Method for improving thermoplasticity of composite board

By preparing plasticizing components and modified fibers, combined with silane coupling agent, a mesh crosslinking structure is formed, which solves the problems of insufficient thermoplastic, mechanical properties and flame retardant properties of composite sheets, and significantly improves its stability at high temperatures and safety performance.

CN118879006AInactive Publication Date: 2024-11-01SHENZHEN QIANHAI TONGYI TECH R & D CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411166552.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional composite sheets have limitations in thermoplastics, mechanical properties and flame retardant properties, and are difficult to meet the strict needs of modern industry.

Method used

Preparing plasticizing components by using choline chloride and xylitol, modifying sepiolite and fibers, combining silane coupling agents, plasticizing polyvinyl chloride, and modifying them by melamine polyphosphate and dopamine hydrochloride nanoferrous tetraoxide to form a mesh crosslinked structure to improve the thermoplastic, mechanical properties and flame retardant properties of composite sheets.

Benefits of technology

The thermoplastic, mechanical properties and flame retardant properties of composite sheets are significantly improved, and their stability and safety performance in high temperature environments are enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005008045470000111
    Figure BDA0005008045470000111
Patent Text Reader

Abstract

The invention relates to the technical field of composite boards, in particular to a method for improving thermoplasticity of a composite board, choline chloride and xylitol are co-melted and then melt-blended with polyvinyl chloride, thermoplasticity of polyvinyl chloride can be improved, choline chloride and xylitol have excellent thermal stability, and when choline chloride and xylitol are added into polyvinyl chloride, the thermoplasticity of the composite board can be improved. According to the present invention, the sepiolite is added to the polyvinyl chloride, such that the stability of the polyvinyl chloride at the high temperature can be improved, the thermal decomposition and degradation phenomena can be reduced, the melting point and the viscosity of the polyvinyl chloride can be reduced, the melting fluidity of the polyvinyl chloride can be improved, and the polyvinyl chloride can be easily molded during the processing process; the sepiolite is added into polyvinyl chloride, the sepiolite is combined with a silane coupling agent KH-560 after the surface property of the sepiolite is improved, the silane coupling agent KH-560 can be used as a bridge molecule, one end of the silane coupling agent KH-560 reacts with hydroxyl on the surface of the sepiolite, the other end of the silane coupling agent KH-560 is combined with a polyvinyl chloride molecular chain, and therefore the interface bonding force between two phases is enhanced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of composite board materials, and in particular to a method for improving the thermoplasticity of a composite board material. Background Art

[0002] With the development of modern industry, composite panels have been widely used in aerospace, construction, automobile manufacturing, electronic and electrical fields due to their excellent comprehensive properties, such as high strength, light weight, and corrosion resistance. However, traditional composite panels still have certain limitations in thermoplasticity, mechanical properties, and flame retardancy, and are difficult to meet the increasingly stringent application requirements. Therefore, it is particularly important to develop a new method that can not only improve the thermoplasticity of composite panels, but also significantly improve their mechanical properties and flame retardancy.

[0003] At present, the preparation of composite panels mainly depends on the composite of resin matrix and fiber reinforcement materials. Although the traditional method can improve certain properties of the panels to a certain extent, it often performs poorly in terms of thermoplasticity, which limits its application in high temperature environments. At the same time, due to the weak interfacial bonding between the resin and the fiber, it is difficult to give full play to the mechanical properties of the composite material. In addition, the flame retardant properties of composite panels are also a major challenge, especially in areas with high safety requirements, such as building fire protection and vehicle interiors. Therefore, how to improve the preparation method of composite panels in the prior art, and improve its mechanical properties and flame retardant properties on the basis of improving the thermoplasticity of the composite panels, has become a technical problem that needs to be solved urgently by those skilled in the art. Summary of the invention

[0004] Technical issues solved

[0005] In view of the above-mentioned shortcomings of the prior art, the present invention provides a method for improving the thermoplasticity of a composite board, which can effectively solve the problems of poor thermoplasticity, mechanical properties and flame retardancy of the composite board in the prior art.

[0006] Technical Solution

[0007] To achieve the above objectives, the present invention is implemented through the following technical solutions:

[0008] A method for improving the thermoplasticity of a composite sheet, the method comprising the following steps:

[0009] S1, firstly preparing a first plasticizing component using choline chloride and xylitol as raw materials, and then modifying sepiolite to prepare a second plasticizing component;

[0010] S2, plasticizing and modifying polyvinyl chloride with a first plasticizing component and a second plasticizing component to prepare plasticized polyvinyl chloride;

[0011] S3, modifying aramid fiber with melamine polyphosphate to prepare modified aramid fiber, and modifying carbon fiber with dopamine hydrochloride and nano-ferroferric oxide to prepare modified carbon fiber;

[0012] S4, the modified aramid fiber and the modified carbon fiber are mixed in an equal weight ratio and recorded as mixed fiber, the mixed fiber and the silane coupling agent solution are mixed in a material-liquid ratio of 3:1 and placed in an oven at 56° C. to dry to constant weight, and the obtained fiber is recorded as enhanced fiber;

[0013] S5. Weigh 180-200g of plasticized polyvinyl chloride and pour it into a mixer. Add 15-18g of diethylenetriamine and 50-80g of enhanced fiber at a temperature of 120°C. After evenly dispersing, place in an oven at 82-85°C for curing for 12 hours to obtain a composite sheet with improved thermoplasticity.

