Wear-resistant and wet-skid-resistant tire rubber composition and screening method thereof

By selecting specific micro-composition polystyrene butadiene rubber and butadiene rubber with rubber and establishing a relational screening formula, the problem of difficult to take into account both wear resistance and slip resistance in new energy electric vehicle tires. Improve development efficiency and reduce costs.

CN118878951APending Publication Date: 2024-11-01QINGDAO DOUBLESTAR TIRE IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411179441.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The prior art is difficult to take into account both wear resistance and slip resistance in new energy electric vehicle tires, resulting in low development efficiency and high cost.

Method used

By selecting polystyrene butadiene rubber and butadiene rubber of specific microscopic composition and content, the relationship between the anti-slip performance parameters and the wear resistance parameters is established, and tire rubber compositions that meet both wear resistance and anti-slip performance are selected. formula.

Benefits of technology

The wear resistance and slip resistance of the tire rubber composition are achieved, shortening the development cycle and reducing workload and cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005011667680000061
    Figure BDA0005011667680000061
  • Figure BDA0005011667680000101
    Figure BDA0005011667680000101
Patent Text Reader

Abstract

The invention provides a wear-resistant and wet-skid-resistant tire rubber composition and a screening method thereof, and belongs to the technical field of rubber compositions. The wear-resistant and wet-skid-resistant tire rubber composition comprises solution polymerized styrene-butadiene rubber and butadiene rubber, and the difference between the wet-skid-resistant performance parameter and the wear-resistant performance parameter of the wear-resistant and wet-skid-resistant tire rubber composition meets the following relational expression: 0.67 * WB * (1.4 * StS + 0.85 * ViS) * 2.72 * StS-0. 69 * ViS > 0.09, in the formula, WB represents the mass percentage of butadiene rubber in a blended rubber raw rubber system, and ViS represents the mass percentage of butadiene rubber in a blended rubber raw rubber system. StS represents the mass percent of styryl in the molecular chain of the solution polymerized styrene-butadiene rubber, and ViS represents the mass percent of vinyl in the molecular chain of the solution polymerized styrene-butadiene rubber. By selecting the solution polymerized styrene-butadiene rubber and butadiene rubber combined rubber with specific microcosmic composition and content, the tire tread rubber composition has wear resistance and wet skid resistance, the development cycle of the product is shortened, the workload is reduced, and the cost is saved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of rubber compositions, and in particular relates to a wear-resistant and anti-slip tire rubber composition and a screening method thereof. Background Art

[0002] Tire wear resistance and wet-skid resistance are crucial properties, closely linked to tire life and driving safety. With the implementation of the dual-carbon policy, new energy electric vehicles have experienced rapid growth. However, due to lagging battery technology, the weight and bulk of batteries increase tire wear during driving. Tire wear also produces a high level of ultrafine particulate matter, which is detrimental to ecological protection. Furthermore, the high motor output makes tires prone to slipping. Therefore, new energy electric vehicles place higher demands on tire wear resistance and wet-skid resistance.

[0003] Solution-polymerized styrene-butadiene rubber (SBR) and cis-1,4-butadiene rubber (CIBR) are commonly used in tire tread rubber compositions. CIBR has a low glass transition temperature, good molecular chain flexibility, and excellent wear resistance, but poor wet skid resistance. Solution-polymerized styrene-butadiene rubber (SBR) has a high glass transition temperature and good wet skid resistance, but poor wear resistance. With hundreds of SBR grades available, selecting the appropriate SBR and CIBR combination to achieve a tire rubber composition that balances wear resistance and wet skid resistance remains a challenge in the industry. Moreover, currently, developing a tire rubber composition formula that balances wear resistance and wet skid resistance can only be done by mixing and testing all the options one by one according to the formula. The specific implementation method is as follows: select different rubbers and proportions for test verification, conduct internal mixing for all the options, open milling for sheeting, prepare samples, and use a flat plate vulcanizer for vulcanization. All samples are tested for wear resistance and dynamic mechanical properties using a DIN abrasion tester and a dynamic thermomechanical analyzer, respectively. Options that do not meet the target wear resistance and wet skid resistance are discarded. If no suitable option is selected, all options are discarded and the next round of option design and verification is carried out until a suitable option is selected. This testing method requires a large amount of manpower, material, and financial resources to implement, and the workload is heavy, seriously affecting development efficiency and resulting in a huge waste of labor, materials, and testing costs.

