Breathable acrylate composition, preparation method and application

Through the coordinated design of modified acrylate copolymer and modified magnesium silicate, the problems of complex preparation and poor breathability of VAP unidirectional breathable membrane materials are solved, high-strength and uniform microporous structure are achieved, and the application performance of breathable membranes is improved. .

CN118879013APending Publication Date: 2024-11-01ZHEJIANG YOUWEI NEW MATERIAL
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410959668.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The semi-permeable membrane materials of existing VAP unidirectional breathable membranes are complex in preparation, inconvenient to separate from the product, poor ductility, prone to tearing and breakage, and the agglomeration of fill particles leads to poor pore size uniformity, low breathability, and difficult to use.

Method used

Provided is a breathable composition including a modified acrylate copolymer, a modified magnesium silicate, pigment, additive and crosslinking agent, and the formation of tiny holes during the structural design and crosslinking process of the modified acrylate copolymer is improved. The tensile strength and pore uniformity of the material, combined with the dispersion of modified magnesium silicate, form an appropriate microporous structure to improve breathability and mechanical properties.

Benefits of technology

It significantly improves the tensile strength and breathability of the breathable membrane, forms a tight microporous structure, ensures that gas with a smaller molecular structure passes through and prevents the penetration of the ester liquid, and improves the mechanical properties and application convenience of the membrane.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118879013A_ABST
    Figure CN118879013A_ABST
Patent Text Reader

Abstract

The invention provides a breathable acrylate composition as well as a preparation method and application thereof. The composition is prepared from the following components in parts by mass: 50 to 80 parts of modified acrylate copolymer, 10 to 20 parts of modified magnesium silicate, 1 to 10 parts of pigment, 0.01 to 2 parts of auxiliary agent and 0.03 to 0.05 part of cross-linking agent. Acrylate copolymer resin is modified to improve the tensile strength and tensile elasticity of the resin, magnesium silicate is modified to enhance the dispersity of the magnesium silicate, and the acrylate copolymer resin and the magnesium silicate cooperate to enable the resin to be elastically recovered in the film preparation process and form uniform holes with proper sizes, so that the defects that an existing breathable film is poor in ester resistance and breathability and poor in breathability are overcome. Or the mechanical property is poor.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, and in particular to a breathable acrylate composition, a preparation method and application thereof. Background Art

[0002] VAP one-way breathable membrane is a material that can block resin and allow gas to pass through. The product consists of two parts: base cloth and semi-permeable membrane. It is used in the "vacuum introduction resin" process and "wet vacuum bag forming process". VAP one-way breathable membrane can continuously extract air and volatiles to prevent the loss of resin in the laminate.

[0003] The semi-permeable membrane is the main breathable and ester-blocking membrane on the VAP one-way breathable membrane. This breathable isolation membrane is a high-tech breathable isolation resin membrane with micropores on the surface of the substrate that can pass gas but prevent resin from passing through by adopting a special resin material formula and advanced production technology. The micropores can only allow gas molecules with smaller molecular structures to pass through, but cannot allow ester liquid in a state of aggregation to penetrate through, so it has the characteristics of being breathable but not ester-permeable, thus achieving the role of separation.

[0004] Currently, the semipermeable membranes prepared by stretching high-filled inorganic and organic particles on the market still have problems such as easy agglomeration of the filled particles, poor uniformity of the pore size of the breathable membrane due to uneven particle size distribution of the filled particles, poor compatibility of the filled particles with the matrix resin resulting in reduced film strength, and uneven dispersion of the filled particles resulting in color difference or color spots on the breathable membrane.

[0005] Chinese patent CN103739962A discloses a polyolefin microporous breathable membrane and a preparation method thereof; the microporous breathable membrane is made of a polyolefin substrate filled with a surface-treated calcium carbonate filler, and is made by cast extrusion, stretching, and heat-setting film-forming processes. During preparation, polyolefin and surface-treated calcium carbonate filler are blended, extruded, and granulated to obtain breathable particles. However, the breathable membrane obtained by the patent has relatively poor tensile strength and low air permeability, and it is difficult to apply it to VAP one-way breathable membranes. Chinese invention patent CN113248776A discloses a waterproof and oil-proof breathable membrane with super-amphiphobic function. The waterproof and breathable membrane prepared by this method has excellent waterproof and oil-proof properties, but the patent does not involve the mechanical properties of the super-amphiphobic coating, which is also crucial for the practical application of VAP one-way breathable membranes. Summary of the invention

[0006] In order to solve the problems in the prior art that the semi-permeable membrane material used in the VAP one-way breathable membrane is complicated to prepare, inconvenient to separate from the product, has general ductility, and is prone to tearing and breakage, the present invention provides a breathable acrylate composition, a preparation method and an application to improve the above problems.

