Transparent medical PVC modified material and preparation method thereof

By using plasticizers such as trioctyl trimellitetate, diisononyl cyclohexane 1,2-dicarboxylate, and thermal stabilizers such as barium stearate and zinc stearate in polyvinyl chloride materials, combined with Methyl methacrylate-butadiene-styrene terpolymer and silane-modified nanotalc powder solve the problem of insufficient toughness and thermal stability of PVC materials in the medical field, and achieve high transparency and excellent comprehensive performance. Applicable to high standards in the medical field.

CN118879002APending Publication Date: 2024-11-01INVENTECH XIAMEN CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411100076.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Existing polyvinyl chloride (PVC) materials have shortcomings in toughness, thermal stability and fluidity, which limits their application in the medical field, especially the small market share of transparent medical products.

Method used

Trioctyl trimellitetate and diisononyl 1,2-dicarboxylate as plasticizers, barium stearate and zinc stearate as heat stabilizers, methyl methacrylate-stydiodinium Ethylene-styrene terpolymers are used as impact modifiers, silane-modified nanotalc powder is used as fillers, and ultramarine powder is used as a yellow-removing agent. Through precise proportioning and synergistic effects, the flexibility and thermal stability of the material are improved. , impact strength and transparency.

Benefits of technology

The prepared transparent medical PVC modified materials have high transparency, good temperature and weather resistance, excellent impact resistance and processing performance, and meet high standards in the medical field and are suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004989134630000121
    Figure BDA0004989134630000121
  • Figure BDA0004989134630000131
    Figure BDA0004989134630000131
Patent Text Reader

Abstract

The invention relates to the technical field of high polymer materials, in particular to a transparent medical PVC modified material and a preparation method thereof. The transparent medical PVC modified material is prepared from the following raw materials in parts by mass: 80 to 120 parts of PVC resin, 60 to 100 parts of plasticizer, 1 to 3 parts of heat stabilizer, 0.5 to 1.5 parts of lubricant, 10 to 15 parts of filling agent, 5 to 15 parts of impact modifier and 0.01 to 0.02 part of yellowing eliminating agent, and the plasticizer is prepared from trioctyl trimellitate TOTM and cyclohexane 1, 2-diisononyl phthalate. Through careful material selection and formula design, the PVC modified material achieves remarkable progress in the aspects of environmental protection, comprehensive performance, balance of transparency and mechanical performance, comprehensive improvement of processability and product performance and the like, and is particularly suitable for meeting the requirement for high-performance materials in the medical field. Meanwhile, the simplified production process and the efficient production method provide powerful guarantee for practical application and popularization of the product.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of polymer materials, and in particular to a transparent medical PVC modified material and a preparation method thereof. Background Art

[0002] Polyvinyl chloride (PVC) is one of the earliest industrialized and widely used general-purpose thermoplastics. It has the advantages of light weight, high strength, insulation, flame retardancy, corrosion resistance, excellent comprehensive performance, low price and wide source of raw materials. However, it also has the following disadvantages: 1. Poor toughness, it is very easy to crack when impacted, so it cannot be used as a structural material. In addition, the brittleness of polyvinyl chloride is greatly affected by temperature. The lower limit of use of general PVC products is -15℃, and the lower limit of use of soft PVC is -30℃; 2. Poor thermal stability, it begins to decompose HCl at 100℃, and decomposes more rapidly at temperatures above 150℃, while the melting temperature of PVC is about 210℃; 3. PVC has extremely high viscosity and poor fluidity, which limits its use to a certain extent. People often use methods such as adding fillers, elastomers, plasticizers, heat stabilizers, processing aids, heat-resistant modifiers and flow modifiers to improve the performance of PVC.

[0003] Polyvinyl chloride is a plastic raw material whose annual global output is second only to polyethylene. It has been widely used in various fields of production and life. Transparent products are also an important application field of polyvinyl chloride. They not only meet the requirements of mechanical, flame retardant and other performance of products, but also increase the beauty of products. However, due to the application of other transparent materials, transparent polyvinyl chloride products account for a small share in the market. Therefore, it is urgent to develop a high-performance transparent medical PVC modified material to meet market needs. Summary of the invention

[0004] The purpose of this application is to provide a transparent medical PVC modified material and a preparation method thereof in view of the deficiencies of the current technology. The transparent medical PVC modified material prepared by this application has high transparency, is environmentally friendly, and has excellent heat and weather resistance, excellent impact resistance, good flame retardant effect, excellent processing performance, and excellent comprehensive performance. In addition, this application provides a preparation method of a transparent medical PVC modified material, which has a simple process, convenient operation, stable quality, high production efficiency, and can be mass-produced industrially.

[0005] In the first aspect, the present application provides a transparent medical PVC modified material, which adopts the following technical solution: A transparent medical PVC modified material comprises the following raw materials by weight: 80-120 parts of PVC resin, 60-100 parts of plasticizer, 1-3 parts of heat stabilizer, 0.5-1.5 parts of lubricant, 10-15 parts of filler, 5-15 parts of impact modifier and 0.01-0.02 parts of anti-yellowing agent, wherein the plasticizer is composed of trioctyl trimellitate (TOTM) and diisononyl cyclohexane 1,2-dicarboxylate.