[0004] Therefore, a wear-resistant and anti-skid tire rubber composition and a screening method thereof are of great significance to those skilled in the art. Summary of the Invention

[0005] The present invention addresses the technical problem in the prior art of how to select a suitable solution-polymerized styrene-butadiene rubber and cis-1,4-butadiene rubber combination to obtain a tire rubber composition that has both wear resistance and wet-skid resistance. The present invention proposes a wear-resistant and wet-skid-resistant tire rubber composition and a screening method thereof. By selecting solution-polymerized styrene-butadiene rubber and cis-1,4-butadiene rubber with specific microscopic compositions and contents and using them together, the tire tread rubber composition has both wear resistance and wet-skid resistance, which is conducive to shortening the product development cycle, reducing workload, and saving costs.

[0006] In order to achieve the above object, the technical solution adopted by the present invention is: a wear-resistant and anti-wet-skid tire rubber composition, comprising solution-polymerized styrene-butadiene rubber and butadiene rubber, wherein the difference between the anti-wet-skid performance parameter and the wear resistance performance parameter of the wear-resistant and anti-wet-skid tire rubber composition satisfies the following relationship:

[0007] 0.67×W B ×(1.4×St S +0.85×Vi S )×|2.72×St S -0.69×Vi S |>0.09,

[0008] In the above relationship, W B St represents the mass percentage of butadiene rubber in the blended rubber system. S Indicates the mass percentage of styrene groups in the molecular chain of solution-polymerized styrene-butadiene rubber, Vi S It indicates the mass percentage of vinyl groups in the solution-polymerized styrene-butadiene rubber molecular chain.

[0009] In some embodiments, the anti-skid performance parameter is greater than 0.53, wherein the anti-skid performance parameter y=(1.4×St S +0.85×Vi S )×(W S +0.67×W B ×|2.72×St S -0.69×Vi S |), where W S It represents the mass percentage of SBR in the blended rubber system. As the mass percentage of SBR in the blended rubber system increases, as does the mass percentage of styrene and vinyl groups in the SBR molecular chain, as well as as the compatibility between SBR and cis-1,1-butadiene rubber decreases and as the glass transition temperature of the blended rubber increases, wet skid resistance improves.

[0010] In some embodiments, the wear resistance parameter x=(1.4×St S +0.85×Vi S )×W SAs the mass percentage of SBR in the blended rubber system and the mass percentage of styrene and vinyl groups in the SBR molecular chain decrease, the flexibility and wear resistance of the rubber molecular chain improve.

[0011] In some embodiments, the mass percentage of butadiene rubber in the blended rubber system is 30% to 40%.

[0012] In some embodiments, the butadiene rubber is a high-cis butadiene rubber, wherein the cis 1,4 structure content thereof is greater than 96%.

[0013] In some embodiments, the mass percentage of styrene groups in the solution-polymerized styrene-butadiene rubber molecular chain is 28%-45%.

[0014] The present invention also provides a method for screening the above-mentioned wear-resistant and anti-slip tire rubber composition, which specifically comprises the following steps:

[0015] The microstructure of the solution-polymerized styrene-butadiene rubber was characterized by nuclear magnetic resonance spectroscopy, and the mass percentage of styrene groups in the solution-polymerized styrene-butadiene rubber molecular chain, St, was obtained. S and the mass percentage of vinyl Vi S ;

[0016] Based on the mass percentage of styrene groups in the molecular chain of solution-polymerized styrene-butadiene rubber (St) S and the mass percentage of vinyl Vi S , and solution polymerized styrene-butadiene rubber W in the rubber system S The mass percentage of butadiene rubber W B , establish a relationship between the difference between the wear resistance performance parameter and the anti-skid performance parameter, and screen the wear-resistant and anti-skid tire rubber composition according to the size of the difference.

[0017] In some embodiments, before establishing the relationship between the wear resistance parameter and the anti-skid performance parameter, the step of establishing the wear resistance parameter and the anti-skid performance parameter is also included, wherein:

[0018] Wear resistance parameter x=(1.4×St S +0.85×Vi S )×W S ,

[0019] Anti-wet skid performance parameter y=(1.4×St S +0.85×Vi S )×(W S +0.67×W B ×|2.72×St S -0.69×Vi S |).

[0020] In some embodiments, a smaller x value indicates better wear resistance, and a larger y value indicates better wet skid resistance.

