline using a protonic acid doping type; Step 3, doping poly (3,4-ethylenedioxythiophene) with polystyrene sulfonic acid; Step 4: magnetically stir the electrochromic polymer, add methanol, stir and filter, and dry to obtain a purified product.
2. The electrochromic polymer and large-scale purification method thereof according to claim 1, characterized in that: The specific steps of step one are: doping the polythiophene with a boron trifluoride ether complex solution, and synthesizing the polythiophene in the boron trifluoride ether complex solution by a constant potential method.
3. The electrochromic polymer and large-scale purification method thereof according to claim 2, characterized in that: The specific steps of step 1 are: filtering the polythiophene and passing it through a chromatography column, placing the chromatographic polythiophene on a rotary evaporator for concentration, and then performing secondary precipitation in an isopropanol solution.
4. The electrochromic polymer and large-scale purification method thereof according to claim 1, characterized in that: The specific steps of step 2 are: polyaniline reacts from a reduced state to an oxidized state in a lithium perchlorate electrolyte solution with perchloric acid as a doping acid, until its color changes to yellow, green, blue and purple.
5. The electrochromic polymer and large-scale purification method thereof according to claim 1, characterized in that: The specific steps of step 2 are: treating the polyaniline solution through activated carbon adsorption to recrystallize it.
6. The electrochromic polymer and large-scale purification method thereof according to claim 1, characterized in that: The specific steps of step three are: adding 100 ml of concentrated sulfuric acid and 0.2 g of silver sulfate into a flask, completely sealing the flask, adding 10 g of polystyrene ten times at 100° C., and stirring at intervals of 15 minutes.
7. An electrochromic polymer and a large-scale purification method thereof according to claim 6, characterized in that: The specific steps of step three are: pouring the reaction mixture into deionized water at 5-10°C, stirring thoroughly to dissolve, refrigerating in a 2-10°C environment for 48 hours, testing the dialyzate with BaCl2 until no white precipitate is present, drying in a 90°C oven, and doping with poly (3,4-ethylenedioxythiophene).
8. The electrochromic polymer and large-scale purification method thereof according to claim 1, characterized in that: The specific steps of step 4 are: placing the electrochromic polymer at 10-30° C. and magnetically stirring for 24 hours, pouring the mixed solution after the reaction into methanol with a methanol content of 500 ml, magnetically stirring again for 60 minutes, and standing for 36 hours.
9. An electrochromic polymer and a large-scale purification method thereof according to claim 8, characterized in that: The specific steps of step 4 are: filtering the solution after standing, cross-washing with methanol and deionized water, placing in an oven for vacuum drying at 60° C. for 24 hours to obtain a purified product.