[0006] By adopting the above technical solutions, PVC resin: as a base material, it provides the mechanical strength and chemical stability of the material. PVC itself has good transparency and processing properties, but requires plasticizers to improve its flexibility and low-temperature performance. Plasticizers (trioctyl trimellitate TOTM and diisononyl cyclohexane 1,2-dicarboxylate): these two plasticizers act together on PVC resin, reducing the forces between molecular chains and improving the plasticity and softness of the material. The synergistic effect between them makes the products have better low-temperature resistance and durability. At the same time, due to their environmentally friendly properties, the safety and non-toxicity of the materials are ensured. Heat stabilizer: prevents PVC from decomposing at high temperatures, maintains the stability of the material and extends its service life. It is particularly important during processing because high temperatures may cause PVC to degrade. Lubricant: reduces the friction between PVC and processing equipment, improves molding efficiency, and also improves the surface quality of the finished product. The choice of lubricant has a direct impact on the appearance and performance of the final product. Filler: enhances the mechanical properties of PVC, such as hardness, tensile strength and impact strength, while also potentially reducing costs. Impact modifiers: significantly improve the impact strength of PVC, making the material tougher and less prone to cracking. This is particularly important for medical uses, as medical devices often need to maintain integrity under impact. Anti-yellowing agents: prevent PVC from yellowing due to long-term exposure to sunlight or other radiation sources, maintaining the transparency and appearance of the material. This is essential for maintaining a clean appearance and accurate readings of medical devices. In summary, through the precise proportions and interactions of these components, the transparent medical PVC modified material prepared not only has excellent physical and chemical properties, but also meets the high requirements of the medical field for material transparency, safety and stability. In addition, the preparation method of this material is simple and efficient, suitable for large-scale production, and provides a high-quality, high-performance material option for the medical device industry.

[0007] Preferably, the mass ratio of trioctyl trimellitate TOTM to diisononyl cyclohexane 1,2-dicarboxylate is 2-4:1.

[0008] By adopting the above technical scheme, trioctyl trimellitate TOTM is an effective main plasticizer, which can significantly reduce the glass transition temperature of PVC and improve the softness and ductility of the material. TOTM has high heat resistance and can keep the physical properties of PVC products stable over a wide temperature range. TOTM has good electrical insulation properties, which is particularly important for the application of medical equipment. The addition of TOTM improves the low-temperature performance of PVC, so that it can still maintain good flexibility in cold environments. Diisononyl cyclohexane 1,2-dicarboxylate (DINCH), as a non-phthalate plasticizer, has excellent toxicological properties and is particularly suitable for medical and food contact applications. DINCH is considered to be an environmentally friendly and safe plasticizer, especially for medical products with extremely high safety requirements. DINCH has low volatility, which helps to maintain long-term plasticization effects and reduce the degradation of material properties caused by plasticizer loss. The combination of TOTM and DINCH takes advantage of the advantages of both. TOTM provides good temperature resistance and electrical insulation, while DINCH provides the necessary environmental protection and safety. The compound use of the two plasticizers, through synergistic effect, further reduces the glass transition temperature of PVC and improves the flexibility and service life of the material at low temperatures. This specific ratio helps to improve the solubility and stability of the plasticizer in PVC, thereby extending the service life of the product. By adjusting the ratio of the two plasticizers, the mechanical properties and environmental adaptability of the material can be optimized while maintaining good processing performance. In summary, the compound use of trioctyl trimellitate TOTM and diisononyl cyclohexane 1,2-dicarboxylate in a mass ratio of 2-4:1 not only improves the transparency and environmental performance of PVC materials, but also significantly improves the material's heat resistance, cold resistance and electrical insulation properties through its synergistic effect, while meeting the high standards of safety and stability of medical-grade products.

[0009] Preferably, the thermal stabilizer is composed of (RC00)2Ba and (RC00)2Zn in a molar ratio of 1.4-2.2:1, wherein R is C8-C 24 Alkenyl or C6-C 24 The alkenyl group.

[0010] By adopting the above technical solutions, the selection of heat stabilizers is crucial to improving the thermal stability and transparency of the material. Preventing PVC from degrading: During the heating process, PVC is prone to degradation and releases HCl, which can lead to a decrease in material properties, such as yellowing and reduced strength. Heat stabilizers can effectively capture the generated HCl, prevent or delay this process, thereby improving the processing stability and use stability of PVC. Improving processing safety: By preventing PVC from degrading prematurely, heat stabilizers ensure that the material does not produce potentially harmful gases due to degradation during high-temperature processing, ensuring the health and safety of operators. Barium (Ba) and zinc (Zn) carboxylates generally have complementary effects in heat stabilizers. Barium salts are mainly responsible for capturing HCl, while zinc salts can replace unstable chlorine atoms in the PVC molecular chain, thereby reducing the initiation point of degradation. The combination of the two can effectively replace unstable chlorine atoms while capturing HCl, thereby providing more comprehensive protection and enhancing the long-term thermal stability of the material. This combination of heat stabilizers helps maintain the physical and chemical properties of PVC, especially under long-term high temperature conditions, ensuring that the material does not lose mechanical strength and transparency, which is extremely important for medical applications. The long-chain fatty acids in traditional calcium-zinc stabilizers have poor compatibility with PVC, which affects the transparency of the material. The design of the new organic calcium-zinc in the present application not only improves the thermal stability by introducing a (poly)ester structure with better compatibility with PVC, but also greatly improves the transparency of the material due to the improved compatibility. In summary, the heat stabilizer combination in the present application, through its unique formula and synergistic effect, not only significantly improves the thermal stability of the PVC material, but also optimizes the transparency and overall performance of the material, making it more suitable for the high standards required in the medical field. The use of this heat stabilizer embodies the advanced concept of dual consideration of performance and environmental safety in material design.