[0014] Furthermore, in S1, the preparation method of the first plasticizer component is: weigh a calculated amount of choline chloride and xylitol according to a molar ratio of 2:1 and pour them into a flask, and stir the reaction at a stirring speed of 200 r / min for 2 hours under an oil bath heating condition of 90°C to obtain the first plasticizer component.

[0015] Furthermore, in S1, the preparation step of the second plasticizing component is:

[0016] Step 3.1, soak the sepiolite in a hydrochloric acid solution with a concentration of 1.5 mol / L for 8 hours, filter out the filtrate after soaking, wash with deionized water for 3 times, dry in an oven at 55°C for 5 hours, grind through a 200-mesh sieve, and the obtained sepiolite is recorded as activated sepiolite;

[0017] Step 3.2, weigh 5-8g of silane coupling agent KH-560 and 200g of deionized water into a flask, stir at a stirring speed of 300r / min for 10min, then add 25-28g of activated sepiolite, stir at the original stirring speed for 5min, then ultrasonically disperse at a frequency of 26-28kHz for 10min, filter to remove the filtrate, and place in an oven at 55°C to dry for 1h, and the result is the second plasticizer component.

[0018] Furthermore, in S2, the preparation steps of the plasticized polyvinyl chloride are:

[0019] Step 4.1, weigh 3-4g of the first plasticizer component and add it to 15g of deionized water, stir at a stirring speed of 200r / min for 10min, then add 4-5g of the second plasticizer component, stir at a stirring speed of 500r / min for 10min, and the result is recorded as a mixed component;

[0020] Step 4.2, weigh 50g of polyvinyl chloride and 12-15g of mixed components, put them in a mixer, mix them at a temperature of 110°C and a stirring speed of 800r / min for 10min, and the obtained product is plasticized polyvinyl chloride.

[0021] Furthermore, in S3, the preparation steps of the modified aramid fiber are:

[0022] Step 5.1, pouring the aramid fiber into the sodium hydroxide solution and soaking it for 30 minutes, filtering out the filtrate and then rinsing it with deionized water until it is neutral, and drying the obtained fiber to be recorded as the pretreated aramid fiber;

[0023] Step 5.2, melamine polyphosphate and deionized water were mixed in a weight ratio of 1:20, and stirred at a stirring speed of 500 r / min for 10 min to obtain a modified solution;

[0024] Step 5.3, heat the modified solution to 80°C and immerse the pretreated aramid fiber, stir at high speed until the modified solution reaches room temperature, then filter and remove the filtrate, dry the obtained solid component at 130°C for 10 minutes, then rinse with deionized water until neutral, and the modified aramid fiber is obtained after drying.

[0025] Furthermore, in step 5.1, the mass fraction of the sodium hydroxide solution is 20%, and the specific operation of the drying treatment is to place it in an oven at 52°C and dry it for 2 hours. In step 5.3, the stirring speed of the high-speed stirring is 600r / min, and the specific operation of the drying treatment is to place it in an oven at 58°C and dry it for 2 hours.

[0026] Furthermore, in S3, the preparation steps of the modified carbon fiber are:

[0027] Step 7.1, soak the carbon fiber in acetone for 24 hours, then rinse it with anhydrous ethanol for 3 times, then soak it in deionized water for 1 hour and ultrasonically disperse it at a frequency of 26 kHz for 10 minutes, filter out the filtrate and dry it, and the obtained carbon fiber is recorded as pretreated carbon fiber;

[0028] Step 7.2, adding the calculated amount of dopamine hydrochloride and nano-ferroferric oxide solution to a Tris-HCl buffer solution with a concentration of 0.02 mol / L and a pH value of 8.5, and mixing them evenly to obtain a sizing solution with a dopamine hydrochloride mass concentration of 2 mg / mL and a nano-ferroferric oxide mass concentration of 1 mg / mL;

[0029] Step 7.3, soak the pretreated carbon fiber in the sizing solution for 12 hours. After the soaking, filter out the filtrate and rinse it with deionized water for 5 times. Then, dry it in an oven at 60°C for 6 hours to obtain the modified carbon fiber.

