MXene composite porous film as well as preparation method and application thereof

By using the combination technology of MXene with polymer conductive polymer and aqueous polymer in electromagnetic shielding materials, MXene composite porous films with low weight density, high flexibility and excellent electromagnetic shielding performance were prepared, and the existing electromagnetic shielding was solved. The problems of high weight density, poor flexibility and poor mechanical properties of the material.

CN118878918APending Publication Date: 2024-11-01NORTHWEST UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411108540.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The existing electromagnetic shielding materials are mainly electromagnetic reflection, and there are problems such as high weight density, poor flexibility and poor mechanical properties.

Method used

MXene, polymer conductive polymer and aqueous polymer are used to sonicate in N-methylpyrrolidone, polyarylether nitrile is added, and MXene composite porous film is prepared by solidifying bath and air-drying, forming a petal-like microporous structure, reducing Weight density and improve mechanical properties.

Benefits of technology

Low weight density, high flexibility and excellent electromagnetic shielding performance have been achieved, the electromagnetic absorption performance accounts for more than 90%, the tensile strength and elongation at break have been significantly improved, and the electrical conductivity and thermal conductivity have also reached a relatively high level.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118878918A_ABST
    Figure CN118878918A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of conductive porous material preparation, and relates to an MXene composite porous film and a preparation method and application thereof, the preparation method comprises the following steps: S1, dispersing MXene and a high-molecular conductive polymer into N-methyl pyrrolidone, and carrying out ultrasonic treatment; adding a water-based high-molecular polymer and bisphenol A type polyarylene ether nitrile, heating and stirring until the materials are completely dissolved to obtain a high-molecular conductive polymer / MXene / water-based high-molecular polymer / BPA-PEN mixed solution; pouring the mixed solution onto a glass surface plate, putting the glass surface plate into a coagulating bath to form a solid film, and soaking the solid film to obtain an MXene composite liquid film; and further draining water, and air-drying to obtain the MXene composite porous film. The MXene composite porous film disclosed by the invention is low in weight density, excellent in flexibility and mechanical property, relatively high in electromagnetic shielding capability and remarkable in electromagnetic absorption performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of conductive porous material preparation, and relates to a MXene composite porous film and a preparation method and application thereof. Background Art

[0002] With the high power and integration of electronic communication equipment, the electromagnetic radiation pollution problem is becoming increasingly serious, which has an adverse effect on human health and electronic equipment. In order to solve the problem of electromagnetic wave pollution, a lot of research has been conducted to develop efficient electromagnetic shielding materials. Metals and alloys are currently commonly used electromagnetic shielding materials, but they have disadvantages such as high weight density, poor flexibility, poor scratch resistance, and high processing costs. At the same time, the shielding effect of the above electromagnetic shielding materials is mainly electromagnetic reflection, which often causes secondary pollution of electromagnetic waves. In order to solve this problem, a new two-dimensional inorganic material MXene was selected as the substrate to prepare a MXene composite porous film, which overcomes the defects of traditional metal alloy materials and improves the performance of electromagnetic shielding materials.

[0003] Compared with other materials, MXene has significant advantages such as high conductivity, large specific surface area, and rich surface functional groups. These characteristics make it popular in the field of manufacturing electromagnetic shielding films. However, in practice, to achieve high-performance electromagnetic shielding effects, it is usually necessary to add a large amount of MXene, which leads to increased material costs. At the same time, a large amount of MXene will also produce negative effects such as mechanical property degradation, complex processing, and increased electromagnetic wave reflection on the material surface. The strategy of improving the electromagnetic shielding performance of MXene-based composites by designing multiple interfaces has been widely verified, including isolation, multiphase, interlayer and porous structure methods.

