Tackifying resin modified polyol for polyurethane adhesive and preparation method of tackifying resin modified polyol
Polycondensation reaction of tackifying resin, polyacid and small molecule polyol under the action of catalysts, terminal hydroxyl polyols are prepared, which solves the problem of poor bonding of polyurethane adhesives on low-surface energy substrates, and improves the comprehensiveness of polyurethane adhesives Performance and high and low temperature resistance.
Patent Information
- Application Number
- CN202411193952.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-01
AI Technical Summary
The existing polyurethane adhesives have poor adhesion effect on low-surface energy substrates (such as PP and PE), and have insufficient hydrolysis resistance, making it difficult to prepare polyurethane adhesives with high comprehensive performance.
Under the action of a catalyst, the viscosity-enhancing resin, polyacid and small molecule polyol are carried out to undergo polycondensation reaction, and end-hydroxyl polyols with low cohesion energy and low crystallinity are prepared. It is used to prepare polyurethane adhesives and improve their low surface energy base. The bonding effect and high and low temperature resistance of the material.
It has achieved good bonding effect on low-surface energy substrates and improved comprehensive performance of polyurethane adhesives, and has high fluidity and good high and low temperature resistance.
Abstract
Description
Technical Field
[0001] The invention relates to the field of polyurethane adhesives, and in particular to a tackifying resin modified polyol for polyurethane adhesives and a preparation method thereof. Background Art
[0002] Polyurethane adhesives are widely used due to their strong bonding strength, good resistance to high and low temperatures, oil resistance, and good softness. However, due to the high polarity of polyurethane, it has poor bonding effect on low surface energy substrates (such as PP, PE, etc.), and its relatively insufficient hydrolysis resistance also limits its scope of application. Generally, polyurethane adhesives can be prepared by combining two or more of the above raw materials. However, the polyurethane prepared in this way is just a simple superposition or compounding of physical constants, and it is difficult to prepare polyurethane adhesive products with high comprehensive performance. For this reason, many scholars have used chemical polymerization methods to solve the problem. For example, a Japanese patent uses acrylic acid monomers and polymer polyols with a molecular weight distribution of 1000 to 20000 to polymerize, and uses active hydrogen-containing compounds (such as 2,2-azobishydroxymethylpropionitrile) as initiators to obtain terminal hydroxyl-containing acrylic polymers, which are then reacted with polyisocyanates. The adhesive obtained by this method has high bonding strength and resistance to boiling (KOBA YASHI. One-component moisture-curable polyurethane adhesives and sealants [P], JP2001005129, 2001.).
[0003] Rosin is a mixture of natural condensed heterocyclic compounds, with a general molecular formula of C19H29COOH. The main component is abietic acid. The acid value of rosin is an indicator of its acidity, and its standard value should be between 120 and 160 mgKOH / g. On the market, rosin and polyols (such as diethylene glycol and ethylene glycol) are esterified to prepare small molecular weight rosin ester polyols, with a molecular weight generally less than 1000. Applied to polyurethane rigid foam, it has good miscibility with other raw materials and excellent heat resistance and flame retardancy (Handbook of Polyurethane Raw Materials and Additives, Liu Yijun, 2012.11). However, due to its low molecular weight, the prepared polyurethane adhesive has high hardness and weak adhesion to the substrate.
[0004] Terpene is a class of naturally occurring hydrocarbons widely found in plants, and can be obtained from many plants, especially conifers. It is the main component of resin and turpentine derived from resin, and has good adhesion to a variety of substrates, especially low surface energy substrates. Terpene phenol resin is a phenol-modified resin with increased polarity. It is an excellent tackifier for polyurethane, acrylic resin, styrene-butadiene rubber, natural rubber and chloroprene rubber. Terpene phenol resin has a stronger tackifying effect than other resins, has heat resistance, stable color, and can be miscible with many polymer resins in a wide range, and can be dissolved in many polar or non-polar solvents. Terpene phenol resin is widely used in hot melt adhesives, pressure-sensitive adhesives, coatings, inks, printed circuits, plastic modification, rubber products, etc.