[0021] In some embodiments, if the difference between the anti-wet skid performance parameter and the wear resistance performance parameter is less than 0.09, it means that the wear resistance and anti-wet skid performance of the tire rubber composition cannot meet the requirements at the same time; if the difference between the anti-wet skid performance parameter and the wear resistance performance parameter is greater than 0.09, it means that the wear resistance and anti-wet skid performance of the tire rubber composition can be taken into account.

[0022] Compared with the prior art, the advantages and positive effects of the present invention are: the wear-resistant and anti-slip tire rubber composition of the present invention can take into account both wear resistance and anti-slip performance; the screening method of the wear-resistant and anti-slip tire tread rubber of the present invention is simple to operate, and by selecting solution-polymerized styrene-butadiene rubber and butadiene rubber with specific microscopic compositions and contents and using them together, the tire tread rubber composition can take into account both wear resistance and anti-slip performance, which is conducive to shortening the product development cycle, reducing workload, and saving costs. DETAILED DESCRIPTION

[0023] The following is a clear and complete description of the technical solutions in the embodiments of the present invention. Obviously, the embodiments described are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making any creative efforts are within the scope of protection of the present invention.

[0024] An embodiment of the present invention provides a wear-resistant and anti-wet-skid tire rubber composition and a screening method thereof. The provided tire rubber composition has both wear resistance and anti-wet-skid performance. The screening method of the wear-resistant and anti-wet-skid tire rubber composition of the present invention selects a solution-polymerized styrene-butadiene rubber and butadiene rubber with a specific microscopic composition and content, so that the tire tread rubber composition has both wear resistance and anti-wet-skid performance. The operation is simple, which is conducive to shortening the product development cycle, reducing workload, and saving costs.

[0025] The wear-resistant and anti-wet-skid tire rubber composition provided in an embodiment of the present invention has a raw rubber system composed of solution-polymerized styrene-butadiene rubber and butadiene rubber, wherein the difference between the anti-wet-skid performance parameter and the wear-resistant performance parameter of the wear-resistant and anti-wet-skid tire rubber composition satisfies the following relationship: 0.67×W B ×(1.4×St S +0.85×Vi S )×|2.72×St S -0.69×Vi S |>0.09, in the above relationship, W B St represents the mass percentage of butadiene rubber in the blended rubber system. SIndicates the mass percentage of styrene groups in the molecular chain of solution-polymerized styrene-butadiene rubber, Vi S It indicates the mass percentage of vinyl groups in the solution-polymerized styrene-butadiene rubber molecular chain.

[0026] In a preferred embodiment, the anti-skid performance parameter y=(1.4×St S +0.85×Vi S )×(W S +0.67×W B ×|2.72×St S -0.69×Vi S |), where W S Indicates the mass percentage of solution-polymerized styrene-butadiene rubber in the rubber-based system; wear resistance parameter x = (1.4 × St S +0.85×Vi S )×W S . The anti-wet skid performance parameters and wear resistance performance parameters of the present invention are established by characterizing the styrene content and vinyl content in the solution-polymerized styrene-butadiene rubber molecular chain and the solution-polymerized styrene-butadiene rubber content and the cis-1,4-butadiene rubber content in the blended rubber system. A large y value indicates good anti-wet skid performance. Preferably, y>0.53; a small x value indicates good wear resistance. As the mass percentage of the solution-polymerized styrene-butadiene rubber in the blended rubber system, the mass percentage of styrene groups and vinyl groups in the solution-polymerized styrene-butadiene rubber molecular chain increase, and the compatibility between the solution-polymerized styrene-butadiene rubber and the cis-1,4-butadiene rubber decreases, and the glass transition temperature of the blended rubber increases, the anti-wet skid performance improves; as the mass percentage of the solution-polymerized styrene-butadiene rubber in the blended rubber system, the mass percentage of styrene groups and vinyl groups in the solution-polymerized styrene-butadiene rubber molecular chain decreases, the flexibility and wear resistance of the rubber molecular chain improve.

[0027] In the wear-resistant and anti-slip tire rubber composition provided by the embodiments of the present invention, the mass percentage of cis-1,4-butadiene rubber in the blended rubber system is 30% to 40%. The cis-1,4-butadiene rubber is high-cis-1,4-butadiene rubber, with a cis-1,4-butadiene structure content of at least 96%. Cis-1,4-butadiene rubber has a low glass transition temperature, good molecular chain flexibility, and excellent wear resistance. By limiting the amount and structure of the cis-1,4-butadiene rubber, the present invention can improve the wear resistance of the tire rubber composition.