[0004] According to the existing electromagnetic shielding theory, the construction of porous structures is conducive to obtaining excellent electromagnetic shielding materials with strong impedance matching and high attenuation capabilities. The porous structure can promote matching with the air, which helps more electromagnetic waves enter the electromagnetic shielding material from the air. However, the flexibility of MXene nanosheets limits the stability of the porous film. Therefore, the rational design of the porous structure, obtaining more excellent electromagnetic shielding performance at a lower MXene material content, and preparing multi-interface MXene-based composite materials with electromagnetic wave absorption as the main focus of research. For example, the public document "Superiorelectromagnetic interference shielding 3D graphene nanoplatelets / reducedgraphene oxide foam / epoxy nanocomposites with high thermal conductivity" (Electromagnetic interference shielding 3D graphene nanoplatelets / reduced graphene oxide foam / epoxy nanocomposites with high thermal conductivity) uses freeze-drying technology to obtain a porous MXene skeleton, followed by epoxy resin infiltration. This method can effectively reduce the aggregation effect of MXene and promote its dispersion on the pore wall; in addition, there is also a porous conductive network constructed by bidirectional freezing technology. Although existing technologies can significantly enhance the electromagnetic shielding performance of materials, there are problems with complex manufacturing processes and difficult-to-control costs. In addition, the "Research Progress of Two-Dimensional Nanomaterials MXene" mentioned that due to the strong interaction between its nanosheets and its poor compatibility with polymers, MXene is very prone to agglomeration, which increases the amount of MXene required to build a porous conductive network, resulting in uneven pore size distribution and decreased mechanical properties.

[0005] In summary, existing electromagnetic shielding materials are mainly based on electromagnetic reflection, and have technical defects such as high weight density, poor flexibility and poor mechanical properties. Summary of the invention

[0006] In view of the technical problems that existing electromagnetic shielding materials are mainly electromagnetic reflection, high weight density, poor flexibility and poor mechanical properties, a MXene composite porous film and a preparation method and application thereof are provided.

[0007] The present invention disperses MXene and a high molecular conductive polymer in N-methylpyrrolidone, and ultrasonically treats the film; then adds an aqueous high molecular polymer and poly(arylether nitrile), and then solidifies the film in a coagulation bath, soaks the film, and air-dries the film to obtain a MXene composite porous film with low weight density, excellent flexibility, mechanical properties, high electromagnetic shielding capability, and significant electromagnetic absorption performance.

[0008] In order to achieve the above object, the technical solution adopted by the present invention is:

[0009] A method for preparing a MXene composite porous film comprises the following steps:

[0010] S1. Preparation of mixed solution of conductive polymer / MXene / waterborne polymer / BPA-PEN

[0011] MXene and high molecular conductive polymer are dispersed in N-methylpyrrolidone and ultrasonically treated; then water-based polymer and poly(arylether nitrile) are added and stirred until completely dissolved to obtain a mixed solution of high molecular conductive polymer / MXene / water-based polymer / BPA-PEN; the mass ratio of MXene, high molecular conductive polymer, N-methylpyrrolidone, water-based polymer and poly(arylether nitrile) is (6-18): 2:80:3:9

[0012] S2. Preparation of MXene composite liquid membrane

[0013] The mixed solution of high molecular conductive polymer / MXene / aqueous high molecular polymer / BPA-PEN in step S1 is poured onto a glass plate, placed in a coagulation bath to form a solid film, and soaked to obtain a MXene composite liquid film;

[0014] S3. Preparation of MXene composite porous film

[0015] The water in the MXene composite liquid membrane prepared in step S2 is drained and air-dried to obtain a MXene composite porous film.

[0016] It is further defined that in step S1, the ultrasonic treatment is performed for 80 min to 100 min, and the heating and stirring are continued for 70 min to 120 min.

[0017] It is further defined that the specific process of step S2 is:

[0018] A 1000 μm liquid film is scraped off from the glass plate, and then placed in a coagulation liquid. After the liquid film is converted into a solid film, it is peeled off from the glass plate and finally soaked for 20 h to 30 h to obtain a MXene composite liquid film; the coagulation liquid is an ethanol solution or water.

[0019] It is further defined that in step S3, the MXene composite liquid membrane is placed on a clean bench for 1 hour to 2 hours, the ethanol is drained, and then air-dried at room temperature to obtain a MXene composite porous film.

[0020] A MXene composite porous film prepared by the method for preparing a MXene composite porous film.

[0021] It is further defined that the MXene composite porous film has a petal-shaped microporous structure and a thickness of 0.2 mm.

[0022] It is further defined that the MXene composite porous film has a maximum tensile strength of 8.6 MPa and an elongation at break of 87.9%.

[0023] Such as the application of MXene composite porous films in enhancing electromagnetic shielding capabilities and / or electromagnetic absorption performance.

[0024] It is further defined that the MXene composite porous film has an electrical conductivity of up to 184.2 S / m, a maximum electromagnetic shielding performance of over 26.4 dB, a maximum electromagnetic absorption performance accounting for 91.6% of the total shielding performance, and a maximum thermal conductivity of 1.214 W / mK.