[0011] Preferably, the heat stabilizer is composed of barium stearate and zinc stearate in a molar ratio of 1.4-1.8:1.

[0012] By adopting the above technical scheme, the barium zinc heat stabilizer composed of barium stearate and zinc stearate is a non-toxic, transparent heat stabilizer, which can capture HCl produced by thermal decomposition of PVC to prevent the catalytic degradation of HCl and achieve thermal stability of the material. The present application selects barium stearate and zinc stearate as heat stabilizers and controls their molar ratio to 1.4-1.8:1, so that the heat stabilization effect is good and the material has lubricity, so that the material has good dispersibility, compatibility and processing fluidity during the processing, and the material has excellent thermal stability and high efficiency weather resistance.

[0013] Preferably, the heat stabilizer is composed of barium laurate and zinc laurate in a molar ratio of 1.6-2.0:1.

[0014] By adopting the above technical scheme, the barium zinc heat stabilizer composed of barium laurate and zinc laurate is a non-toxic, transparent heat stabilizer, which can capture the HC1 generated by the thermal decomposition of PVC to prevent the catalytic degradation of HC1, thereby achieving thermal stability of the material. The present application selects barium laurate and zinc laurate as heat stabilizers and controls their molar ratio to 1.6-2.0:1, so that the heat stabilization effect is good and the material has lubricity, so that the material has good dispersibility, compatibility and processing fluidity during the processing, so that the material has excellent thermal stability and high efficiency weather resistance. Preferably, the heat stabilizer is composed of barium ricinoleate and zinc ricinoleate in a molar ratio of 1.8-2.2:1.

[0015] By adopting the above technical scheme, the barium zinc heat stabilizer composed of barium ricinoleate and zinc ricinoleate is a non-toxic, transparent heat stabilizer, which can capture HCl generated by thermal decomposition of PVC to prevent the catalytic degradation of HCl, thereby achieving thermal stability of the material. The present application selects barium ricinoleate and zinc ricinoleate as heat stabilizers and controls their molar ratio to 1.8-2.2:1, so that the heat stabilization effect is good and the material has lubricity, so that the material has good dispersibility, compatibility and processing fluidity during the processing, and the material has excellent thermal stability and high efficiency weather resistance.

[0016] Preferably, the lubricant is composed of liquid paraffin and stearic acid in a mass ratio of 1.2-1.8:1.

[0017] By adopting the above technical scheme, liquid paraffin is used as an external lubricant to reduce the friction between the PVC melt and the mold and the barrel; stearic acid is used as an internal lubricant to reduce the intermolecular friction of the PVC melt; the two lubricants are mixed in a weight ratio of 1.2-1.8:1 to improve the fluidity of the material and the demoulding property of the product during the processing.

[0018] Preferably, the filler is silane-modified nano-talc powder with a particle size of 2-20 nm.

[0019] By adopting the above technical scheme, the transparent medical PVC modified material of the present application can prepare a translucent environmentally friendly PVC modified material by adding a filler; the smaller the particle size of the filler, the more beneficial it is to the tensile strength and impact strength of the filling material. The present application selects silane-modified nano talc as a filler and controls its particle size to 2-20nm, which can improve the strength of the material; the good compatibility of silane-modified nano talc with resin is the key to exerting its function and controlling the addition amount. The present application uses silane-modified nano talc with a particle size of 2-20nm, which can improve the compatibility of talc with PVC resin, thereby improving the strength of the material.

[0020] Preferably, the method for preparing the silane-modified nano-talc powder comprises the following steps: S71, according to the mass fractions, 1 part of γ-(methacryloyloxy)propyltrimethoxysilane was mixed with 70 parts of ethanol and 10 parts of water, and the mixture was hydrolyzed for 4 hours to obtain a mixture A; S72, adding 80 parts of nano talc powder to mixture A, then heating to 45°C, stirring at 200 r / min for 200 min, finally centrifugally filtering, washing with ethanol, drying at 80°C, and grinding to obtain silane-modified nano talc powder with a particle size of 2-20 nm.