[0005] The raw materials of existing polyester polyols are mostly: dibasic acids, such as adipic acid, phthalic anhydride, isophthalic acid, etc., and diols are ethylene glycol, 1,4-butanediol, etc. The prepared polyester polyols have very high cohesive energy, but the adhesion to low surface energy substrates is not ideal. Generally, the substrates such as PP and PE surfaces need to be treated with corona or plasma. However, corona treatment can only maintain a very short validity period and is affected by the environment, such as moisture. Plasma treatment is expensive and not suitable for the treatment of complex parts. The polyester polyol of the present invention introduces a tackifying resin to reduce the cohesive energy and crystallinity of the polyester polyol, so that the prepared polyurethane adhesive has good adhesion to low surface energy substrates such as PP and PE.
[0006] In view of this, the present invention is proposed. Summary of the invention
[0007] The purpose of the present invention is to provide a tackifying resin modified polyol for polyurethane adhesive and a preparation method thereof, which has good adhesion to substrates with low surface energy, can improve the comprehensive performance of polyurethane adhesive, and thus solve the above-mentioned technical problems existing in the prior art.
[0008] The objective of the present invention is achieved through the following technical solutions:
[0009] A tackifying resin modified polyol for polyurethane adhesive is a terminal hydroxyl polyol prepared by polycondensation reaction of tackifying resin, dibasic acid and small molecule polyol under the action of a catalyst.
[0010] Preferably, in the above-mentioned tackifying resin modified polyol, the terminal hydroxyl polyol has a hydroxyl value of 10 to 120 mgKOH / g and an acid value of 0.1 to 3 mgKOH / g.
[0011] Preferably, in the above-mentioned tackifying resin modified polyol, the tackifying resin is a mixture of natural rosin resin and terpene phenol resin, or any one of natural rosin resin and terpene phenol resin.
[0012] Preferably, in the above-mentioned tackifying resin modified polyol, the dibasic acid is any one or more of dimer acid, malonic acid, succinic acid, adipic acid, and sebacic acid.
[0013] Preferably, in the above-mentioned tackifying resin modified polyol, the catalyst is any one or more of tetrabutyl titanate, stannous octoate and tetraisopropyl titanate.
[0014] Preferably, in the above-mentioned tackifying resin modified polyol, the small molecule polyol is any one or more of 1,4-butanediol, 1,6-hexanediol, isoprene glycol, pentanediol, ethylene glycol, trimethylolpropane, 1,2-propylene glycol and diethylene glycol.
[0015] A method for preparing a tackifying resin modified polyol for a polyurethane adhesive according to the present invention is characterized by comprising the following steps:
[0016] Step A, adding a tackifying resin, a dibasic acid, a small molecule polyol and a catalyst into a reaction kettle in sequence, sealing with nitrogen and heating, and when the temperature rises to 140-150° C., controlling the reflux tower top temperature of the reaction kettle at 98-105° C., and heating to 200-255° C. at a heating rate of 10-20° C. per hour;
[0017] Step B, reacting at 220-225° C. for 2-8 hours, when the water yield reaches more than 90% or the acid value drops below 30 mgKOH / g, starting the vacuum pump of the reactor with a vacuum degree of 1000-5000 Pa, until the acid value drops below 1.0 mgKOH / g, the obtained product is a tackifying resin modified polyol for polyurethane adhesive.
[0018] Compared with the prior art, the tackifying resin modified polyol for polyurethane adhesive provided by the present invention and the preparation method thereof have the following beneficial effects:
[0019] Due to the addition of tackifying resin for polycondensation reaction, the obtained terminal hydroxyl polyol has low cohesive energy, low crystallinity, good fluidity and good wettability to the substrate. Therefore, this terminal hydroxyl polyol has a good bonding effect on low surface energy substrates (such as PP and PE, etc.), and can be used in polyurethane adhesives to make the performance of polyurethane adhesives excellent; in addition, since polyester polyol is the soft segment part of polyurethane adhesive, it has low crystallinity and low cohesive energy and high crystallinity, and the hard segment part with high cohesive energy has good microphase separation, the terminal hydroxyl polyol also has good high and low temperature resistance. DETAILED DESCRIPTION
[0020] The following is a clear and complete description of the technical solutions in the embodiments of the present invention in combination with the specific content of the present invention; it is obvious that the described embodiments are only part of the embodiments of the present invention, not all of the embodiments, which does not constitute a limitation of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the protection scope of the present invention.