[0025] The beneficial effects of the present invention are:

[0026] 1. In the present invention, the MXene composite porous film has a large number of petal-shaped nano-microporous structures, which helps to promote the uniform dispersion of high molecular conductive polymers / water-based polymers in the MXene porous skeleton, and can effectively reduce the weight density of the system; at the same time, the introduction of the porous structure promotes the uniform dispersion of high molecular conductive polymers / water-based polymers on the MXene skeleton to form a continuous 3D conductive network structure, which helps to improve the electromagnetic shielding capability, and the electromagnetic absorption performance is significantly enhanced. In addition, the reduction of mechanical properties caused by MXene agglomeration is avoided, and the flexibility of the composite film is improved.

[0027] 2. In the present invention, the MXene composite porous film is prepared by a simple and environmentally friendly phase inversion processing technology; the size of the petal-shaped micropores is adjustable, and only a small amount of high molecular conductive polymer / water-based high molecular polymer is required to form a continuous conductive network structure.

[0028] 3. The present invention adjusts the performance of the material through MXene, with an electrical conductivity of up to 184.2S / m, an electromagnetic shielding performance of more than 26dB, an electromagnetic absorption performance accounting for more than 90% of the total shielding performance, and a thermal conductivity of up to 1.214W / mK.

[0029] 4. The MXene composite porous film of the present invention also has excellent mechanical properties, with a maximum tensile strength of 8.6 MPa and an elongation at break of 87.9%. In addition, it also exhibits excellent flexibility and stability, meeting the requirements of lightweight and high-performance electromagnetic shielding materials.

[0030] 5. The present invention disperses MXene and high molecular conductive polymer in N-methylpyrrolidone (NMP) by ultrasonic treatment, introduces water-based high molecular polymer and poly(arylether nitrile) (BPA-PEN) into the high molecular conductive polymer / MXene solution after ultrasonic treatment, heats and stirs to dissolve; then pours the solution onto a glass plate, puts it into a coagulation bath to form a solid film, and obtains a liquid film by immersion; finally, air-dries it to obtain a MXene composite porous film. The preparation method is simple and easy to operate, and can be widely applied to the mixing of various polymer matrices and various fillers, and is easy to realize industrialization. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 It is a schematic cross-sectional view of a MXene composite porous film;

[0032] Figure 2 is the conductivity diagram of MXene composite porous film; wherein: the MXene content in implementation examples 1 to 5 gradually increases from 6% to 18%, and all are ethanol baths, represented by F e-p ; In Example 6-Example 10, the MXene content gradually increased from 6% to 18%, and all were in a water bath, denoted as F w-p ;

[0033] Figure 3 It is the electromagnetic shielding performance diagram of MXene composite porous film; wherein: the MXene content in implementation examples 1 to 5 gradually increases from 6% to 18%, and all of them are ethanol baths, represented by F e-p ; In Example 6-Example 10, the MXene content gradually increased from 6% to 18%, and all were in a water bath, denoted as F w-p ;

[0034] Figure 4 It is a graph showing the ratio of electromagnetic absorption performance to reflection performance;

[0035] Figure 5 This is the effect of MXene content on thermal conductivity;

[0036] Figure 6 The effect of MXene content on tensile strength;

[0037] Figure 7 This is the effect of MXene content on elongation at break. DETAILED DESCRIPTION

[0038] The technical solution protected by the present invention is described in detail below with reference to the accompanying drawings. Although the drawings show specific embodiments of the present disclosure, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments described herein.

[0039] The present invention provides a method for preparing a MXene composite porous film, characterized by comprising the following steps:

[0040] S1. Preparation of mixed solution of conductive polymer / MXene / waterborne polymer / BPA-PEN

[0041] MXene and a high molecular conductive polymer are dispersed in N-methylpyrrolidone and ultrasonically treated; then an aqueous polymer and poly(arylether nitrile) are added and stirred until completely dissolved to obtain a mixed solution of a high molecular conductive polymer / MXene / aqueous polymer / BPA-PEN; the mass ratio of MXene, high molecular conductive polymer, N-methylpyrrolidone, aqueous polymer and poly(arylether nitrile) is (6-18):2:80:3:9.