[0028] In the wear-resistant and anti-wet-skid tire rubber composition provided by an embodiment of the present invention, the solution-polymerized styrene-butadiene rubber is a medium-styrene-structured solution-polymerized styrene-butadiene rubber or a high-styrene-structured solution-polymerized styrene-butadiene rubber, and the mass percentage of styrene groups in the solution-polymerized styrene-butadiene rubber molecular chain is 28%-45%; the medium-high styrene-structured solution-polymerized styrene-butadiene rubber has a high glass transition temperature and good anti-wet-skid performance, which can improve the anti-wet-skid performance of the tire rubber composition.

[0029] The method for screening a wear-resistant and anti-slip tire rubber composition provided in an embodiment of the present invention specifically comprises the following steps:

[0030] The microstructure of the solution polymerized styrene butadiene rubber was characterized by nuclear magnetic resonance spectroscopy, and the mass percentage of styrene groups in the solution polymerized styrene butadiene rubber molecular chain was obtained. S The mass percentage of vinyl in the solution polymerized styrene-butadiene rubber molecular chain Vi S ;

[0031] Based on the mass percentage St of the styrene group in the solution polymerized styrene-butadiene rubber molecular chain obtained by characterization S and the mass percentage of vinyl Vi S , and the mass percentage W of solution polymerized styrene-butadiene rubber in the rubber system S , mass percentage of butadiene rubber W B , first establish the wear resistance parameter x=(1.4×St S +0.85×Vi S )×W S And the anti-skid performance parameter y=(1.4×St S +0.85×Vi S )×(W S +0.67×W B ×|2.72×St S -0.69×Vi S |), a small x value indicates that the rubber composition has good wear resistance, and a large y value indicates that the rubber composition has good wet skid resistance;

[0032] Then according to the difference between the anti-wet skid performance parameter and the wear resistance performance parameter a=0.67×W B ×(1.4×St S +0.85×Vi S )×|2.72×St S -0.69×Vi S |'s size is used to screen wear-resistant and wet-skid-resistant tire rubber compositions; when the difference a between the wet-skid-resistant performance-related parameter and the wear-resistant performance-related parameter is less than 0.09, the wear resistance and wet-skid-resistant performance of the obtained tire rubber composition cannot meet the requirements at the same time; when the difference a between the wet-skid-resistant performance-related parameter and the wear-resistant performance-related parameter is greater than 0.09, the wear resistance and wet-skid-resistant performance of the tire rubber composition can be taken into account.

[0033] In order to more clearly and in detail introduce the wear-resistant and anti-slip tire rubber composition and the screening method thereof provided by the embodiments of the present invention, they will be described below in conjunction with specific embodiments.

[0034] The formulations of the tire rubber compositions of Examples 1-5 of the present invention and Comparative Examples 1-5 are shown in Table 1.

[0035] Table 1: Formula and microstructure of tire rubber compositions of Examples 1-5 and Comparative Examples 1-5

[0036]

[0037] Note: The number of raw rubber parts is calculated based on dry rubber

[0038] Example 1

[0039] Raw material formula: 30 parts of cis-1,4-butadiene rubber; 70 parts of solution-polymerized styrene-butadiene rubber, wherein the mass percentage of styrene groups in the solution-polymerized styrene-butadiene rubber molecular chain is 36% and the mass percentage of vinyl groups is 26%;

[0040] The filler is 80 parts of SiO2; the plasticizer is 37.5 parts; the activator is 5 parts; the antioxidant is 3 parts; the silane coupling agent is 12.8 parts of solid Si69; the vulcanizing agent is 1.5 parts; and the accelerator is 4 parts.

[0041] The tire rubber composition of this embodiment is mixed and vulcanized according to the following steps:

[0042] S1. Add cis-1,4-butadiene rubber, solution-polymerized styrene-butadiene rubber, activator, antioxidant, SiO2 and silane coupling agent into an internal mixer, press and mix for 40 seconds or at 115°C, with the mixer speed at 90 rpm.