[0021] First, the terms that may be used in this article are explained as follows:
[0022] The term “and / or” means that either or both of them can be realized at the same time. For example, X and / or Y means both “X” or “Y” and “X and Y”.
[0023] The terms "include", "comprises", "contains", "has" or other descriptions with similar semantics should be interpreted as non-exclusive inclusion. For example, including certain technical feature elements (such as raw materials, components, ingredients, carriers, dosage forms, materials, dimensions, parts, components, mechanisms, devices, steps, procedures, methods, reaction conditions, processing conditions, parameters, algorithms, signals, data, products or products, etc.) should be interpreted as including not only certain technical feature elements explicitly listed, but also other technical feature elements known in the art that are not explicitly listed.
[0024] The term "consisting of..." means excluding any technical feature elements not explicitly listed. If this term is used in a claim, it will make the claim closed, so that it does not contain technical feature elements other than the technical feature elements explicitly listed, except for the conventional impurities related to them. If this term only appears in a clause of a claim, it only limits the elements explicitly listed in the clause, and the elements recorded in other clauses are not excluded from the overall claim.
[0025] The term "parts by mass" refers to the mass ratio relationship between multiple components. For example, if it is described that component X is x parts by mass and component Y is y parts by mass, then the mass ratio of component X to component Y is x:y. 1 part by mass can represent any mass, for example, 1 part by mass can be represented as 1 kg or 3.1415926 kg. The sum of the parts by mass of all components is not necessarily 100 parts, but can be greater than 100 parts, less than 100 parts or equal to 100 parts. Unless otherwise specified, the parts, proportions and percentages described herein are all measured by mass.
[0026] When concentration, temperature, pressure, size or other parameters are expressed in the form of a numerical range, the numerical range should be understood to specifically disclose all ranges formed by the pairing of any upper limit, lower limit, and preferred value in the numerical range, regardless of whether the range is explicitly stated; for example, if a numerical range of "2 to 8" is stated, the numerical range should be interpreted as including ranges such as "2 to 7", "2 to 6", "5 to 7", "3 to 4 and 6 to 7", "3 to 5 and 7", "2 and 5 to 7", etc. Unless otherwise specified, the numerical ranges stated herein include both their end values and all integers and fractions within the numerical range.
[0027] The scheme provided by the present invention is described in detail below. The contents not described in detail in the embodiments of the present invention belong to the prior art known to professionals in the field. If the specific conditions are not specified in the embodiments of the present invention, they are carried out according to the conventional conditions in the field or the conditions recommended by the manufacturer. If the manufacturers are not specified in the reagents or instruments used in the embodiments of the present invention, they are all conventional products that can be purchased commercially.
[0028] The embodiment of the present invention provides a tackifying resin modified polyol for use in the field of polyurethane adhesives. The tackifying resin modified polyol is a hydroxyl-terminated polyol prepared by polycondensation of a tackifying resin, a dibasic acid and a small molecule polyol under the action of a catalyst.
[0029] Preferably, the hydroxyl value of the above-mentioned terminal hydroxyl polyol is 10 to 120 mgKOH / g, and the acid value is 0.1 to 3 mgKOH / g.
[0030] Preferably, in the above-mentioned tackifying resin modified polyol, the tackifying resin is a mixture of natural rosin resin and terpene phenol resin, natural rosin resin, or any one of terpene phenol resin.
[0031] Preferably, in the above-mentioned tackifying resin modified polyol, the dibasic acid is any one or more of dimer acid, malonic acid, succinic acid, adipic acid, and sebacic acid.