[0042] In step S1 of the present invention, the ultrasonic treatment is performed for 80 to 100 minutes, and the stirring is performed for 70 to 120 minutes. In practice, the ultrasonic treatment is performed for 80 minutes, 85 minutes, 90 minutes, 95 minutes or 100 minutes, and the heating and stirring are performed for another 70 minutes, 80 minutes, 90 minutes, 100 minutes, 110 minutes or 120 minutes. Preferably, the ultrasonic treatment is performed for 90 minutes, and the stirring is performed for 90 minutes.

[0043] S2. Preparation of MXene composite liquid membrane

[0044] The mixed solution of high molecular conductive polymer / MXene / aqueous high molecular polymer / BPA-PEN in step S1 is poured onto a glass plate, placed in a coagulation bath to form a solid film, and then soaked to obtain a MXene composite liquid film.

[0045] The specific process of step S2 of the present invention is: scraping a 1000 μm liquid film on a glass plate with a wet film preparation device, then placing it in a coagulation liquid, peeling it off from the glass plate after the liquid film is converted into a solid film, and finally soaking it for 20h to 24h to obtain a MXene composite liquid film; the coagulation liquid is an ethanol solution.

[0046] S3. Preparation of MXene composite porous film

[0047] The water in the MXene composite liquid membrane prepared in step S2 is drained and air-dried to obtain a MXene composite porous film.

[0048] In step S3 of the present invention, the MXene composite liquid film is placed on a clean bench for 1 h to 2 h, the ethanol is drained, and then air-dried at room temperature to obtain a MXene composite porous film.

[0049] A MXene composite porous film prepared by the above-mentioned method for preparing a MXene composite porous film.

[0050] The technical advantages of the MXene composite porous film prepared by the present invention are described below through several groups of implementation methods and performance tests.

[0051] It should be noted that, unless otherwise specified, the reagents, drugs, instruments, etc. used in the following examples are all conventional products in the field purchased from the market.

[0052] Example 1

[0053] The method for preparing the MXene composite porous film provided in this embodiment comprises the following steps:

[0054] S1. Preparation of PAL / MXene / WPU / BPA-PEN mixed solution

[0055] 6g MXene and 2g polyaniline (PAL) were added to 80g N-methylpyrrolidone (NMP) and ultrasonicated for 90min to obtain a uniform MXene / PAL suspension. 3g waterborne polyurethane (WPU) and 9g polyarylether nitrile (BPA-PEN) were then added to the suspension and mechanically stirred at 300r / min for 90min until the mixture was completely dissolved to obtain a PAL / MXene / WPU / BPA-PEN mixed solution.

[0056] S2. Preparation of MXene composite liquid membrane

[0057] The PAL / MXene / WPU / BPA-PEN mixed solution obtained in step S1 was poured onto a glass plate, and a 1000 μm liquid film was scraped out with a wet film preparation device. Then 200 mL of ethanol was prepared, and then the glass plate and the liquid film on its surface were immersed in the ethanol solution together. After the liquid film was converted into a solid film, it was peeled off from the glass plate, and then continued to be immersed in ethanol for 24 hours to obtain a MXene composite liquid film.

[0058] S3. Preparation of MXene composite porous film

[0059] The MXene composite porous film prepared in step S2 is placed on a clean bench for 2 hours to drain the ethanol on its surface, and then the prepared porous film is air-dried at room temperature to obtain a MXene composite porous film.

[0060] Example 2

[0061] The method for preparing the MXene composite porous film provided in this embodiment comprises the following steps:

[0062] S1. Preparation of PAL / MXene / WPU / BPA-PEN mixed solution

[0063] 9g MXene and 3g polyaniline (PAL) were added to 76g N-methylpyrrolidone (NMP) and ultrasonicated for 90min to obtain a uniform MXene / PAL suspension. 3g waterborne polyurethane (WPU) and 9g polyarylether nitrile (BPA-PEN) were then added to the suspension and mechanically stirred at 300r / min for 90min until the mixture was completely dissolved to obtain a PAL / MXene / WPU / BPA-PEN mixed solution.

[0064] S2. Preparation of MXene composite liquid membrane

[0065] The process is consistent with that in Example 1.

[0066] S3. Preparation of MXene composite porous film

[0067] The process is consistent with that in Example 1.

[0068] Example 3

[0069] The method for preparing the MXene composite porous film provided in this embodiment comprises the following steps:

[0070] S1. Preparation of PAL / MXene / WPU / BPA-PEN mixed solution

[0071] 12g MXene and 4g polyaniline (PAL) were added to 72g N-methylpyrrolidone (NMP) and ultrasonicated for 90min to obtain a uniform MXene / PAL suspension. 3g waterborne polyurethane (WPU) and 9g polyarylether nitrile (BPA-PEN) were then added to the suspension and mechanically stirred at 300r / min for 90min until the mixture was completely dissolved to obtain a PAL / MXene / WPU / BPA-PEN mixed solution.