[0007] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0008] In one aspect, the present invention provides a breathable acrylate composition; the composition comprises, by weight:

[0009] 50-80 parts of modified acrylate copolymer, 10-20 parts of modified magnesium silicate, 1-10 parts of pigment, 0.01-2 parts of auxiliary agent and 0.03-0.05 parts of crosslinking agent.

[0010] In some embodiments, further preferably, the composition comprises:

[0011] 70-80 parts of modified acrylate copolymer, 15-20 parts of modified magnesium silicate, 1-10 parts of pigment, 0.01-2 parts of auxiliary agent and 0.03-0.05 parts of crosslinking agent.

[0012] In some embodiments, the structural formula of the modified acrylate copolymer is as shown in Formula 1:

[0013]

[0014] Wherein, m is any integer from 4 to 12; n is any integer from 1 to 6; and * is a repeating unit connection site.

[0015] Furthermore, m is any integer from 10 to 12; and n is any integer from 3 to 5.

[0016] The tensile stress and other conditions of the acrylic copolymers in the existing market cannot meet the requirements of the VAP one-way breathable membrane. During the stretching process, incomplete stretching or excessive stretching deformation will affect the size of the micropores, thereby affecting the diameter of the particles passing through the breathable membrane. The modified acrylic copolymer provided by the present invention has a carbon six-membered ring and a boron element in its structure, which can significantly improve the tensile strength of the material, and the modified acrylic copolymer is self-crosslinked by a crosslinking agent, leaving tiny holes during the crosslinking process, so that the VAP one-way breathable membrane is compact, and only gas molecules with smaller molecular structures can pass through, but ester liquids in an aggregated state cannot penetrate through, achieving a better separation effect.

[0017] In some embodiments, the preparation method of the modified acrylate copolymer comprises:

[0018] Step 1: Trimethylheptanediol is reacted with allyl bromide to obtain intermediate 1;

[0019] Step 2: react intermediate 1 with boric acid to obtain intermediate 2;

[0020] Step 3: polymerize the intermediate 2 and acrylate to obtain a modified acrylate copolymer.

[0021] In some embodiments, the method for preparing the modified magnesium silicate comprises:

[0022] After the modifier is mixed with the ball-milled hydroxy magnesium silicate powder, anhydrous ethanol is added, and magnetic stirring is performed under heating conditions until the anhydrous ethanol is completely evaporated to obtain modified magnesium silicate.

[0023] In some embodiments, the modified magnesium silicate can improve the dispersibility and detachability of magnesium silicate in the composition, and is convenient for separation from the resin matrix during stretching to form micropores. Optionally, the modifier is selected from one or more combinations of oleic acid, stearic acid, KH560, hexadecyltrimethylammonium bromide (CTAB), hexadecylpyridinium bromide (CPB) and octadecylamine (ODA); preferably, the modifier is one or more combinations of CTAB, CPB and ODA.

[0024] In some embodiments, the auxiliary agent is a leveling agent and a defoaming agent. The leveling agent is an organic silicon leveling agent, for example, one or more combinations selected from TEGO-100, 410, 411, 415, 435, 432, 440, 450, 482, B1484, 300, 370; the defoaming agent is a polyether siloxane copolymer defoaming agent, for example, one or more combinations selected from TEGO-800, 805, 810, 815, 825.

[0025] In a second aspect, the present invention also provides a method for preparing the breathable acrylate composition as described above, which specifically comprises:

[0026] Step 1: weigh the raw materials modified acrylate copolymer, modified magnesium silicate, pigment, and 3 / 4 of the additives according to the formula, mix and stir evenly to obtain an emulsion, and set aside;

[0027] Step 2: After emulsification is completed, 3 / 4 of the emulsion is released, and the remaining 1 / 4 of the emulsion is polymerized with a cross-linking agent for seed polymerization, and the temperature is controlled at 80-90°C for reaction until blue light appears and there is basically no reflux;

[0028] Step 3: Add the remaining 3 / 4 of the emulsion dropwise to the solution obtained in step 2. After the addition is complete, keep the mixture at 80-95° C. for 0.5-1 h to obtain an acrylate composition.