[0043] S2, lift the bolt to clean, press the bolt and mix for 40 seconds or to 135℃, with the internal mixer speed at 90rpm;

[0044] S3, after lifting the bolt, press the bolt and mix for 30 seconds or to 145 ° C, with the internal mixer speed at 90 rpm;

[0045] S4, after lifting the plug, press the plug, mix at a constant temperature of 145℃ for 180s, remove the rubber and cool it to obtain the masterbatch;

[0046] S5. Lift the plug and add the masterbatch, vulcanizing agent and accelerator, press the plug and mix for 30 seconds or until the temperature reaches 85°C, with the internal mixer speed at 60 rpm;

[0047] S6, after lifting the bolt, press the bolt and mix to 100℃, with the internal mixer speed at 60rpm;

[0048] S7, after lifting the plug, press the plug and mix for 30 seconds or until the temperature reaches 110°C, remove the rubber and cool it to obtain the final rubber mix;

[0049] S8. Vulcanize the final rubber mix on a flat vulcanizer at 161° C. under a pressure of 12 MPa for 20 min to obtain a tire rubber composition.

[0050] Example 2

[0051] Compared with Example 1, the content of styrene groups and vinyl groups in the solution polymerized styrene-butadiene rubber molecular chain in the tire rubber composition of this embodiment is different. The raw material formula of this embodiment is: 30 parts of cis-1,4-butadiene rubber; 70 parts of solution polymerized styrene-butadiene rubber, and the mass percentage of styrene groups in the solution polymerized styrene-butadiene rubber molecular chain is 40%, and the mass percentage of vinyl groups is 14%.

[0052] The filler is 80 parts of SiO2; the plasticizer is 37.5 parts; the activator is 5 parts; the antioxidant is 3 parts; the silane coupling agent is 12.8 parts of solid Si69; the vulcanizing agent is 1.5 parts; and the accelerator is 4 parts.

[0053] The mixing and vulcanization methods of the tire rubber composition of this embodiment are the same as those of Example 1.

[0054] Example 3

[0055] Compared with Example 1, the amounts of solution-polymerized styrene-butadiene rubber and cis-1,4-butadiene rubber in the raw material and rubber system of the tire rubber composition of this embodiment are different, and the contents of styrene groups and vinyl groups in the molecular chain of the solution-polymerized styrene-butadiene rubber are different. The raw material formula of this embodiment is: 40 parts of cis-1,4-butadiene rubber; 60 parts of solution-polymerized styrene-butadiene rubber, and the mass percentage of styrene groups in the molecular chain of the solution-polymerized styrene-butadiene rubber is 28%, and the mass percentage of vinyl groups is 42%.

[0056] The filler is 80 parts of SiO2; the plasticizer is 37.5 parts; the activator is 5 parts; the antioxidant is 3 parts; the silane coupling agent is 12.8 parts of solid Si69; the vulcanizing agent is 1.5 parts; and the accelerator is 4 parts.

[0057] The mixing and vulcanization methods of the tire rubber composition of this embodiment are the same as those of Example 1.

[0058] Example 4

[0059] Compared with Example 1, the amounts of solution-polymerized styrene-butadiene rubber and cis-1,4-butadiene rubber in the raw material and combined rubber system of the tire rubber composition of this embodiment are different. The raw material formula of this embodiment is: 40 parts of cis-1,4-butadiene rubber; 60 parts of solution-polymerized styrene-butadiene rubber, and the mass percentage of styrene groups in the molecular chain of the solution-polymerized styrene-butadiene rubber is 36% and the mass percentage of vinyl groups is 26%.

[0060] The filler is 80 parts of SiO2; the plasticizer is 37.5 parts; the activator is 5 parts; the antioxidant is 3 parts; the silane coupling agent is 12.8 parts of solid Si69; the vulcanizing agent is 1.5 parts; and the accelerator is 4 parts.

[0061] The mixing and vulcanization methods of the tire rubber composition of this embodiment are the same as those of Example 1.

[0062] Example 5

[0063] Compared with Example 2, the amounts of solution-polymerized styrene-butadiene rubber and cis-1,4-butadiene rubber in the raw material and combined rubber system of the tire rubber composition of this embodiment are different. The raw material formula of this embodiment is: 40 parts of cis-1,4-butadiene rubber; 60 parts of solution-polymerized styrene-butadiene rubber, and the mass percentage of styrene groups in the molecular chain of the solution-polymerized styrene-butadiene rubber is 40%, and the mass percentage of vinyl groups is 14%.

[0064] Filler is SiO2 80 parts; plasticizer 37.5 parts; active agent 5 parts; antioxidant 3 parts; silane coupling agent is solid Si6912.8 parts; vulcanizing agent 1.5 parts; accelerator 4 parts;

[0065] The mixing and vulcanization methods of the tire rubber composition of this embodiment are the same as those of Example 1.