[0072] S2. Preparation of MXene composite liquid membrane

[0073] The process is consistent with that in Example 1.

[0074] S3. Preparation of MXene composite porous film

[0075] The process is consistent with that in Example 1.

[0076] Example 4

[0077] The method for preparing the MXene composite porous film provided in this embodiment comprises the following steps:

[0078] S1. Preparation of PAL / MXene / WPU / BPA-PEN mixed solution

[0079] 15g MXene and 5g polyaniline (PAL) were added to 68g N-methylpyrrolidone (NMP) and ultrasonicated for 90min to obtain a uniform MXene / PAL suspension. Then 3g waterborne polyurethane (WPU) and 9g polyarylether nitrile (BPA-PEN) were added to the suspension and mechanically stirred at 300r / min for 90min until the mixture was completely dissolved to obtain a PAL / MXene / WPU / BPA-PEN mixed solution.

[0080] S2. Preparation of MXene composite liquid membrane

[0081] The process is consistent with that in Example 1.

[0082] S3. Preparation of MXene composite porous film

[0083] The process is consistent with that in Example 1.

[0084] Example 5

[0085] The method for preparing the MXene composite porous film provided in this embodiment comprises the following steps:

[0086] S1. Preparation of PAL / MXene / WPU / BPA-PEN mixed solution

[0087] 18g MXene and 6g polyaniline (PAL) were added to 64g N-methylpyrrolidone (NMP) and ultrasonicated for 90min to obtain a uniform MXene / PAL suspension. 3g waterborne polyurethane (WPU) and 9g poly(arylether nitrile) (BPA-PEN) were then added to the suspension and mechanically stirred at 300r / min for 90min until the mixture was completely dissolved to obtain a PAL / MXene / WPU / BPA-PEN mixed solution.

[0088] S2. Preparation of MXene composite liquid membrane

[0089] The process is consistent with that in Example 1.

[0090] S3. Preparation of MXene composite porous film

[0091] The process is consistent with that in Example 1.

[0092] Example 6

[0093] The method for preparing the MXene composite porous film provided in this embodiment comprises the following steps:

[0094] S1. Preparation of PAL / MXene / WPU / BPA-PEN mixed solution

[0095] 6g MXene and 2g polyaniline (PAL) were added to 80g N-methylpyrrolidone (NMP) and ultrasonicated for 90min to obtain a uniform MXene / PAL suspension. 3g waterborne polyurethane (WPU) and 9g polyarylether nitrile (BPA-PEN) were then added to the suspension and mechanically stirred at 300r / min for 90min until the mixture was completely dissolved to obtain a PAL / MXene / WPU / BPA-PEN mixed solution.

[0096] S2. Preparation of MXene composite liquid membrane

[0097] The PAL / MXene / WPU / BPA-PEN mixed solution obtained in step S1 was poured onto a glass plate, and a 1000 μm liquid film was scraped out using a wet film preparation device. Then 200 mL of ethanol was prepared, and the glass plate and the liquid film on its surface were immersed in the ethanol solution together. After the liquid film was converted into a solid film, it was peeled off from the glass plate, and then continued to be immersed in deionized water for 24 hours to obtain a lightweight MXene composite liquid film.

[0098] S3. Preparation of MXene composite porous film

[0099] The lightweight MXene composite porous film prepared in step S2 is placed on an ultra-clean workbench for 2 hours to drain the water on its surface, and then the prepared porous film is air-dried at room temperature to obtain a lightweight and high-performance MXene composite porous film.

[0100] Example 7

[0101] The method for preparing the MXene composite porous film provided in this embodiment comprises the following steps:

[0102] S1. Preparation of PAL / MXene / WPU / BPA-PEN mixed solution

[0103] 9g MXene and 3g polyaniline (PAL) were added to 76g N-methylpyrrolidone (NMP) and ultrasonicated for 90min to obtain a uniform MXene / PAL suspension. 3g waterborne polyurethane (WPU) and 9g poly(arylether nitrile) (BPA-PEN) were then added to the suspension and mechanically stirred at 300r / min for 90min until the mixture was completely dissolved to obtain a PAL / MXene / WPU / BPA-PEN mixed solution.