[0030] Furthermore, in step 7.1, the specific operation of the drying treatment is to place in an oven at 55° C. for 2 hours, and in step 7.2, the specific operation of mixing evenly is to stir at a stirring speed of 300 r / min for 10 minutes.

[0031] Furthermore, in S4, the preparation method of the silane coupling agent solution is: weigh 6-8g of silane coupling agent KH-570, add it into 100g of deionized water, and ultrasonically disperse it at a frequency of 27kHz for 30min to obtain the silane coupling agent solution.

[0032] Furthermore, in S5, the specific operation of uniform dispersion is stirring at a stirring speed of 200 r / min for 10 min.

[0033] Beneficial Effects

[0034] The present invention provides a method for improving the thermoplasticity of a composite plate. Compared with the prior art, the present invention has the following beneficial effects:

[0035] 1. The present invention melts choline chloride and xylitol and then melts and blends them with polyvinyl chloride, which can improve the thermoplasticity of polyvinyl chloride. Choline chloride and xylitol have excellent thermal stability. Adding them to polyvinyl chloride can improve the stability of polyvinyl chloride at high temperatures, reduce thermal decomposition and degradation, and reduce the melting point and viscosity of polyvinyl chloride, improve its melt fluidity, and make polyvinyl chloride easier to shape during processing; secondly, the present invention first places sepiolite in a hydrochloric acid solution for activation, and then combines it with a silane coupling agent KH-560 after its surface properties are improved. Adding the silane coupling agent KH-560 to polyvinyl chloride can make the silane coupling agent KH-560 act as a bridge molecule, one end of which reacts with the hydroxyl group on the surface of the sepiolite and the other end combines with the polyvinyl chloride molecular chain, thereby enhancing the interface bonding force between the two phases. The enhanced interface bonding force helps to improve the overall strength and toughness of the composite board; through the compatibility between the first plasticizing component and the second plasticizing component, the thermoplasticity of the composite board can be further improved.

[0036] 2. The modification of aramid fiber by melamine polyphosphate of the present invention can make the prepared modified aramid fiber have stable flame retardant properties. The carbon fiber is modified by dopamine hydrochloride and nano-ferroferric oxide and then mixed with the modified aramid fiber. The surface of the mixed fiber is then grafted with a silane coupling agent. The fiber with the silane coupling agent grafted on the surface is then added to plasticized polyvinyl chloride to prepare a composite board. The silane coupling agent can be used as an intermediate connecting substance to graft the fiber and the polyvinyl chloride molecules, thereby forming a network cross-linked structure in the composite board. While improving the thermal stability and thermoplasticity of the composite board, the composite board can also have stable flame retardant properties and better mechanical properties. DETAILED DESCRIPTION

[0037] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0038] The present invention will be further described below in conjunction with the embodiments.

[0039] Example 1

[0040] A method for improving the thermoplasticity of a composite plate in this embodiment includes the following steps:

[0041] S1, firstly preparing a first plasticizing component using choline chloride and xylitol as raw materials, and then modifying sepiolite to prepare a second plasticizing component;

[0042] The preparation method of the first plasticizer component is as follows: weigh a calculated amount of choline chloride and xylitol according to a molar ratio of 2:1 and pour them into a flask; stir and react for 2 hours at a stirring speed of 200 r / min under an oil bath heating condition of 90°C to obtain the first plasticizer component.

[0043] The preparation steps of the second plasticizing component are:

[0044] Step 3.1, soak the sepiolite in a hydrochloric acid solution with a concentration of 1.5 mol / L for 8 hours, filter out the filtrate after soaking, wash with deionized water for 3 times, dry in an oven at 55°C for 5 hours, grind through a 200-mesh sieve, and the obtained sepiolite is recorded as activated sepiolite;

[0045] Step 3.2, weigh 5g of silane coupling agent KH-560 and 200g of deionized water into a flask, stir at a stirring speed of 300r / min for 10min, then add 25g of activated sepiolite, stir at the original stirring speed for 5min, and then ultrasonically disperse at a frequency of 26kHz for 10min. After filtering to remove the filtrate, place it in an oven at 55°C and dry it for 1h. The result is the second plasticizer component.

[0046] S2, plasticizing and modifying polyvinyl chloride with a first plasticizing component and a second plasticizing component to prepare plasticized polyvinyl chloride;

[0047] Wherein, the preparation steps of plasticized polyvinyl chloride are:

[0048] Step 4.1, weigh 3 g of the first plasticizer component and add it to 15 g of deionized water, stir at a stirring speed of 200 r / min for 10 min, then add 4 g of the second plasticizer component, stir at a stirring speed of 500 r / min for 10 min, and the result is recorded as a mixed component;

[0049] Step 4.2, weigh 50g of polyvinyl chloride and 12g of mixed components, put them into a mixer, mix them at a temperature of 110°C and a stirring speed of 800r / min for 10min, and the obtained product is plasticized polyvinyl chloride.