[0066] Comparative Example 1

[0067] Compared with Example 1, the content of styrene groups and vinyl groups in the solution polymerized styrene butadiene rubber molecular chain in the raw materials of the tire rubber composition of this comparative example is different. The raw material formula of this comparative example is: 30 parts of cis-1,4-butadiene rubber; 70 parts of solution polymerized styrene butadiene rubber, and the mass percentage of styrene groups in the solution polymerized styrene butadiene rubber molecular chain is 21% and the mass percentage of vinyl groups is 43%.

[0068] The filler is 80 parts of SiO2; the plasticizer is 37.5 parts; the activator is 5 parts; the antioxidant is 3 parts; the silane coupling agent is 12.8 parts of solid Si69; the vulcanizing agent is 1.5 parts; and the accelerator is 4 parts.

[0069] The mixing and vulcanization methods of the tire rubber composition of this comparative example are the same as those in Example 1.

[0070] Comparative Example 2

[0071] Compared with Example 2, the raw rubber system of the tire rubber composition of this comparative example is solution polymerized styrene-butadiene rubber. The raw material formula of this comparative example is: 100 parts of solution polymerized styrene-butadiene rubber, and the mass percentage of styrene groups in the solution polymerized styrene-butadiene rubber molecular chain is 40% and the mass percentage of vinyl groups is 14%;

[0072] The filler is 80 parts of SiO2; the plasticizer is 37.5 parts; the activator is 5 parts; the antioxidant is 3 parts; the silane coupling agent is 12.8 parts of solid Si69; the vulcanizing agent is 1.5 parts; and the accelerator is 4 parts.

[0073] The mixing and vulcanization methods of the tire rubber composition of this comparative example are the same as those in Example 1.

[0074] Comparative Example 3

[0075] Compared with Example 2, the amounts of solution-polymerized styrene-butadiene rubber and cis-1,4-butadiene rubber in the raw material and mixed rubber system of the tire rubber composition of this comparative example are different. The raw material formula of this comparative example is: 10 parts of cis-1,4-butadiene rubber; 90 parts of solution-polymerized styrene-butadiene rubber, and the mass percentage of styrene groups in the molecular chain of the solution-polymerized styrene-butadiene rubber is 40%, and the mass percentage of vinyl groups is 14%.

[0076] The filler is 80 parts of SiO2; the plasticizer is 37.5 parts; the activator is 5 parts; the antioxidant is 3 parts; the silane coupling agent is 12.8 parts of solid Si69; the vulcanizing agent is 1.5 parts; and the accelerator is 4 parts.

[0077] The mixing and vulcanization methods of the tire rubber composition of this comparative example are the same as those in Example 1.

[0078] Comparative Example 4

[0079] Compared with Example 3, the content of styrene groups and vinyl groups in the solution polymerized styrene-butadiene rubber molecular chain in the raw materials of the tire rubber composition of this comparative example is different. The raw material formula of this comparative example is: 40 parts of cis-1,4-butadiene rubber; 60 parts of solution polymerized styrene-butadiene rubber, and the mass percentage of styrene groups in the solution polymerized styrene-butadiene rubber molecular chain is 21%, and the mass percentage of vinyl groups is 43%;

[0080] Filler is SiO2 80 parts; plasticizer 37.5 parts; active agent 5 parts; antioxidant 3 parts; silane coupling agent is solid Si6912.8 parts; vulcanizing agent 1.5 parts; accelerator 4 parts;

[0081] The mixing and vulcanization methods of the tire rubber composition of this comparative example are the same as those in Example 1.

[0082] Comparative Example 5

[0083] Compared with Example 1, the raw rubber system of the tire rubber composition of this comparative example is butadiene rubber, and the raw material formula of this comparative example is: 100 parts of butadiene rubber; 80 parts of SiO2 filler; 37.5 parts of plasticizer; 5 parts of activator; 3 parts of antioxidant; 12.8 parts of solid Si69 silane coupling agent; 1.5 parts of vulcanizing agent; and 4 parts of accelerator.

[0084] The mixing and vulcanization methods of the tire rubber composition of this comparative example are the same as those in Example 1.