[0104] S2. Preparation of MXene composite liquid membrane

[0105] The same process as in Example 6.

[0106] S3. Preparation of MXene composite porous film

[0107] The same process as in Example 6.

[0108] Example 8

[0109] The method for preparing the MXene composite porous film provided in this embodiment comprises the following steps:

[0110] S1. Preparation of PAL / MXene / WPU / BPA-PEN mixed solution

[0111] 12g MXene and 4g polyaniline (PAL) were added to 72g N-methylpyrrolidone (NMP) and ultrasonicated for 90min to obtain a uniform MXene / PAL suspension. 3g waterborne polyurethane (WPU) and 9g polyarylether nitrile (BPA-PEN) were then added to the suspension and mechanically stirred at 300r / min for 90min until the mixture was completely dissolved to obtain a PAL / MXene / WPU / BPA-PEN mixed solution.

[0112] S2. Preparation of MXene composite liquid membrane

[0113] The same process as in Example 6.

[0114] S3. Preparation of MXene composite porous film:

[0115] The same process as in Example 6.

[0116] Example 9

[0117] The method for preparing the MXene composite porous film provided in this embodiment comprises the following steps:

[0118] S1. Preparation of PAL / MXene / WPU / BPA-PEN mixed solution

[0119] 15g MXene and 5g polyaniline (PAL) were added to 68g N-methylpyrrolidone (NMP) and ultrasonicated for 90min to obtain a uniform MXene / PAL suspension. 3g waterborne polyurethane (WPU) and 9g polyarylether nitrile (BPA-PEN) were then added to the suspension and mechanically stirred at 300r / min for 90min until the mixture was completely dissolved to obtain a PAL / MXene / WPU / BPA-PEN mixed solution.

[0120] S2. Preparation of MXene composite liquid membrane

[0121] The same process as in Example 6.

[0122] S3. Preparation of MXene composite porous film

[0123] The same process as in Example 6.

[0124] Example 10

[0125] The method for preparing the MXene composite porous film provided in this embodiment comprises the following steps:

[0126] S1. Preparation of PAL / MXene / WPU / BPA-PEN mixed solution

[0127] 18g MXene and 6g polyaniline (PAL) were added to 64g N-methylpyrrolidone (NMP) and ultrasonicated for 90min to obtain a uniform MXene / PAL suspension. 3g waterborne polyurethane (WPU) and 9g polyarylether nitrile (BPA-PEN) were then added to the suspension and mechanically stirred at 300r / min for 90min until the mixture was completely dissolved to obtain a PAL / MXene / WPU / BPA-PEN mixed solution.

[0128] S2. Preparation of MXene composite liquid membrane

[0129] The same process as in Example 6.

[0130] S3. Preparation of MXene composite porous film

[0131] The same process as in Example 6.

[0132] The performance of the MXene composite porous film prepared in the above example was verified by the following experiments.

[0133] Test 1

[0134] Test sample: MXene composite porous film prepared in Example 1 and Example 6.

[0135] Test process: test film thickness; and film cross-section SEM microstructure, see Figure 1 shown.

[0136] Through testing, it was found that the thickness of the MXene composite porous film was 0.2 mm.

[0137] Figure 1 In the SEM microstructure diagram, A is the cross-sectional structure of the MXene composite porous film prepared in Example 1. It can be seen from the figure that the overall cross-sectional structure of the film is composed of honeycomb pores with an average size of 32 μm, and the WPU and PAL attached to the surface are uniformly dispersed in the MXene porous skeleton; B is the cross-sectional structure of the MXene composite porous film prepared in Example 6. It can be seen that the film has a three-dimensional cross-linked skeleton structure, and the WPU and PAL attached to the surface are uniformly dispersed in the MXene porous skeleton.

[0138] Test 2

[0139] Test sample: MXene composite porous film prepared in Examples 1 to 10.

[0140] Test method: The conductivity of each group of MXene composite porous films was measured using the conventional method of existing film conductivity. The test results are as follows Figure 2 As shown in Table 1, Figure 2 In Example 1 to Example 5, the mass fraction of MXene is 6%, 9%, 12%, 15% and 18% respectively, and all of them are ethanol baths, denoted as F e-p In Examples 6 to 10, the mass fractions of MXene are 6%, 9%, 12%, 15% and 18% respectively, and all of them are in a water bath, denoted as F w-p .