[0032] Preferably, in the above-mentioned tackifying resin modified polyol, the small molecule polyol is any one or more of 1,4-butanediol, 1,6-hexanediol, isoprene glycol, pentanediol, ethylene glycol, trimethylolpropane, 1,2-propylene glycol and diethylene glycol.
[0033] Preferably, in the above-mentioned tackifying resin modified polyol, the catalyst is any one or more of tetrabutyl titanate, stannous octoate and tetraisopropyl titanate.
[0034] The present invention also provides a method for preparing the above-mentioned tackifying resin modified polyol for polyurethane adhesive, comprising the following steps:
[0035] Step A, adding tackifying resin, dibasic acid, small molecule polyol and catalyst into a reaction kettle in sequence, sealing with nitrogen, heating, and when the temperature rises to 140-150° C., controlling the top temperature of the reflux tower at 98-105° C., and heating to 200-255° C. at a heating rate of 10-20° C. per hour;
[0036] Step B, reacting at 220-225° C. for 2-8 hours, when the water yield reaches more than 90% or the acid value drops below 30 mgKOH / g, starting the vacuum pump and increasing the vacuum degree to 1000-5000 Pa until the acid value drops below 1.0 mgKOH / g, the obtained product is a tackifying resin modified polyol for polyurethane adhesive.
[0037] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0038] By adding a mixture of natural rosin resin and terpene phenol resin, or any one of natural rosin resin and terpene phenol resin as a tackifying resin for polycondensation reaction, the obtained terminal hydroxyl polyol has low cohesive energy, low crystallinity, good fluidity, and good wettability to the substrate. Therefore, this terminal hydroxyl polyol has a good bonding effect on low surface energy substrates (such as PP and PE, etc.), and can be used in polyurethane adhesives to make the performance of polyurethane adhesives excellent; in addition, since polyester polyol is the soft segment part of polyurethane adhesive, it has low crystallinity and low cohesive energy and high crystallinity, and the hard segment part with high cohesive energy has good microphase separation, the terminal hydroxyl polyol also has good high and low temperature resistance.
[0039] In order to more clearly demonstrate the technical solution and technical effects provided by the present invention, the solution provided by the embodiment of the present invention is described in detail with specific embodiments below.
[0040] Example 1
[0041] This embodiment provides a tackifying resin modified polyol for use in the field of polyurethane adhesives, which is prepared according to the following steps, including:
[0042] Add 600 kg of rosin, 1072 kg of adipic acid, 300 kg of dimer acid, 1600 kg of isoprene glycol and 1 kg of tetraisobutyl titanate as a catalyst into a reaction kettle in sequence; after heating to 150° C., control the reflux tower top temperature of the reaction kettle to be between 99 and 101° C., heat to 230° C. at a heating rate of 10° C. per hour, react at 240° C. for 3 hours, and when the water yield reaches more than 90%, start a vacuum pump to evacuate until the acid value is reduced to less than 1.0 mgKOH / g, so as to prepare a terminal hydroxyl polyol with a hydroxyl value of 45 mgKOH / g and an acid value of 0.20 mgKOH / g, namely, a tackifying resin modified polyol.
[0043] The tackifying resin modified polyol of this embodiment is used to prepare a reactive polyurethane hot melt adhesive: the tackifying resin modified polyol is dehydrated at 120°C in a vacuum for 2 hours, pure MDI is added (the molar ratio of pure MDI: tackifying resin modified polyol = 1.8:1), reacted at 120°C for 2 hours, and the NCO is detected to reach the theoretical value before discharging and packaging.
[0044] After curing at room temperature for 1 week, the bonding properties of the prepared product are as follows:
[0045] Bonding strength / Mpa Low temperature performance High temperature performance PP 11 The colloid does not crack or debond. The colloid does not flow or soften PE 3.5 The colloid does not crack or debond. The colloid does not flow or soften ABS 17 The colloid does not crack or debond. The colloid does not flow or soften
[0046] Note: Low temperature performance refers to -40 degrees, stationary for 12 hours. High temperature performance refers to 150 degrees, stationary for 12 hours.