[0029] In a third aspect, the present invention also provides use of the breathable acrylate composition described above in a VAP process.

[0030] Beneficial effects:

[0031] The invention improves the mechanical properties of the resin by modifying the acrylic copolymer resin and making the modified acrylic copolymer resin self-crosslinked through a crosslinking agent, leaving tiny holes in the crosslinking process; at the same time, magnesium silicate is modified to enhance the dispersibility of magnesium silicate, and the two cooperate to enable the resin to elastically recover during the film-making process and form uniform holes of appropriate size, thereby improving the problems of poor anti-ester air permeability or poor mechanical properties of existing breathable films. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] The present invention is further described below with reference to the accompanying drawings:

[0033] Figure 1 This is a SEM electron microscope image of the film product prepared from the acrylic acid ester composition obtained in Example 1. DETAILED DESCRIPTION

[0034] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.

[0035] Unless otherwise specified, the chemical reagents used in the present invention are all commercially available analytically pure.

[0036] Preparation of modified magnesium silicate-Span 80

[0037] After mixing 5 g of Span 80 and 5 g of ball-milled magnesium silicate hydroxy powder, 30 ml of anhydrous ethanol was added, ultrasonic oscillation was performed for 50 min, and stirring was performed at a constant temperature of 80° C. for 1 h. The anhydrous ethanol was completely evaporated to obtain the modified magnesium silicate-Span 80.

[0038] Preparation of modified magnesium silicate-oleic acid

[0039] The preparation method of modified magnesium silicate-oleic acid is similar to that of modified magnesium silicate-Span 80, except that oleic acid is used instead of Span 80.

[0040] Preparation of modified magnesium silicate-CTAB

[0041] The preparation method of modified magnesium silicate-CTAB refers to the preparation method of modified magnesium silicate-Span 80, the only difference is that CTAB is used instead of Span 80.

[0042] Preparation of modified acrylate copolymer-1

[0043] Step 1: Take 1 mol of trimethylheptanediol and 1.1 mol of propylene bromide, add them into 70 ml of dimethylformamide, then add 0.05 mol of potassium carbonate, heat to 80°C and react for 3 hours to obtain a DMF solution of intermediate 1;

[0044] Step 2: Add 1.1 mol of boric acid to the DMF solution of the intermediate 1, heat to 50°C for 5 hours, and obtain the intermediate 2 through extraction, recrystallization, washing and drying.

[0045] The obtained products were analyzed by LC-MS, and the m / z of the products were 268.18 (100.0%), 268.00 (41.1%), and 268.74 (5.4%), confirming that intermediate 2 was successfully obtained.

[0046] Step 3: Add 1 mol of intermediate 2 and 12 mol of acrylate into a reactor, then add 0.1 mol of benzoyl peroxide, heat to 110° C. for polymerization reaction, and obtain modified acrylate copolymer-1.

[0047] Preparation of modified acrylate copolymer-2

[0048] The preparation method of modified acrylate copolymer-2 is similar to that of modified acrylate copolymer-1, except that the added molar amounts of intermediate 2 and acrylate are 6 mol and 4 mol, respectively.

[0049] Preparation of modified acrylate copolymer-3

[0050] The preparation method of modified acrylate copolymer-3 is similar to that of modified acrylate copolymer-1, except that the added molar amounts of intermediate 2 and acrylate are 5 mol and 10 mol, respectively.

[0051] Preparation of modified acrylate copolymer-4

[0052] The preparation method of modified acrylate copolymer-4 is similar to that of modified acrylate copolymer-1, except that the added molar amount of boric acid is 0 mol.

[0053] Preparation of Acrylate Copolymer-5

[0054] Commercially available acrylic acid-ethylene copolymers.