[0021] By adopting the above technical scheme, the preparation method of silane-modified nano talc involves multiple chemical and physical processes, aiming to improve the compatibility of talc with PVC resin and enhance the mechanical properties of the final material. S71, hydrolysis reaction: In this step, γ-(methacryloyloxy)propyltrimethoxysilane is mixed with ethanol and water, and a silane hydrolyzate is generated after a 4-hour hydrolysis reaction. This step is the key to the preparation of silane-modified nano talc, because the hydrolysis reaction enables the silane compound to react chemically with the surface of talc. S72, the combination of silane and talc: Nano talc is added to the mixture A containing silane hydrolyzate, heated to 45 ° C, and stirred at a speed of 200r / min for 200 minutes. This process promotes the full contact and reaction of the silane hydrolyzate with the surface of talc, and the silane compound is evenly coated on the surface of talc by chemical bonding. Subsequently, by centrifugal filtration, ethanol washing, drying and grinding, a silane-modified nano talc with a particle size of 2-20nm is obtained. The main function of silane-modified nano-talc is to improve the compatibility between inorganic filler (talc) and organic polymer (PVC resin). Silane acts as a coupling agent, with one end chemically reacting with the surface of talc and the other end forming a stable chemical bond with PVC resin. This dual chemical action significantly enhances the interfacial adhesion between talc and PVC, thereby improving the mechanical properties of the material, such as tensile strength and impact strength. Due to the good compatibility of silane-modified talc with PVC, the modified talc can be more evenly dispersed in the PVC matrix, reducing the agglomeration of fillers. This helps talc to play its reinforcing role more effectively and improve the mechanical properties of the material. The addition of silane-modified talc also helps to improve the thermal stability and weather resistance of PVC materials, which is particularly important for medical applications. The addition of silane-modified talc can also improve the processing properties of PVC due to its good compatibility and dispersibility. During the processing, the modified talc can reduce the melt viscosity and improve the fluidity, thereby improving the molding processability. In summary, the preparation and application of silane-modified nano-talc not only improves the mechanical properties and processing properties of PVC materials, but also achieves an overall improvement in material performance by improving the compatibility between inorganic fillers and organic polymers.

[0022] Preferably, the impact modifier is a methyl methacrylate-butadiene-styrene terpolymer, wherein the mass content of the methyl methacrylate unit is 40-60%, the mass content of the butadiene unit is 20-30%, and the mass content of the styrene unit is 20-30%.

[0023] By adopting the above technical solution, methyl methacrylate-butadiene-styrene terpolymer (MBS) plays a vital role as an impact modifier. The content ratio of MBS - 40-60% by mass of methyl methacrylate units, 20-30% by mass of butadiene units, and 20-30% by mass of styrene units - is carefully designed to optimize the multi-faceted performance of PVC materials. Improve impact strength: MBS has good thermodynamic compatibility with PVC, which is mainly due to the similarity of their solubility parameters. Good compatibility ensures that MBS can be evenly dispersed in the PVC matrix to form a stable polymer alloy. When the material is impacted by external force, MBS particles can effectively absorb and disperse energy, inhibit the expansion of cracks, and thus significantly improve the impact strength of PVC materials. Maintain the transparency of the material: MBS and PVC have similar refractive indices (MBS is 1.528-1.540, PVC is 1.534-1.538), which enables the two to achieve a uniform refractive index after melt blending, without light scattering, and thus without affecting the transparency of the material. The particle size of MBS particles is smaller than the wavelength of visible light, which further ensures that it effectively improves the impact resistance of the material while not affecting the transparency of PVC. Improve cold resistance and processing fluidity: By controlling the content of methyl methacrylate units, butadiene units and styrene units in MBS, not only can the mechanical properties of PVC materials be optimized, but also their cold resistance and processing fluidity can be improved. The methyl methacrylate unit provides good mechanical strength and hardness, the butadiene unit gives the material excellent cold resistance and toughness, and the styrene unit helps to improve the rigidity and processing fluidity of the material. The addition of MBS not only improves the impact resistance of PVC materials, but also further improves the transparency, cold resistance and processing fluidity of the material through its good compatibility with PVC. This synergistic effect enables the modified PVC material to meet the transparency and mechanical property requirements of medical devices while also having good low temperature resistance and processing performance, greatly expanding its application range in the medical field. In short, methyl methacrylate-butadiene-styrene terpolymer, as an impact modifier, plays a key role in transparent medical PVC modified materials, achieving a comprehensive improvement in material performance by improving the material's impact strength, maintaining transparency, and improving cold resistance and processing fluidity.

[0024] Preferably, the yellowing agent is ultramarine powder; Preferably, the PVC resin is a PVC resin with a degree of polymerization of 1000-1200.

[0025] By adopting the above technical scheme, the molecular weight (polymerization degree) of PVC resin is directly related to its physical and mechanical properties. The higher the degree of polymerization, the longer the molecular chain of PVC resin, the stronger the interaction force between molecules, so that the product has higher tensile strength, impact strength and elastic modulus. For medical applications, the improvement of these properties is particularly important, because medical devices often need to withstand various external forces without damage, and at the same time, they need to maintain sufficient toughness and elasticity to adapt to complex use environments. The melt formed by PVC resin with a higher degree of polymerization when heated is relatively stable and has high melt strength, which helps to prevent material breakage during processing and ensure the quality of the product. At the same time, good melt strength can also improve the processing fluidity of the material, making PVC modified materials easier to form during extrusion, injection molding and other processing processes, and the size is stable after forming, which is particularly important for the production of precision medical devices. PVC resins with a higher degree of polymerization usually have better temperature resistance and weather resistance. This is because the longer molecular chain makes the internal structure of the material more compact, thereby improving its resistance to the external environment (such as temperature changes, ultraviolet radiation, etc.). These characteristics enable the modified PVC material to maintain its physical properties and transparency for a long time, and can be reliably used in the medical field even under harsh environmental conditions. Compared with PVC resins with low polymerization degrees, PVC resins with a polymerization degree of 1000-1200 have better compatibility with other components such as plasticizers and heat stabilizers, which helps to form a more uniform mixture between the components, thereby improving the overall performance of the material. In particular, when used in conjunction with specific plasticizers (such as trioctyl trimellitate TOTM and diisononyl cyclohexane 1,2-dicarboxylate), the softness, low temperature resistance and transparency of the product can be further improved, meeting the various requirements of medical applications for material performance. In short, by selecting PVC resins with a polymerization degree of 1000-1200, the transparent medical PVC modified material of this application is not only significantly improved in physical and mechanical properties, but also shows excellent performance in terms of temperature resistance, weather resistance and processing performance, fully meeting the high standards for material performance in the field of medical applications.