[0141] Table 1 Electrical conductivity of each group of MXene composite porous films

[0142]

[0143]

[0144] from Figure 2 As can be seen from Table 1, as the mass fraction of MXene increases, the electrical conductivity increases; at the same time, the electrical conductivity of the MXene composite porous film obtained in an ethanol bath is better than that of the MXene composite porous film obtained in a water bath.

[0145] Test 3

[0146] Test sample: MXene composite porous film prepared in Example 1 to Example 10, and the electromagnetic shielding performance of the composite film was tested.

[0147] Electromagnetic shielding test method: Use the network analyzer PNA network analyzer N5224B to measure the EMI shielding performance of a sample with a diameter of 12 mm. The measurement frequency range is 8.2 to 12.4 GHz (X band). Calculate the total electromagnetic shielding effectiveness SET. For details, see Figure 3 , Figure 4 and Table 2.

[0148] Figure 3 and Figure 4 In Example 1 to Example 5, the mass fraction of MXene is 6%, 9%, 12%, 15% and 18% respectively, and all of them are ethanol baths, denoted as F e-p In Examples 6 to 10, the mass fractions of MXene are 6%, 9%, 12%, 15% and 18% respectively, and all of them are in a water bath, denoted as F w-p .

[0149] Table 2 Electromagnetic shielding properties of each group of MXene composite porous films

[0150]

[0151]

[0152] from Figure 3 , Figure 4 As can be seen from Table 2: as the mass fraction of MXene increases, the electromagnetic shielding performance is enhanced, but the proportion of electromagnetic absorption performance in the total shielding performance decreases; at the same time, the electromagnetic properties of the MXene composite porous film obtained in an ethanol bath are better than those of the MXene composite porous film obtained in a water bath.

[0153] Test 4

[0154] Test sample: MXene composite porous film prepared in Examples 1 to 10.

[0155] Test method: The existing conventional methods were used to test the mechanical properties of each group of MXene composite porous films, such as tensile strength, elongation at break and thermal conductivity. The test results are shown in Table 3. Figure 5 , Figure 6 and Figure 7 shown.

[0156] Figure 5 , Figure 6 and Figure 7 In Example 1 to Example 5, the mass fraction of MXene is 6%, 9%, 12%, 15% and 18% respectively, and all of them are ethanol baths, denoted as F e-p In Examples 6 to 10, the mass fractions of MXene are 6%, 9%, 12%, 15% and 18% respectively, and all of them are in a water bath, denoted as F w-p .

[0157] Table 3 Mechanical properties of each group of MXene composite porous films

[0158]

[0159]

[0160] It can be seen from Table 3 that as the mass fraction of MXene increases, the tensile strength and elongation at break decrease, and the thermal conductivity increases; at the same time, the mechanical properties of the MXene composite porous film obtained in an ethanol bath are better than those of the MXene composite porous film obtained in a water bath.

[0161] In order to verify the performance superiority of the MXene composite porous film of the present invention, the following comparative test was carried out.

[0162] Comparative Example 1

[0163] In this comparative example, polyaniline (PAL) was not added, and the rest was referred to Example 4. The mass fraction of MXene was 15%, and the coagulation bath was an ethanol bath.

[0164] This comparative example provides a MXene composite porous film, and its preparation method is as follows:

[0165] S1. Add 15 g MXene into 73 g N-methylpyrrolidone (NMP) and ultrasonicate for 90 min to obtain a uniform MXene suspension.

[0166] S2, add 3g of waterborne polyurethane (WPU) and 9g of poly(arylether nitrile) (BPA-PEN) to the MXene suspension, and stir mechanically at 300r / min for 90min until the mixture is completely dissolved to obtain a MXene / WPU / BPA-PEN mixed solution. The subsequent film preparation method is the same as that in Example 4.

[0167] After testing, the obtained MXene composite porous film had an electrical conductivity of 113.5S / m, an electromagnetic shielding performance of 16.2dB, an electromagnetic absorption performance accounting for 86.3% of the total shielding performance, a tensile strength of 6.2MPa, an elongation at break of 66.3%, and a thermal conductivity of 1.072W / m*K.

[0168] Comparative Example 2

[0169] In this comparative example, waterborne polyurethane (WPU) was not added; the rest was referred to Example 4, the mass fraction of MXene was 15%, and the coagulation bath was an ethanol bath.