[0050] S3, modifying aramid fiber with melamine polyphosphate to prepare modified aramid fiber, and modifying carbon fiber with dopamine hydrochloride and nano-ferroferric oxide to prepare modified carbon fiber;

[0051] Wherein, the preparation steps of modified aramid fiber are:

[0052] Step 5.1, soaking the aramid fiber in a sodium hydroxide solution with a mass fraction of 20% for 30 minutes, filtering out the filtrate, and then rinsing with deionized water until neutral, placing in an oven at 52° C. and drying for 2 hours to obtain the pretreated aramid fiber;

[0053] Step 5.2, melamine polyphosphate and deionized water were mixed in a weight ratio of 1:20, and stirred at a stirring speed of 500 r / min for 10 min to obtain a modified solution;

[0054] Step 5.3, heat the modified solution to 80°C and immerse the pretreated aramid fiber, stir the modified solution at a stirring speed of 600 r / min until it reaches room temperature, then filter and remove the filtrate, dry the obtained solid component at 130°C for 10 min, rinse with deionized water until neutral, and dry it in an oven at 58°C for 2 h to obtain the modified aramid fiber.

[0055] The preparation steps of modified carbon fiber are as follows:

[0056] Step 7.1, soak the carbon fiber in acetone for 24 hours, then rinse it with anhydrous ethanol three times, then soak it in deionized water for 1 hour and ultrasonically disperse it at a frequency of 26 kHz for 10 minutes, filter out the filtrate, and dry it in an oven at 55°C for 2 hours. The obtained carbon fiber is recorded as pretreated carbon fiber;

[0057] Step 7.2, adding the calculated amount of dopamine hydrochloride and nano-ferroferric oxide solution to a Tris-HCl buffer solution with a concentration of 0.02 mol / L and a pH value of 8.5, stirring at a stirring speed of 300 r / min for 10 min to obtain a sizing solution with a dopamine hydrochloride mass concentration of 2 mg / mL and a nano-ferroferric oxide mass concentration of 1 mg / mL;

[0058] Step 7.3, soak the pretreated carbon fiber in the sizing solution for 12 hours. After the soaking, filter out the filtrate and rinse it with deionized water for 5 times. Then, dry it in an oven at 60°C for 6 hours to obtain the modified carbon fiber.

[0059] S4, the modified aramid fiber and the modified carbon fiber are mixed in an equal weight ratio and recorded as mixed fiber, the mixed fiber and the silane coupling agent solution are mixed in a material-liquid ratio of 3:1 and placed in an oven at 56° C. to dry to constant weight, and the obtained fiber is recorded as enhanced fiber;

[0060] The preparation method of the silane coupling agent solution is as follows: 6 g of silane coupling agent KH-570 is weighed and added into 100 g of deionized water, and ultrasonically dispersed at a frequency of 27 kHz for 30 minutes to obtain the silane coupling agent solution.

[0061] S5. Weigh 180g of plasticized polyvinyl chloride and pour it into a mixer. Add 15g of diethylenetriamine and 50g of reinforcing fiber at a temperature of 120°C. Stir at a stirring speed of 200r / min for 10min and then place in an oven at 82°C for curing for 12h. The result is a composite board with improved thermoplasticity.

[0062] Example 2

[0063] A method for improving the thermoplasticity of a composite plate in this embodiment includes the following steps:

[0064] S1, firstly preparing a first plasticizing component using choline chloride and xylitol as raw materials, and then modifying sepiolite to prepare a second plasticizing component;

[0065] The preparation method of the first plasticizer component is as follows: weigh a calculated amount of choline chloride and xylitol according to a molar ratio of 2:1 and pour them into a flask; stir and react for 2 hours at a stirring speed of 200 r / min under an oil bath heating condition of 90°C to obtain the first plasticizer component.

[0066] The preparation steps of the second plasticizing component are:

[0067] Step 3.1, soak the sepiolite in a hydrochloric acid solution with a concentration of 1.5 mol / L for 8 hours, filter out the filtrate after soaking, wash with deionized water for 3 times, dry in an oven at 55°C for 5 hours, grind through a 200-mesh sieve, and the obtained sepiolite is recorded as activated sepiolite;

[0068] Step 3.2, weigh 8g of silane coupling agent KH-560 and 200g of deionized water into a flask, stir at a stirring speed of 300r / min for 10min, then add 28g of activated sepiolite, stir at the original stirring speed for 5min, and then ultrasonically disperse at a frequency of 28kHz for 10min. After filtering to remove the filtrate, place it in an oven at 55°C and dry it for 1h. The result is the second plasticizer component.