[0026] In a second aspect, the present application provides a method for preparing a transparent medical PVC modified material, using the following technical solution: As a general technical concept, the present application also provides a method for preparing the above-mentioned transparent medical PVC modified material, comprising the following steps: S101, mixing PVC resin, plasticizer, heat stabilizer, lubricant, filler, impact modifier and anti-yellowing agent uniformly according to their weight proportions to obtain a mixture A; S102, placing mixed material A into a high-speed blender, stirring at a temperature of 100-140° C. for 15-25 min to obtain mixed material B; S103, extruding and granulating the mixed material B through a twin-screw extruder to obtain a transparent medical PVC modified material, wherein the screw temperatures of the twin-screw extruder are: zone 1 temperature 138-160°C, zone 2 temperature 135-160°C, zone 3 temperature 135-155°C, zone 4 temperature 132-150°C and zone 5 temperature 130-148°C.

[0027] In summary, the beneficial technical effects of this application are: 1. This application uses trioctyl trimellitate TOTM and diisononyl cyclohexane 1,2-dicarboxylate as plasticizers. Both plasticizers are environmentally friendly plasticizers, which can reduce the interaction between PVC molecular chains, reduce the glass transition temperature, flow temperature and melting point of the contained microcrystals of PVC plastics, and improve the plasticity of the resin, making the product soft and resistant to low temperatures. When the two plasticizers are compounded in a weight ratio of 2-4:1, the synergistic effect between them can be used to significantly improve the softness and low temperature resistance of the product.

[0028] 2. This application makes a fundamental change in the organic ligand, breaking through the traditional idea of ​​using long-chain fatty acids as organic ligands for calcium-zinc soaps, and designs and synthesizes a new calcium-zinc ligand with a (poly)ester structure, so that the new organic calcium-zinc has better compatibility with PVC than traditional fatty acid calcium-zinc.

[0029] 3. This application uses methyl methacrylate-butadiene-styrene terpolymer as an impact modifier, which has no effect on the transparency of the PVC material, and by controlling the content of methyl methacrylate units at 40-60%, the content of butadiene units at 20-30%, and the content of styrene units at 20-30%, the impact strength of the material can be improved, and the cold resistance and processing fluidity of the material can also be improved.

[0030] 4. This application selects barium stearate and zinc stearate as heat stabilizers and controls the molar ratio thereof to 1.4-1.8:1, which has good heat stabilization effect and lubricity, so that the material has good dispersibility, compatibility and processing fluidity during the processing, and the material has excellent thermal stability and high weather resistance.

[0031] 5. The present application can make the product have higher strength by controlling the degree of polymerization of PVC resin to 1000-1200.

[0032] 6. The present application uses silane-modified nano-talc as a filler and controls its particle size to 2-20 nm, thereby improving the strength of the material; the use of silane-modified nano-talc with a particle size of 2-20 nm can improve the compatibility of talc with PVC resin, thereby improving the strength of the material.

[0033] 7. The transparent and environmentally friendly PVC modified material prepared by the present application has various properties that exceed the national standards, with high transparency, environmental protection, excellent high temperature resistance, high strength, good flame retardant effect, strong compression performance and toughness, excellent processing performance, and excellent comprehensive performance. The product of the present invention complies with international standards such as REACH, ROHS, PAHS, NP, etc., and can be widely used in the medical field.

[0034] 8. The preparation method of the present application has simple process, convenient operation and control, stable quality, high production efficiency, and can be produced on a large scale in an industrial manner. DETAILED DESCRIPTION

[0035] The embodiments of the present application will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. In the examples, if specific conditions are not specified, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0036] In the following preparation examples and embodiments, 1 part means 0.1 kg.

[0037] Preparation Example 1 Preparation of Silane-modified Nano-talc The preparation method of silane-modified nano talc powder comprises the following steps: S71, according to the mass fractions, 1 part of γ-(methacryloyloxy)propyltrimethoxysilane was mixed with 70 parts of ethanol and 10 parts of water, and the mixture was hydrolyzed for 4 hours to obtain a mixture A; S72, adding 80 parts of nano talc powder to mixture A, then heating to 45°C, stirring at 200 r / min for 200 min, finally centrifugally filtering, washing with ethanol, drying at 80°C, and grinding to obtain silane-modified nano talc powder with a particle size of 2 nm.

[0038] Preparation Example 2 The same as the preparation example, except that 8 nm silane-modified nano talc powder was prepared.

[0039] Preparation Example 3 The same as the preparation example, except that 10 nm silane-modified nano talc powder was prepared.

[0040] Preparation Example 4 The same as the preparation example, except that 15 nm silane-modified nano talc powder was prepared.

[0041] Preparation Example 5 The same as the preparation example, except that 20 nm silane-modified nano talc powder was prepared.