[0170] This comparative example provides a MXene composite porous film, and its preparation method is as follows:

[0171] S1. Add 15 g MXene and 5 g PAL into 71 g N-methylpyrrolidone (NMP) and ultrasonicate for 90 min to obtain a uniform MXene / PAL suspension.

[0172] S2, 9 g of polyarylether nitrile (BPA-PEN) was added to the MXene / PAL suspension, and mechanically stirred at 300 r / min for 90 min until it was completely dissolved to obtain a PAL / MXene / BPA-PEN mixed solution. The subsequent film preparation method was the same as that in Example 4.

[0173] After testing, the electrical conductivity of the obtained MXene composite porous film was 92.3S / m, the electromagnetic shielding performance was 14.1dB, the electromagnetic absorption performance accounted for 82.7% of the total shielding performance, the tensile strength was 5.9MPa, the elongation at break was 64.6%, and the thermal conductivity was 1.028W / m*K.

[0174] Through the above comparison, the present invention disperses MXene and polyaniline in N-methylpyrrolidone and performs ultrasonic treatment; then adds water-based polyurethane and polyarylethernitrile, and then obtains the MXene composite porous film through coagulation in a coagulation bath, immersion and air drying. The synergistic effect of several raw materials can greatly improve the mechanical properties, electromagnetic shielding capability and electromagnetic absorption performance of the porous film.

[0175] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the scope of protection of the invention.

Claims

1. A method for preparing a MXene composite porous film, characterized in that: The following steps are involved: S1. Preparation of polymer conductive polymer / MXene / waterborne polymer / BPA-PEN mixed solution: MXene and polymer conductive polymer are dispersed in N-methylpyrrolidone and subjected to ultrasonic treatment; then, waterborne polymer and poly(arylether nitrile) are added and stirred until completely dissolved to obtain a polymer conductive polymer / MXene / waterborne polymer / BPA-PEN mixed solution; the mass ratio of MXene, polymer conductive polymer, N-methylpyrrolidone, waterborne polymer and poly(arylether nitrile) is (6-18): 2: 80: 3: 9; S2. Preparation of MXene composite liquid membrane The mixed solution of high molecular conductive polymer / MXene / aqueous high molecular polymer / BPA-PEN in step S1 is poured onto a glass plate, placed in a coagulation bath to form a solid film, and soaked to obtain a MXene composite liquid film; S3. Preparation of MXene composite porous film The water in the MXene composite liquid membrane prepared in step S2 is drained and air-dried to obtain a MXene composite porous film.

2. The method for preparing the MXene composite porous film according to claim 1, characterized in that: In the step S1, the ultrasonic treatment is performed for 80 min to 100 min, and the stirring is performed for 70 min to 120 min.

3. The method for preparing the MXene composite porous film according to claim 1, characterized in that: The specific process of step S2 is: A 1000 μm liquid film is scraped off from the glass plate, and then placed in a coagulation liquid. After the liquid film is converted into a solid film, it is peeled off from the glass plate and finally soaked for 20 h to 30 h to obtain a MXene composite liquid film; the coagulation liquid is an ethanol solution or water.

4. The method for preparing the MXene composite porous film according to claim 1, characterized in that: In the step S3, the MXene composite liquid film is placed on a clean bench for 1 h to 2 h, the ethanol is drained, and then air-dried at room temperature to obtain a MXene composite porous film.

5. A MXene composite porous film prepared by the method for preparing a MXene composite porous film according to any one of claims 1 to 4.

6. The MXene composite porous film according to claim 5, characterized in that: The MXene composite porous film has a petal-shaped microporous structure and a thickness of 0.2 mm.

7. The MXene composite porous film according to claim 5, characterized in that: The MXene composite porous film has a maximum tensile strength of 8.6 MPa and an elongation at break of 87.9%.

8. Use of the MXene composite porous film as claimed in claim 5 in enhancing electromagnetic shielding capability and / or electromagnetic absorption performance.

9. The use according to claim 8, characterized in that: The MXene composite porous film has an electrical conductivity of up to 184.2 S / m, an electromagnetic shielding performance of more than 26.4 dB at most, an electromagnetic absorption performance that accounts for 91.6% of the total shielding performance, and a thermal conductivity of up to 1.214 W / mK.

Citation Information

Cited By

  • P-MXene conductive ink and BC reinforced polymer composite film as well as preparation method and application thereof

    CN119613818A

  • MXenePANi-based electrical response microwave reflectivity adjustable device and preparation method and application thereof

    CN121038259A