[0069] S2, plasticizing and modifying polyvinyl chloride with a first plasticizing component and a second plasticizing component to prepare plasticized polyvinyl chloride;

[0070] Wherein, the preparation steps of plasticized polyvinyl chloride are:

[0071] Step 4.1, weigh 4 g of the first plasticizer component and add it to 15 g of deionized water, stir at a stirring speed of 200 r / min for 10 min, then add 5 g of the second plasticizer component, stir at a stirring speed of 500 r / min for 10 min, and the result is recorded as a mixed component;

[0072] Step 4.2, weigh 50g of polyvinyl chloride and 15g of mixed components, put them into a mixer, mix them at a temperature of 110°C and a stirring speed of 800r / min for 10min, and the obtained product is plasticized polyvinyl chloride.

[0073] S3, modifying aramid fiber with melamine polyphosphate to prepare modified aramid fiber, and modifying carbon fiber with dopamine hydrochloride and nano-ferroferric oxide to prepare modified carbon fiber;

[0074] Wherein, the preparation steps of modified aramid fiber are:

[0075] Step 5.1, soaking the aramid fiber in a sodium hydroxide solution with a mass fraction of 20% for 30 minutes, filtering out the filtrate, and then rinsing with deionized water until neutral, placing in an oven at 52° C. and drying for 2 hours to obtain the pretreated aramid fiber;

[0076] Step 5.2, melamine polyphosphate and deionized water were mixed in a weight ratio of 1:20, and stirred at a stirring speed of 500 r / min for 10 min to obtain a modified solution;

[0077] Step 5.3, heat the modified solution to 80°C and immerse the pretreated aramid fiber, stir the modified solution at a stirring speed of 600 r / min until it reaches room temperature, then filter and remove the filtrate, dry the obtained solid component at 130°C for 10 min, rinse with deionized water until neutral, and dry it in an oven at 58°C for 2 h to obtain the modified aramid fiber.

[0078] The preparation steps of modified carbon fiber are as follows:

[0079] Step 7.1, soak the carbon fiber in acetone for 24 hours, then rinse it with anhydrous ethanol three times, then soak it in deionized water for 1 hour and ultrasonically disperse it at a frequency of 26 kHz for 10 minutes, filter out the filtrate, and dry it in an oven at 55°C for 2 hours. The obtained carbon fiber is recorded as pretreated carbon fiber;

[0080] Step 7.2, adding the calculated amount of dopamine hydrochloride and nano-ferroferric oxide solution to a Tris-HCl buffer solution with a concentration of 0.02 mol / L and a pH value of 8.5, stirring at a stirring speed of 300 r / min for 10 min to obtain a sizing solution with a dopamine hydrochloride mass concentration of 2 mg / mL and a nano-ferroferric oxide mass concentration of 1 mg / mL;

[0081] Step 7.3, soak the pretreated carbon fiber in the sizing solution for 12 hours. After the soaking, filter out the filtrate and rinse it with deionized water for 5 times. Then, dry it in an oven at 60°C for 6 hours to obtain the modified carbon fiber.

[0082] S4, the modified aramid fiber and the modified carbon fiber are mixed in an equal weight ratio and recorded as mixed fiber, the mixed fiber and the silane coupling agent solution are mixed in a material-liquid ratio of 3:1 and placed in an oven at 56° C. to dry to constant weight, and the obtained fiber is recorded as enhanced fiber;

[0083] The preparation method of the silane coupling agent solution is as follows: 8 g of silane coupling agent KH-570 is weighed and added into 100 g of deionized water, and ultrasonically dispersed at a frequency of 27 kHz for 30 minutes to obtain the silane coupling agent solution.

[0084] S5. Weigh 200g of plasticized polyvinyl chloride and pour it into a mixer. Add 18g of diethylenetriamine and 80g of enhanced fiber at a temperature of 120°C. Stir at a stirring speed of 200r / min for 10min and then place in an oven at 85°C for curing for 12h. The result is a composite plate with improved thermoplasticity.

[0085] Example 3

[0086] A method for improving the thermoplasticity of a composite plate in this embodiment includes the following steps:

[0087] S1, firstly preparing a first plasticizing component using choline chloride and xylitol as raw materials, and then modifying sepiolite to prepare a second plasticizing component;

[0088] The preparation method of the first plasticizer component is as follows: weigh a calculated amount of choline chloride and xylitol according to a molar ratio of 2:1 and pour them into a flask; stir and react for 2 hours at a stirring speed of 200 r / min under an oil bath heating condition of 90°C to obtain the first plasticizer component.