[0042] Example 1 A transparent medical PVC modified material, comprising the following raw materials by mass: 80 parts of PVC resin, 60 parts of plasticizer, 1.5 parts of heat stabilizer, 0.5 parts of lubricant, 10 parts of filler, 5 parts of impact modifier, and 0.01 parts of ultramarine powder, wherein the plasticizer is composed of trioctyl trimellitate TOTM and diisononyl cyclohexane 1,2-dicarboxylate in a mass ratio of 2:1, and the heat stabilizer is composed of barium stearate and zinc stearate in a molar ratio of 1. 4:1, the lubricant is composed of liquid paraffin and stearic acid in a mass ratio of 1.2:1, the filler is the silane-modified nano talc prepared in Preparation Example 1, the impact modifier is a methyl methacrylate-butadiene-styrene terpolymer, wherein the mass content of methyl methacrylate units is 40%, the mass content of butadiene units is 30%, and the mass content of styrene units is 30%, and the PVC resin is a PVC resin with a degree of polymerization of 1000; The method for preparing the above-mentioned transparent medical PVC modified material comprises the following steps: S101, mixing PVC resin, plasticizer, heat stabilizer, lubricant, filler, impact modifier and ultramarine powder uniformly according to parts by mass to obtain a mixture A; S102, placing mixed material A into a high-speed blender, and stirring at 100° C. for 15 min to obtain mixed material B; S103, extruding and granulating the mixed material B through a twin-screw extruder to obtain a transparent medical PVC modified material, wherein the screw temperatures of the twin-screw extruder are: zone 1 temperature 138° C., zone 2 temperature 135° C., zone 3 temperature 135° C., zone 4 temperature 132° C. and zone 5 temperature 130° C.

[0043] Example 2 A transparent medical PVC modified material, comprising the following raw materials by mass: 90 parts of PVC resin, 70 parts of plasticizer, 2 parts of heat stabilizer, 0.8 parts of lubricant, 11 parts of filler, 8 parts of impact modifier, and 0.02 parts of ultramarine powder, wherein the plasticizer is composed of trioctyl trimellitate TOTM and diisononyl cyclohexane 1,2-dicarboxylate in a mass ratio of 2.5:1, and the heat stabilizer is composed of barium stearate and zinc stearate in a molar ratio of 1.6: 1, the lubricant is composed of liquid paraffin and stearic acid in a mass ratio of 1.3:1, the filler is the silane-modified nano talc prepared in Preparation Example 2, the impact modifier is a methyl methacrylate-butadiene-styrene terpolymer, wherein the mass content of methyl methacrylate units is 45%, the mass content of butadiene units is 27.5%, and the mass content of styrene units is 27.5%, and the PVC resin is a PVC resin with a degree of polymerization of 1050; The method for preparing the above-mentioned transparent medical PVC modified material comprises the following steps: S101, mixing PVC resin, plasticizer, heat stabilizer, lubricant, filler, impact modifier and ultramarine powder uniformly according to parts by mass to obtain a mixture A; S102, placing mixed material A into a high-speed blender, and stirring at 110° C. for 18 min to obtain mixed material B; S103, extruding and granulating the mixed material B through a twin-screw extruder to obtain a transparent medical PVC modified material, wherein the screw temperatures of the twin-screw extruder are: zone 1 temperature 144° C., zone 2 temperature 141° C., zone 3 temperature 140° C., zone 4 temperature 136° C. and zone 5 temperature 135° C.

[0044] Example 3 A transparent medical PVC modified material, comprising the following raw materials by mass: 100 parts of PVC resin, 80 parts of plasticizer, 2.1 parts of heat stabilizer, 1 part of lubricant, 12.5 parts of filler, 10 parts of impact modifier, and 0.01 parts of ultramarine powder, wherein the plasticizer is composed of trioctyl trimellitate TOTM and diisononyl cyclohexane 1,2-dicarboxylate in a mass ratio of 3:1, and the heat stabilizer is composed of barium stearate and zinc stearate in a molar ratio of 1:1. .7:1, the lubricant is composed of liquid paraffin and stearic acid in a mass ratio of 1.5:1, the filler is the silane-modified nano talc powder obtained in Preparation Example 3, the impact modifier is a methyl methacrylate-butadiene-styrene terpolymer, wherein the mass content of methyl methacrylate units is 50%, the mass content of butadiene units is 25%, and the mass content of styrene units is 25%, and the PVC resin is a PVC resin with a degree of polymerization of 1100; The method for preparing the above-mentioned transparent medical PVC modified material comprises the following steps: S101, mixing PVC resin, plasticizer, heat stabilizer, lubricant, filler, impact modifier and ultramarine powder uniformly according to parts by mass to obtain a mixture A; S102, placing mixed material A into a high-speed blender, and stirring at 120° C. for 20 min to obtain mixed material B; S103, extruding and granulating the mixed material B through a twin-screw extruder to obtain a transparent medical PVC modified material, wherein the screw temperatures of the twin-screw extruder are: zone 1 temperature 149° C., zone 2 temperature 147° C., zone 3 temperature 145° C., zone 4 temperature 141° C. and zone 5 temperature 139° C.