[0047] Example 2
[0048] This embodiment provides a tackifying resin modified polyol for use in the field of polyurethane adhesives, which is prepared according to the following steps, including:
[0049] Add 300 kg of rosin, 200 kg of terpene phenol, 1000 kg of dimer acid, 1300 kg of isoprene glycol and 1 kg of tetraisobutyl titanate as a catalyst into a reaction kettle in sequence; after heating to 150° C., control the reflux tower top temperature of the reaction kettle to be between 99 and 101° C., heat the reaction kettle to 230° C. at a heating rate of 10° C. per hour, react at 240° C. for 3 hours, and when the water yield reaches more than 90%, start a vacuum pump to evacuate until the acid value is reduced to less than 1.0 mgKOH / g, so as to prepare a terminal hydroxyl polyol with a hydroxyl value of 35 mgKOH / g and an acid value of 0.20 mgKOH / g, namely, a tackifying resin modified polyol.
[0050] The tackifying resin modified polyol of this embodiment is used to prepare a reactive polyurethane hot melt adhesive: the tackifying resin modified polyol is dehydrated at 120°C in a vacuum for 2 hours, pure MDI is added (the molar ratio of pure MDI: tackifying resin modified polyol = 1.8:1), reacted at 120°C for 2 hours, and the NCO is detected to reach the theoretical value before discharging and packaging.
[0051] After curing at room temperature for 1 week, the bonding properties of the prepared product are as follows:
[0052] Bonding strength / Mpa Low temperature performance High temperature performance PP 12 The colloid does not crack or debond. The colloid does not flow or soften PE 4 The colloid does not crack or debond. The colloid does not flow or soften ABS 15 The colloid does not crack or debond. The colloid does not flow or soften
[0053] Example 3
[0054] This embodiment provides a tackifying resin modified polyol for use in the field of polyurethane adhesives, which is prepared according to the following steps, including:
[0055] 400 kg of original rosin, 300 kg of terpene phenol, 772 kg of adipic acid, 300 kg of dimer acid, 1500 kg of isoprene glycol and 1 kg of tetraisobutyl titanate as a catalyst are sequentially added into a reaction kettle; after heating to 150° C., the reflux tower top temperature of the reaction kettle is controlled to be between 99 and 101° C., the temperature is raised to 230° C. at a heating rate of 10° C. per hour, and the reaction is carried out at 240° C. for 3 hours. When the water yield reaches more than 90%, a vacuum pump is turned on to evacuate until the acid value is reduced to less than 1.0 mgKOH / g, and a terminal hydroxyl polyol with a hydroxyl value of 54 mgKOH / g and an acid value of 0.20 mgKOH / g is prepared, which is a tackifying resin modified polyol.
[0056] The tackifying resin modified polyol of this embodiment is used to prepare a reactive polyurethane hot melt adhesive: the tackifying resin modified polyol is dehydrated at 120°C in a vacuum for 2 hours, pure MDI is added (the molar ratio of pure MDI: tackifying resin modified polyol = 1.8:1), reacted at 120°C for 2 hours, and the NCO is detected to reach the theoretical value before discharging and packaging.
[0057] After curing at room temperature for 1 week, the bonding properties of the prepared product are as follows:
[0058] Bonding strength / Mpa Low temperature performance High temperature performance PP 9 The colloid does not crack or debond. The colloid does not flow or soften PE 3.5 The colloid does not crack or debond. The colloid does not flow or soften ABS 25 The colloid does not crack or debond. The colloid does not flow or soften
[0059] Example 4
[0060] This embodiment provides a tackifying resin modified polyol for use in the field of polyurethane adhesives, which is prepared according to the following steps, including:
[0061] Add 300 kg of terpene phenol, 872 kg of adipic acid, 1702 kg of succinic acid, 2600 kg of pentanediol and 2.5 kg of stannous octoate as a catalyst into a reaction kettle in sequence; after heating to 150 ° C, control the reflux tower top temperature of the reaction kettle to be between 99 and 101 ° C, heat to 230 ° C at a heating rate of 10 ° C per hour, react for 3 hours at 240 ° C, and when the water output rate reaches more than 90%, start a vacuum pump to evacuate until the acid value is reduced to less than 1.0 mgKOH / g, and prepare a terminal hydroxyl polyol with a hydroxyl value of 37 mgKOH / g and an acid value of 0.20 mgKOH / g, that is, a tackifying resin modified polyol.