[0089] The preparation steps of the second plasticizing component are:

[0090] Step 3.1, soak the sepiolite in a hydrochloric acid solution with a concentration of 1.5 mol / L for 8 hours, filter out the filtrate after soaking, wash with deionized water for 3 times, dry in an oven at 55°C for 5 hours, grind through a 200-mesh sieve, and the obtained sepiolite is recorded as activated sepiolite;

[0091] Step 3.2, weigh 7g of silane coupling agent KH-560 and 200g of deionized water into a flask, stir at a stirring speed of 300r / min for 10min, then add 26g of activated sepiolite, stir at the original stirring speed for 5min, and then ultrasonically disperse at a frequency of 27kHz for 10min. After filtering to remove the filtrate, place it in an oven at 55°C and dry it for 1h. The result is the second plasticizer component.

[0092] S2, plasticizing and modifying polyvinyl chloride with a first plasticizing component and a second plasticizing component to prepare plasticized polyvinyl chloride;

[0093] Wherein, the preparation steps of plasticized polyvinyl chloride are:

[0094] Step 4.1, weigh 4 g of the first plasticizer component and add it to 15 g of deionized water, stir at a stirring speed of 200 r / min for 10 min, then add 5 g of the second plasticizer component, stir at a stirring speed of 500 r / min for 10 min, and the result is recorded as a mixed component;

[0095] Step 4.2, weigh 50g of polyvinyl chloride and 14g of mixed components, put them into a mixer, mix them at a temperature of 110°C and a stirring speed of 800r / min for 10min, and the obtained product is plasticized polyvinyl chloride.

[0096] S3, modifying aramid fiber with melamine polyphosphate to prepare modified aramid fiber, and modifying carbon fiber with dopamine hydrochloride and nano-ferroferric oxide to prepare modified carbon fiber;

[0097] Wherein, the preparation steps of modified aramid fiber are:

[0098] Step 5.1, soaking the aramid fiber in a sodium hydroxide solution with a mass fraction of 20% for 30 minutes, filtering out the filtrate, and then rinsing with deionized water until neutral, placing in an oven at 52° C. and drying for 2 hours to obtain the pretreated aramid fiber;

[0099] Step 5.2, melamine polyphosphate and deionized water were mixed in a weight ratio of 1:20, and stirred at a stirring speed of 500 r / min for 10 min to obtain a modified solution;

[0100] Step 5.3, heat the modified solution to 80°C and immerse the pretreated aramid fiber, stir the modified solution at a stirring speed of 600 r / min until it reaches room temperature, then filter and remove the filtrate, dry the obtained solid component at 130°C for 10 min, rinse with deionized water until neutral, and dry it in an oven at 58°C for 2 h to obtain the modified aramid fiber.

[0101] The preparation steps of modified carbon fiber are as follows:

[0102] Step 7.1, soak the carbon fiber in acetone for 24 hours, then rinse it with anhydrous ethanol three times, then soak it in deionized water for 1 hour and ultrasonically disperse it at a frequency of 26 kHz for 10 minutes, filter out the filtrate, and dry it in an oven at 55°C for 2 hours. The obtained carbon fiber is recorded as pretreated carbon fiber;

[0103] Step 7.2, adding the calculated amount of dopamine hydrochloride and nano-ferroferric oxide solution to a Tris-HCl buffer solution with a concentration of 0.02 mol / L and a pH value of 8.5, stirring at a stirring speed of 300 r / min for 10 min to obtain a sizing solution with a dopamine hydrochloride mass concentration of 2 mg / mL and a nano-ferroferric oxide mass concentration of 1 mg / mL;

[0104] Step 7.3, soak the pretreated carbon fiber in the sizing solution for 12 hours. After the soaking, filter out the filtrate and rinse it with deionized water for 5 times. Then, dry it in an oven at 60°C for 6 hours to obtain the modified carbon fiber.

[0105] S4, the modified aramid fiber and the modified carbon fiber are mixed in an equal weight ratio and recorded as mixed fiber, the mixed fiber and the silane coupling agent solution are mixed in a material-liquid ratio of 3:1 and placed in an oven at 56° C. to dry to constant weight, and the obtained fiber is recorded as enhanced fiber;

[0106] The preparation method of the silane coupling agent solution is as follows: 7 g of silane coupling agent KH-570 is weighed and added into 100 g of deionized water, and ultrasonically dispersed at a frequency of 27 kHz for 30 minutes to obtain the silane coupling agent solution.

[0107] S5. Weigh 190g of plasticized polyvinyl chloride and pour it into a mixer. Add 17g of diethylenetriamine and 70g of reinforcing fiber at a temperature of 120°C. Stir at a stirring speed of 200r / min for 10min and then place in an oven at 83°C for curing for 12h. The result is a composite plate with improved thermoplasticity.