[0045] Example 4 A transparent medical PVC modified material, comprising the following raw materials by mass: 110 parts of PVC resin, 90 parts of plasticizer, 2.5 parts of heat stabilizer, 1.2 parts of lubricant, 13 parts of filler, 12 parts of impact modifier, and 0.02 parts of ultramarine color powder, wherein the plasticizer is composed of trioctyl trimellitate TOTM and diisononyl cyclohexane 1,2-dicarboxylate in a mass ratio of 3.5:1, and the heat stabilizer is composed of barium laurate and zinc laurate in a molar ratio of 1. 8:1, the lubricant is composed of liquid paraffin and stearic acid in a mass ratio of 1.7:1, the filler is the silane-modified nano talc prepared in Preparation Example 4, the impact modifier is a methyl methacrylate-butadiene-styrene terpolymer, wherein the mass content of methyl methacrylate units is 55%, the mass content of butadiene units is 22.5%, and the mass content of styrene units is 22.5%, and the PVC resin is a PVC resin with a degree of polymerization of 1150; The method for preparing the above-mentioned transparent medical PVC modified material comprises the following steps: S101, mixing PVC resin, plasticizer, heat stabilizer, lubricant, filler, impact modifier and ultramarine powder uniformly according to parts by mass to obtain a mixture A; S102, placing mixed material A into a high-speed blender, and stirring at 130° C. for 22 min to obtain mixed material B; S103, extruding and granulating the mixed material B through a twin-screw extruder to obtain a transparent medical PVC modified material, wherein the screw temperatures of the twin-screw extruder are: zone 1 temperature 155° C., zone 2 temperature 153° C., zone 3 temperature 150° C., zone 4 temperature 145° C. and zone 5 temperature 144° C.

[0046] Example 5 A transparent medical PVC modified material, comprising the following raw materials by mass: 120 parts of PVC resin, 100 parts of plasticizer, 3 parts of heat stabilizer, 1.5 parts of lubricant, 15 parts of filler, 15 parts of impact modifier, and 0.01 parts of ultramarine color powder, wherein the plasticizer is composed of trioctyl trimellitate TOTM and diisononyl cyclohexane 1,2-dicarboxylate in a mass ratio of 4:1, and the heat stabilizer is composed of barium ricinoleate and zinc ricinoleate in molar proportions. The lubricant is composed of liquid paraffin and stearic acid in a mass ratio of 2:1, the filler is the silane-modified nano talc prepared in Preparation Example 5, the impact modifier is a methyl methacrylate-butadiene-styrene terpolymer, wherein the mass content of the methyl methacrylate unit is 60%, the mass content of the butadiene unit is 20%, and the mass content of the styrene unit is 20%, and the PVC resin is a PVC resin with a degree of polymerization of 1200; The method for preparing the above-mentioned transparent medical PVC modified material comprises the following steps: S101, mixing PVC resin, plasticizer, heat stabilizer, lubricant, filler, impact modifier and ultramarine powder uniformly according to parts by mass to obtain a mixture A; S102, placing mixed material A into a high-speed blender, and stirring at 140° C. for 25 min to obtain mixed material B; S103, extruding and granulating the mixed material B through a twin-screw extruder to obtain a transparent medical PVC modified material, wherein the screw temperatures of the twin-screw extruder are: zone 1 temperature 160° C., zone 2 temperature 160° C., zone 3 temperature 155° C., zone 4 temperature 150° C. and zone 5 temperature 148° C.

[0047] Comparative Example 1 The same as Example 3, except that the plasticizer is trioctyl trimellitate TOTM.

[0048] Comparative Example 2 The same as Example 3, except that the plasticizer is diisononyl cyclohexane 1,2-dicarboxylate.

[0049] Comparative Example 3 The same as Example 3, except that an equal amount of nano talc powder with a particle size of 10 nm is used to replace the silane-modified nano talc powder prepared in Preparation Example 3.

[0050] Comparative Example 4 The same as Example 3, except that the thermal stabilizer is barium stearate.

[0051] Comparative Example 5 The same as Example 3, except that the thermal stabilizer is zinc stearate.

[0052] Performance Testing The transparent medical PVC modified materials prepared in Examples 1 to 5 and Comparative Examples 1 to 5 were sampled and subjected to the following tests. The test results are shown in Table 1.

[0053] Flame retardancy test: tested using UL94 standard; Light transmittance: Use a light transmittance / haze tester to test the light transmittance of the sample in accordance with GB / T2410-2008 standard; Tensile strength, elongation at break and flexural strength: tested in accordance with GB / T1040-1992 "Test method for tensile properties of plastics"; The hardness was tested using a durometer (Shore D); Thermal stability: thermal stability is characterized according to the national standard GB / T 2917.1-2002 "Determination of hydrogen chloride and any other acidic products released by blends and products based on vinyl chloride homopolymers and copolymers at 200°C"; Impact brittleness temperature (℃): Use an impact testing machine to test the impact brittleness temperature of the sample in accordance with GB / T2843-2008 standard; Heat deformation temperature (℃): Test in accordance with GB / T1634.1-2020.

[0054] Table 1 Performance test Analyzing the data in Table 1, we can see that: 1) The transparent medical PVC modified materials prepared by Examples 1 to 5 have various properties that exceed the national standards, have high transparency, a light transmittance of up to 93-95%, are environmentally friendly, have excellent high temperature resistance, high strength, good flame retardant effect, strong compression performance and toughness, excellent processing performance, and excellent comprehensive performance. The products of the present invention comply with international standards such as REACH, ROHS, PAHS, NP, etc., and can be widely used in the medical field.