[0055] Example

[0056] Step 1: weigh the raw materials modified acrylate copolymer, modified magnesium silicate, pigment, and 3 / 4 of the additives according to the formula described in Table 1, mix and stir evenly to obtain an emulsion, and set aside;

[0057] Step 2: After emulsification is completed, 3 / 4 of the emulsion is released, and the remaining 1 / 4 of the emulsion is polymerized with a cross-linking agent for seed polymerization, and the temperature is controlled at 80°C for reaction until blue light appears and there is almost no reflux;

[0058] Step 3: Add the remaining 3 / 4 of the emulsion dropwise to the solution obtained in step 2. After the addition is complete, keep the mixture at 90° C. for 1 hour to obtain an acrylate composition.

[0059] Table 1 Example formula table (unit: mass parts)

[0060] Material S1 S2 S3 S4 S5 S6 Modified acrylate copolymer 1 50 70 80 0 0 70 Modified acrylate copolymer 2 0 0 0 70 0 0 Modified acrylate copolymer 3 0 0 0 0 70 0 Modified magnesium silicate-oleic acid 0 0 0 0 0 15 Modified magnesium silicate-CTAB 20 15 10 15 15 0 Pigment (Titanium Dioxide) 10 10 10 10 10 10 Leveling agent (TEGO-100) 1 1 1 1 1 1 Defoaming agent (TEGO-800) 0.5 0.5 0.5 0.5 0.5 0.5 Initiator (p-toluenesulfonic acid) 0.03 0.03 0.03 0.03 0.03 0.03

[0061] Note: In the above table, "S" represents an embodiment, such as "S1" represents embodiment 1.

[0062] Comparative Example

[0063] The preparation steps of the comparative example are the same as those of the embodiment, except that the raw material formula of the comparative example is shown in Table 2.

[0064] Table 2 Comparative Example Formula Table (Unit: mass parts)

[0065]

[0066]

[0067] Note: In the above table, "D" means comparative example, such as "D1" means comparative example 1.

[0068] The acrylic ester composition prepared above was rolled into a film product with a length of 30 times the diameter and a thickness of 50 μm on a double screw extruder. After the film was quickly air-cooled by a film blowing machine, an eight-roller differential longitudinal stretching process was used, with the temperature of the preheating roller 1 being 40°C, the temperature of the preheating roller 2 being 50°C, the temperature of the stretching roller 1 being set to 80°C, and the temperature of the stretching roller 2 being set to 100 degrees; the temperature of the annealing roller 1 being set to 60°C, the temperature of the annealing roller 2 being set to 50°C, the stretching speed being 30 m / min, the stretching ratio being 3.3, and the film was stretched to 12 gsm. The above film was tested, and the test results are shown in Table 3.

[0069] 1. SEM: The film product prepared from the acrylic acid ester composition of Example 1 was subjected to SEM electron microscope analysis, and the results obtained are as follows: Figure 1 shown.

[0070] 2. Water vapor transmission rate: The water vapor transmission rate is measured by the electrolytic sensor method (GB / T21529-2008) (ASTM F-1249-90). Instrument: American ILLINOIS water vapor transmission rate tester; The specific test steps are: clamp the pre-treated sample between the test chambers, and the nitrogen with stable relative humidity flows on one side of the film, and the dry nitrogen flows on the other side of the film. Due to the existence of humidity gradient, water vapor will diffuse from the high humidity side through the film to the low humidity side. On the low humidity side, the permeated water vapor is carried to the sensor by the flowing dry nitrogen. When entering the sensor, an electrical signal of the same proportion will be generated. The water vapor transmission rate of the sample is obtained by analyzing and calculating the sensor electrical signal.

[0071] 3. Tensile strength and elongation at break: The film was cut into 10 mm × 10 mm squares and the mechanical properties were tested using an ASTM Standard D882 tensile analyzer with a tension increase rate of 0.2 N / min to obtain the tensile strength MPa and elongation at break (%).

[0072] Table 3 Test results

[0073]

[0074]

[0075] It can be seen from the SEM image of Example 1 that the membrane product provided by the present invention has uniformly dispersed micropores of uniform size, with a micropore diameter of 13-27 μm, and is suitable for use as a fat-blocking breathable film.

[0076] It can be seen from the test data in Table 3 that by modifying the structure of the acrylate copolymer and adding a carbon hexagonal ring structure and boron elements, the tensile strength and elongation at break of the material can be significantly improved, so that the film product has the characteristics of compactness and high strength during use; and by modifying the surface of the filler magnesium silicate, the magnesium silicate is dispersed more evenly, which is also convenient for separation from the resin matrix during the stretching process, resulting in regular and uniform pores.