[0108] Comparative Example 1

[0109] The method for improving the thermoplasticity of a composite board provided in this comparative example is substantially the same as that in Example 1, the main difference is that in this comparative example 1, the first plasticizing component in Example 1 is replaced with deionized water.

[0110] Comparative Example 2

[0111] The method for improving the thermoplasticity of a composite board provided in this comparative example is substantially the same as that in Example 1, the main difference being that in this comparative example 2, the second plasticizing component in Example 1 is replaced with unmodified sepiolite.

[0112] Comparative Example 3

[0113] The method for improving the thermoplasticity of a composite board provided in this comparative example is substantially the same as that in Example 1, the main difference being that in this comparative example 3, the reinforcing fiber in Example 1 is replaced with glass fiber.

[0114] Performance Testing

[0115] The composite plates with improved thermoplasticity in Examples 1-3 and Comparative Examples 1-3 are marked as Example 1, Example 2, Example 3, Comparative Example 1, Comparative Example 2 and Comparative Example 3, respectively, and then the performances of Examples 1-3 and Comparative Examples 1-3 are tested, and the specific testing methods and test items are as follows.

[0116] 1. The thermal decomposition temperature, melting point and melt mass flow rate of the composite plates with improved thermoplasticity in Examples 1-3 and Comparative Examples 1-3 were tested, and the obtained data were recorded in Table 1;

[0117] 2. The mechanical properties and flame retardant properties of the composite plates with improved thermoplasticity in Examples 1-3 and Comparative Examples 1-3 were tested, and the obtained data are recorded in Table 2.

[0118] Table 1

[0119]

[0120] Table 2

[0121] Tensile strength(MPa) <![CDATA[Impact strength (KJ / m 2 )]]> Limiting oxygen index (%) Testing standards GB / T1049-92 GB / T1043-93 ASTMD2863 Example 1 48.7 9.3 27.3 Example 2 48.1 9.1 27.5 Example 3 47.9 9.5 27.1 Comparative Example 1 46.2 9.1 25.3 Comparative Example 2 46.1 9.3 25.8 Comparative Example 3 45.7 9.7 20.2

[0122] The data in Table 1 show that the composite sheet with improved thermoplasticity in Examples 1-3 has better thermal decomposition stability and lower melting point, indicating that the composite sheet with improved thermoplasticity in Examples 1-3 has better thermal stability and better thermoplasticity than Comparative Examples 1-3. The data in Table 2 show that the composite sheet with improved thermoplasticity in Examples 1-3 has better mechanical properties and better flame retardant properties. In summary, a method for improving the thermoplasticity of a composite sheet in the present invention can improve the mechanical properties and flame retardant properties of the composite sheet on the basis of improving the thermoplasticity of the composite sheet, and has excellent market promotion value.

[0123] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.

[0124] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements will not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for improving the thermoplasticity of a composite sheet, characterized in that: The method comprises the following steps: S1, firstly preparing a first plasticizing component using choline chloride and xylitol as raw materials, and then modifying sepiolite to prepare a second plasticizing component; S2, plasticizing and modifying polyvinyl chloride with a first plasticizing component and a second plasticizing component to prepare plasticized polyvinyl chloride; S3, modifying aramid fiber with melamine polyphosphate to prepare modified aramid fiber, and modifying carbon fiber with dopamine hydrochloride and nano-ferroferric oxide to prepare modified carbon fiber; S4, the modified aramid fiber and the modified carbon fiber are mixed in an equal weight ratio and recorded as mixed fiber, the mixed fiber and the silane coupling agent solution are mixed in a material-liquid ratio of 3:1 and placed in an oven at 56° C. to dry to constant weight, and the obtained fiber is recorded as enhanced fiber; S5. Weigh 180-200g of plasticized polyvinyl chloride and pour it into a mixer. Add 15-18g of diethylenetriamine and 50-80g of enhanced fiber at a temperature of 120°C. After evenly dispersing, place in an oven at 82-85°C for curing for 12 hours to obtain a composite sheet with improved thermoplasticity.

2. A method for improving the thermoplasticity of a composite sheet according to claim 1, characterized in that: In S1, the preparation method of the first plasticizer component is: weighing a calculated amount of choline chloride and xylitol according to a molar ratio of 2:1 and pouring them into a flask, stirring and reacting them at a stirring speed of 200 r / min for 2 hours under an oil bath heating condition of 90°C, and the obtained product is the first plasticizer component.

3. The method for improving the thermoplasticity of a composite sheet according to claim 1, characterized in that: In S1, the preparation steps of the second plasticizing component are: Step 3.1, soaking the sepiolite in a hydrochloric acid solution with a concentration of 1.5 mol / L for 8 hours, filtering out the filtrate after soaking, washing with deionized water for 3 times, drying in an oven at 55° C. for 5 hours, and grinding through a 200-mesh sieve, the obtained sepiolite is recorded as activated sepiolite; Step 3.2, weigh 5-8g of silane coupling agent KH-560 and 200g of deionized water into a flask, stir at a stirring speed of 300r / min for 10min, then add 25-28g of activated sepiolite, stir at the original stirring speed for 5min, then ultrasonically disperse at a frequency of 26-28kHz for 10min, filter to remove the filtrate, and place in an oven at 55°C to dry for 1h, and the result is the second plasticizer component.