[0055] 2) The performance comparison analysis of the transparent medical PVC modified material obtained in combination with Example 3 and Comparative Examples 1-2 shows that the mass fraction ratio of trioctyl trimellitate TOTM and diisononyl cyclohexane 1,2-dicarboxylate is 3:1. The synergistic effect between them not only improves the transparency and environmental performance of the PVC material, but also significantly improves the heat resistance, cold resistance and electrical insulation performance of the material through its synergistic effect, while meeting the high standards for safety and stability of medical-grade products.

[0056] 3) The comparative analysis of the performance of the transparent medical PVC modified material prepared in Example 3 and Comparative Example 3 shows that the silane-modified nano talc with a particle size of 10 nm can improve the compatibility of talc with PVC resin, thereby improving the overall performance of the material.

[0057] 4) The performance comparison analysis of the transparent medical PVC modified material obtained in combination with Example 3 and Comparative Examples 4-5 shows that by selecting barium stearate and zinc stearate as heat stabilizers and controlling their molar ratio to 1.7:1, the synergistic effect between them can improve the thermal stability and lubricity of the material. The material has good dispersibility, compatibility and processing fluidity during processing, and the material has excellent thermal stability and high weather resistance.

[0058] The above embodiments are only used to explain the technical solutions of the present application rather than to limit them. Although the above embodiments provide a specific description of the present application, relevant technical personnel should understand that the specific implementation modes of the present invention can still be modified or replaced by equivalents, and any modifications and equivalent replacements that do not depart from the spirit and scope of the present application should be included in the scope of protection of the present application.

Claims

1. A transparent medical PVC modified material, characterized in that: The preparation material comprises the following raw materials by weight: 80-120 parts of PVC resin, 60-100 parts of plasticizer, 1-3 parts of heat stabilizer, 0.5-1.5 parts of lubricant, 10-15 parts of filler, 5-15 parts of impact modifier and 0.01-0.02 parts of anti-yellowing agent, wherein the plasticizer is composed of trioctyl trimellitate TOTM and diisononyl cyclohexane 1,2-dicarboxylate.

2. A transparent medical PVC modified material according to claim 1, characterized in that: The mass ratio of trioctyl trimellitate TOTM to diisononyl cyclohexane 1,2-dicarboxylate is 2-4:

1.

3. A transparent medical PVC modified material according to claim 1, characterized in that: The thermal stabilizer is composed of (RC00)2Ba and (RC00)2Zn in a molar ratio of 1.4-2.2:1, wherein R is C8-C 24 Alkenyl or C6-C 24 The alkenyl group.

4. A transparent medical PVC modified material according to claim 3, characterized in that: The heat stabilizer is composed of barium stearate and zinc stearate in a molar ratio of 1.4-1.8:1; or, the heat stabilizer is composed of barium laurate and zinc laurate in a molar ratio of 1.6-2.0:1; or, the heat stabilizer is composed of barium ricinoleate and zinc ricinoleate in a molar ratio of 1.8-2.2:

1.

5. The transparent medical PVC modified material according to claim 1, characterized in that: The lubricant is composed of liquid paraffin and stearic acid in a mass ratio of 1.2-1.8:

1.

6. The transparent medical PVC modified material according to claim 1, characterized in that: The filler is silane-modified nano-talc powder with a particle size of 2-20 nm.

7. A transparent medical PVC modified material according to claim 6, characterized in that: The preparation method of the silane-modified nano talc powder comprises the following steps: S71, mixing 1 part of γ-(methacryloyloxy)propyltrimethoxysilane with 70 parts of ethanol and 10 parts of water according to their weight proportions, and hydrolyzing for 4 hours to obtain a mixture A; S72, adding 80 parts of nano talc powder to mixture A, then heating to 45°C, stirring at 200 r / min for 200 min, finally centrifugally filtering, washing with ethanol, drying at 80°C, and grinding to obtain silane-modified nano talc powder with a particle size of 2-20 nm.

8. The transparent medical PVC modified material according to claim 1, characterized in that: The impact modifier is a methyl methacrylate-butadiene-styrene terpolymer, wherein the mass content of the methyl methacrylate unit is 40-60%, the mass content of the butadiene unit is 20-30%, and the mass content of the styrene unit is 20-30%.

9. The transparent medical PVC modified material according to claim 1, characterized in that: The anti-yellowing agent is ultramarine powder; and the PVC resin is a PVC resin with a polymerization degree of 1000-1200.

10. A method for preparing a transparent medical PVC modified material according to any one of claims 1 to 9, characterized in that: The following steps are involved: S101, mixing PVC resin, plasticizer, heat stabilizer, lubricant, filler, impact modifier and anti-yellowing agent uniformly according to their weight proportions to obtain a mixture A; S102, the mixture A is placed in a high-speed blender, stirred at a temperature of 100-140 ℃ for 15-25min, to obtain a mixture B; S103, extruding and granulating the mixed material B through a twin-screw extruder to obtain a transparent medical PVC modified material, wherein the screw temperatures of the twin-screw extruder are: zone 1 temperature 138-160°C, zone 2 temperature 135-160°C, zone 3 temperature 135-155°C, zone 4 temperature 132-150°C and zone 5 temperature 130-148°C.

Citation Information

Cited By

  • Environment-friendly calcium-zinc stabilizer for PVC calendering film and preparation method of environment-friendly calcium-zinc stabilizer