[0085] Performance Testing

[0086] The tire rubber compositions prepared in Examples 1-5 and Comparative Examples 1-5 were tested for wear resistance and wet skid resistance, and the test results were recorded. The test results were compared with the differences between the wet skid resistance-related parameters and the wear resistance-related parameters of the tire rubber compositions of Examples 1-5 and Comparative Examples 1-5 calculated according to the screening method of the present invention. The results are shown in Table 2.

[0087] The wear resistance was measured using a DIN abrasion tester (Kamishima Co., Ltd., Japan, model GT-7012-D) in accordance with the national standard GB / T 9867-2008 "Determination of wear resistance of vulcanized or thermoplastic rubber (rotating roller abrader method)". The DIN abrasion loss of the tire tread rubber compositions of Examples 1-5 and Comparative Examples 1-5 was measured at a load of 5 N. A smaller DIN abrasion loss indicates better wear resistance. The measurement results were expressed as an index, with the result of Comparative Example 1 set to 100. The other Examples and Comparative Examples were converted based on Comparative Example 1. A larger index indicates better wear resistance of the tire tread rubber composition.

[0088] The anti-skid performance was measured using a dynamic thermomechanical analyzer DMA (NETZSCH, Germany, model EPLEXOR 500N) at a frequency of 10 Hz, a static strain of 7%, and a dynamic strain of 0.25%. The loss factors (tan δ) of the tire tread rubber compositions of Examples 1-5 and Comparative Examples 1-5 at different temperatures were measured, and the loss factors (tan δ@0°C) at 0°C were recorded. A larger loss factor (tan δ@0°C) indicated better anti-skid performance of the tire tread rubber composition. The measurement results were expressed as an index, with the result of Comparative Example 1 set to 100. The other Examples and Comparative Examples were converted based on Comparative Example 1. A larger index indicated better anti-skid performance.

[0089] Table 2 Properties of tire rubber compositions of Examples 1-7 and Comparative Examples 1-5

[0090]

[0091] As can be seen from the above, compared with Example 1, the content of styrene and vinyl in the molecular chain of solution polymerized styrene butadiene rubber in Comparative Example 1 is different, and the difference between the anti-skid performance parameter and the wear resistance performance parameter of Comparative Example 1 is 0.036, which is less than 0.09; compared with Example 2, the raw rubber system of the tire rubber composition of Comparative Example 2 only adopts solution polymerized styrene butadiene rubber. Although the tire tread rubber composition of Comparative Example 2 has good anti-skid performance, it has poor wear resistance, and the difference between the anti-skid performance parameter and the wear resistance performance parameter of Comparative Example 2 is 0; compared with Example 2, the amount of solution polymerized styrene butadiene rubber and butadiene rubber in the raw rubber system of Comparative Example 3 is different. Although the tire tread rubber composition of Comparative Example 3 has good anti-skid performance, it has poor wear resistance. The wear performance is poor. The difference between the anti-wet skid performance parameter and the wear resistance performance parameter of Comparative Example 3 is 0.045, which is less than 0.09. Compared with Example 3, the styrene and vinyl contents in the solution-polymerized styrene-butadiene rubber molecular chain of Comparative Example 4 are different. Although the tire tread rubber composition of Comparative Example 4 has good wear resistance, the anti-wet skid performance is poor. The difference between the anti-wet skid performance parameter and the wear resistance performance parameter of Comparative Example 4 is 0.049, which is less than 0.09. Compared with Example 1, the raw rubber system of the tire rubber composition of Comparative Example 5 only uses butadiene rubber. Although the tire tread rubber composition of Comparative Example 5 has good wear resistance, the anti-wet skid performance is poor. The difference between the anti-wet skid performance parameter and the wear resistance performance parameter of Comparative Example 5 is 0.

[0092] Examples 1-5 are tire rubber compositions prepared according to the screening method for wear-resistant and wet-skid-resistant tire rubber compositions provided by the present invention. The differences between their wet-skid-resistant performance parameters and wear-resistant performance parameters are all greater than 0.09, indicating that the tire rubber compositions of the embodiments of the present invention can take into account both wear resistance and wet-skid resistance. Moreover, after performance testing, the loss factors of tanδ@0℃ of the tire rubber compositions prepared in Examples 1-5 are all greater than those of Comparative Example 1, and the DIN indexes of the tire rubber compositions prepared in Examples 1-5 are all equivalent to or greater than those of Comparative Example 1, which is consistent with the judgment results of the screening method for wear-resistant and wet-skid-resistant tire rubber compositions provided by the present invention, indicating that the tire rubber compositions obtained by the screening method for wear-resistant and wet-skid-resistant tire rubber compositions of the present invention can take into account both wear resistance and wet-skid resistance of the tire rubber compositions.