4. A method for improving the thermoplasticity of a composite sheet according to claim 1, characterized in that: In S2, the preparation steps of the plasticized polyvinyl chloride are: Step 4.1, weigh 3-4g of the first plasticizer component and add it to 15g of deionized water, stir at a stirring speed of 200r / min for 10min, then add 4-5g of the second plasticizer component, stir at a stirring speed of 500r / min for 10min, and the result is recorded as a mixed component; Step 4.2, weigh 50g of polyvinyl chloride and 12-15g of mixed components, put them in a mixer, mix them at a temperature of 110°C and a stirring speed of 800r / min for 10min, and the obtained product is plasticized polyvinyl chloride.

5. The method for improving the thermoplasticity of a composite sheet according to claim 1, characterized in that: In S3, the preparation steps of the modified aramid fiber are: Step 5.1, pouring the aramid fiber into the sodium hydroxide solution and soaking it for 30 minutes, filtering out the filtrate and then rinsing it with deionized water until it is neutral, and drying the obtained fiber to be recorded as the pretreated aramid fiber; Step 5.2, melamine polyphosphate and deionized water were mixed in a weight ratio of 1:20, and stirred at a stirring speed of 500 r / min for 10 min to obtain a modified solution; Step 5.3, heat the modified solution to 80°C and immerse the pretreated aramid fiber, stir at high speed until the modified solution reaches room temperature, then filter and remove the filtrate, dry the obtained solid component at 130°C for 10 minutes, then rinse with deionized water until neutral, and the modified aramid fiber is obtained after drying.

6. A method for improving the thermoplasticity of a composite sheet according to claim 5, characterized in that: In step 5.1, the mass fraction of the sodium hydroxide solution is 20%, and the specific operation of the drying treatment is to place it in an oven at 52°C for 2 hours. In step 5.3, the stirring speed of the high-speed stirring is 600r / min, and the specific operation of the drying treatment is to place it in an oven at 58°C for 2 hours.

7. The method for improving the thermoplasticity of a composite sheet according to claim 1, characterized in that: In S3, the preparation steps of the modified carbon fiber are: Step 7.1, soak the carbon fiber in acetone for 24 hours, then rinse it with anhydrous ethanol for 3 times, then soak it in deionized water for 1 hour and ultrasonically disperse it at a frequency of 26 kHz for 10 minutes, filter out the filtrate and dry it, and the obtained carbon fiber is recorded as pretreated carbon fiber; Step 7.2, adding calculated amounts of dopamine hydrochloride and nano-ferroferric oxide solution to a Tris-HCl buffer solution having a concentration of 0.02 mol / L and a pH value of 8.5, and mixing them evenly to obtain a sizing solution having a dopamine hydrochloride mass concentration of 2 mg / mL and a nano-ferroferric oxide mass concentration of 1 mg / mL; Step 7.3, soak the pretreated carbon fiber in the sizing solution for 12 hours. After the soaking, filter out the filtrate and rinse it with deionized water for 5 times. Then, dry it in an oven at 60°C for 6 hours to obtain the modified carbon fiber.

8. A method for improving the thermoplasticity of a composite sheet according to claim 7, characterized in that: In step 7.1, the specific operation of the drying treatment is to place the mixture in an oven at 55° C. for 2 hours, and in step 7.2, the specific operation of the mixing treatment is to stir the mixture at a stirring speed of 300 r / min for 10 minutes.

9. The method for improving the thermoplasticity of a composite sheet according to claim 1, characterized in that: In S4, the silane coupling agent solution is prepared by weighing 6-8 g of silane coupling agent KH-570 and adding it into 100 g of deionized water, and ultrasonically dispersing it at a frequency of 27 kHz for 30 minutes to obtain the silane coupling agent solution.

10. The method for improving the thermoplasticity of a composite sheet according to claim 1, characterized in that: In S5, the specific operation of uniform dispersion is stirring at a stirring speed of 200 r / min for 10 min.

Citation Information

Patent Citations

  • Carbon fiber filled and modified polyvinyl chloride plastic and preparation method thereof

    CN104861359A

  • Antistatic PVC board composition

    CN107459727A

  • Polyvinyl chloride wood-plastic flame retardance composite plate and preparation method

    CN109161121A

  • Method for fiber-reinforced modified wood-plastic decorative plate

    CN110092970A