[0077] The selection of modifiers also has certain requirements. From the data in Table 3, it can be seen that the air permeability of the membrane product prepared by using Span 80 as a modifier is significantly reduced. This may be because Span 80 has hydroxyl groups, which will form chemical bonds with the resin matrix during the film formation process, affecting the stretching and pore formation process.

[0078] At the same time, it can be seen from the comparison between the examples and the comparative examples that the filler magnesium silicate and the polyacrylate copolymer are modified at the same time, the obtained membrane product has better air permeability and better mechanical properties.

[0079] The present invention can also have many other embodiments. Without departing from the spirit and essence of the present invention, those skilled in the art can make various corresponding changes and modifications based on the present invention, but these corresponding changes and modifications should all fall within the scope of protection of the claims attached to the present invention.

Claims

1. A breathable acrylic composition, characterized in that: In parts by mass, the composition comprises: 70-80 parts of modified acrylate copolymer, 10-20 parts of modified magnesium silicate, 1-10 parts of pigment, 0.01-2 parts of auxiliary agent and 0.03-0.05 parts of crosslinking agent.

2. The acrylate composition according to claim 1, characterized in that: The composition comprises, by weight, 50-80 parts of modified acrylate copolymer, 15-20 parts of modified magnesium silicate, 1-10 parts of pigment, 0.01-2 parts of auxiliary agent and 0.03-0.05 parts of crosslinking agent.

3. The acrylate composition according to claim 1, characterized in that: The structural formula of the modified acrylate copolymer is shown in Formula 1: Wherein, m is any integer from 4 to 12; n is any integer from 1 to 6; and * is a repeating unit connection site.

4. The acrylate composition according to claim 1, characterized in that: The preparation method of the modified acrylate copolymer comprises: Step 1: Trimethylheptanediol is reacted with allyl bromide to obtain intermediate 1; Step 2: react intermediate 1 with boric acid to obtain intermediate 2; Step 3: polymerize the intermediate 2 and acrylate to obtain a modified acrylate copolymer.

5. The acrylate composition according to claim 1, characterized in that: The preparation method of the modified magnesium silicate comprises: After the modifier is mixed with the ball-milled hydroxy magnesium silicate powder, anhydrous ethanol is added, and magnetic stirring is performed under heating conditions until the anhydrous ethanol is completely evaporated to obtain modified magnesium silicate.

6. The acrylate composition according to claim 5, characterized in that: The modifier is selected from one or more combinations of oleic acid, stearic acid, KH560, hexadecyltrimethylammonium bromide, hexadecylpyridinium bromide and octadecylamine.

7. The acrylate composition according to claim 1, characterized in that: The auxiliary agent is a leveling agent and a defoaming agent; the leveling agent is selected from one or more combinations of TEGO-100, 410, 411, 415, 435, 432, 440, 450, 482, B1484, 300, and 370; the defoaming agent is selected from one or more combinations of TEGO-800, 805, 810, 815, and 825.

8. The method for preparing the acrylic acid ester composition according to any one of claims 1 to 7, characterized in that: include: Step 1: weigh the raw materials modified acrylate copolymer, modified magnesium silicate, pigment, and 3 / 4 of the additives according to the formula, mix and stir evenly to obtain an emulsion, and set aside; Step 2: After emulsification is completed, 3 / 4 of the emulsion is released, and the remaining 1 / 4 of the emulsion is polymerized with a cross-linking agent for seed polymerization, and the temperature is controlled at 80-90°C for reaction until blue light appears and there is basically no reflux; Step 3: Add the remaining 3 / 4 of the emulsion dropwise to the solution obtained in step 2. After the addition is complete, keep the mixture at 80-95° C. for 0.5-1 h to obtain an acrylate composition.

9. Use of a film product of the acrylic acid ester composition according to any one of claims 1 to 7 in a VAP process.

Citation Information

Patent Citations

  • Air-permeable film composition and preparation method thereof

    CN107955258A

  • Method of modifying polymer barrier films

    CN113874580A

  • Single-layer integral waterproof breathable film

    CN116829345A

  • Breathable flame-retardant acrylic sealant and preparation method thereof

    CN117866557A

  • Multilayer breathable microporous film with reinforced impermeability to liquids and production method

    US20040170852A1