[0093] The above-described embodiments are merely descriptions of preferred embodiments of the present invention and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various deformations, modifications, evolutions, and improvements made to the technical solutions of the present invention by ordinary technicians in this field should fall within the scope of protection determined by the claims of the present invention.

Claims

1. A wear-resistant and anti-skid tire rubber composition, characterized in that: The invention comprises solution-polymerized styrene-butadiene rubber and cis-butadiene rubber, wherein the difference between the anti-skid performance parameter and the wear resistance performance parameter of the wear-resistant and anti-skid tire rubber composition satisfies the following relationship: 0.67×W B ×(1.4×St S +0.85×Vi S )×|2.72×St S -0.69×Vi S |>0.09, Where W B St represents the mass percentage of butadiene rubber in the blended rubber system. S Indicates the mass percentage of styrene groups in the molecular chain of solution-polymerized styrene-butadiene rubber, Vi S It indicates the mass percentage of vinyl in the molecular chain of solution-polymerized styrene-butadiene rubber.

2. The wear-resistant and anti-skid tire rubber composition according to claim 1, characterized in that: The anti-skid performance parameter is greater than 0.53, where the anti-skid performance parameter y = (1.4 × St S +0.85×Vi S )×(W S +0.67×W B ×|2.72×St S -0.69×Vi S |), where W S It indicates the mass percentage of solution-polymerized styrene-butadiene rubber in the blended rubber system.

3. The wear-resistant and anti-skid tire rubber composition according to claim 2, characterized in that: Wear resistance parameter x = (1.4 × St S +0.85×Vi S )×W S .

4. The wear-resistant and anti-skid tire rubber composition according to claim 1, characterized in that: The mass percentage of butadiene rubber in the blended rubber system is 30% to 40%.

5. The wear-resistant and anti-skid tire rubber composition according to claim 1, characterized in that: Butyl rubber is a high cis-butadiene rubber, and its cis-1,4 structure content is above 96%.

6. The wear-resistant and anti-skid tire rubber composition according to claim 1, characterized in that: The mass percentage of styrene groups in the molecular chain of solution-polymerized styrene-butadiene rubber is 28%-45%.

7. The method for screening a wear-resistant and wet-slip resistant tire rubber composition according to any one of claims 1 to 6, characterized in that: The specific steps include: The microscopic composition of the solution polymerized styrene butadiene rubber was characterized by nuclear magnetic resonance, and the mass percentage of styrene groups in the molecular chain of the solution polymerized styrene butadiene rubber was obtained. S and the mass percentage of vinyl Vi S ; Based on the mass percentage of styrene groups in the molecular chain of solution polymerized styrene butadiene rubber (St) S and the mass percentage of vinyl Vi S , and solution polymerized styrene-butadiene rubber W in the rubber system S The mass percentage of butadiene rubber W B , establish a relationship between the difference between the wear resistance performance parameter and the anti-wet skid performance parameter, and screen the wear-resistant and anti-wet skid tire rubber composition according to the size of the difference.

8. The method for screening a wear-resistant and wet-slip resistant tire rubber composition according to claim 7, characterized in that: Before establishing the relationship between the wear resistance parameter and the anti-wet skid resistance parameter, the method further includes establishing the wear resistance parameter and the anti-wet skid resistance parameter, wherein: Wear resistance parameter x = (1.4 × St S +0.85×Vi S )×W S , Anti-slip performance parameter y = (1.4 × St S +0.85×Vi S )×(W S +0.67×W B ×|2.72×St S -0.69×Vi S |).

9. The method for screening a wear-resistant and wet-slip resistant tire rubber composition according to claim 8, characterized in that: A small x value indicates good wear resistance, and a large y value indicates good anti-skid performance.

10. The method for screening a wear-resistant and wet-slip resistant tire rubber composition according to claim 7, characterized in that: If the difference between the anti-skid performance parameter and the wear resistance performance parameter is less than 0.09, it means that the wear resistance and anti-skid performance of the tire rubber composition cannot meet the requirements at the same time; If the difference between the anti-skid performance parameter and the wear resistance performance parameter is greater than 0.09, it means that the wear resistance and anti-skid performance of the tire rubber composition can be taken into account.