[0062] The tackifying resin modified polyol of this embodiment is used to prepare a reactive polyurethane hot melt adhesive: the tackifying resin modified polyol is dehydrated at 120°C in a vacuum for 2 hours, pure MDI is added (the molar ratio of pure MDI: tackifying resin modified polyol = 1.8:1), reacted at 120°C for 2 hours, and the NCO is detected to reach the theoretical value before discharging and packaging.
[0063] After curing at room temperature for 1 week, the bonding properties of the prepared product are as follows:
[0064] Bonding strength / Mpa Low temperature performance High temperature performance PP 9 The colloid does not crack or debond. The colloid does not flow or soften PE 3 The colloid does not crack or debond. The colloid does not flow or soften ABS 15 The colloid does not crack or debond. The colloid does not flow or soften
[0065] The above is only a preferred specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by any technician familiar with the technical field within the technical scope disclosed in the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims. The information disclosed in the background technology section of this article is only intended to deepen the understanding of the overall background technology of the present invention, and should not be regarded as an admission or in any form that the information constitutes prior art known to those skilled in the art.
Claims
1. A tackifying resin modified polyol for polyurethane adhesive, characterized in that: The tackifying resin modified polyol is a terminal hydroxyl polyol prepared by polycondensation reaction of tackifying resin, dibasic acid and small molecule polyol under the action of a catalyst.
2. The tackifying resin modified polyol for polyurethane adhesive according to claim 1, characterized in that: The terminal hydroxyl polyol has a hydroxyl value of 10 to 120 mgKOH / g and an acid value of 0.1 to 3 mgKOH / g.
3. The tackifying resin modified polyol for polyurethane adhesive according to claim 1, characterized in that: The tackifying resin is a mixture of natural rosin resin and terpene phenol resin, or any one of natural rosin resin and terpene phenol resin.
4. The tackifying resin modified polyol for polyurethane adhesive according to any one of claims 1 to 3, characterized in that: The dibasic acid is any one or more of p-dimer acid, malonic acid, succinic acid, adipic acid, and sebacic acid.
5. The tackifying resin modified polyol for polyurethane adhesive according to any one of claims 1 to 3, characterized in that: The catalyst is any one or more of tetrabutyl titanate, stannous octoate and tetraisopropyl titanate.
6. The tackifying resin modified polyol for polyurethane adhesive according to any one of claims 1 to 3, characterized in that: The small molecule polyol is any one or more of 1,4-butanediol, 1,6-hexanediol, isoprene diol, pentanediol, ethylene glycol, trimethylolpropane, 1,2-propylene glycol and diethylene glycol.
7. A method for preparing a tackifying resin modified polyol for polyurethane adhesive according to any one of claims 1 to 6, characterized in that: The following steps are involved: Step A, adding a tackifying resin, a dibasic acid, a small molecule polyol and a catalyst to the reaction in sequence, sealing with nitrogen and heating, when the temperature rises to 140-150° C., controlling the reflux tower top temperature of the reactor at 98-105° C., and heating at a heating rate of 10-20° C. per hour to 200-255° C.; Step B, reacting at 220-225° C. for 2-8 hours, when the water yield reaches more than 90% or the acid value drops below 30 mgKOH / g, starting the vacuum pump of the reactor with a vacuum degree of 1000-5000 Pa, until the acid value drops below 1.0 mgKOH / g, the obtained product is a tackifying resin modified polyol for polyurethane adhesive.