Biodegradable plastic film as well as preparation method and application thereof
Through the combination of polylactic acid, polycaprolactone, polyglylactide and lanthanum modified calcium carbonate, the double-helix extruder and hot-press film formation process are used to solve the problem of insufficient mechanical properties and biodegradability of polylactic acid films. It significantly improves tensile strength and biodegradability, and is suitable for food packaging and agriculture.
Patent Information
- Application Number
- CN202411124172.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-01
AI Technical Summary
The lack of flexibility, low impact strength, poor elongation at break and slow biodegradation rate of polylactic acid plastic films limits its application in some fields.
Using the combination of polylactic acid, polycaprolactone, polyglylactide and lanthanum modified calcium carbonate, biodegradable plastic film is prepared through the melt extrusion granulation and hot pressing film formation process of double helix extruder, and the molar ratio is optimized. , reaction and calcination conditions to improve mechanical properties and biodegradability.
The tensile strength and elongation of breaking of plastic film are significantly improved, and the biodegradability is improved. The weight loss rate in 10 days reaches 5.7%, the weight loss rate in 20 days reaches 15.8%, the weight loss rate in 40 days reaches 31.7%, and the weight loss rate in 80 days reaches 67.8%. , surpassing the performance of ordinary PLA films.
Smart Images

Figure BDA0004995896010000121 
Figure BDA0004995896010000131
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of plastic films, and in particular to a biodegradable plastic film and a preparation method and application thereof. Background Art
[0002] At present, the problem of plastic pollution has attracted great attention. In addition to reducing the generation of waste and strengthening the recycling of plastic waste, the development of biodegradable plastics is considered to be one of the effective ways to solve the problem of plastic pollution. Among the many biodegradable polymer materials, polylactic acid (PLA) has become the focus of research due to its unique properties. Polylactic acid has good biocompatibility and biodegradability, which makes it have a wide range of application prospects in packaging, textiles, medical and other fields. However, polylactic acid also has some shortcomings, such as its insufficient flexibility, low impact strength, low elongation at break, etc. More importantly, the biodegradation rate of polylactic acid is relatively slow. Under natural conditions, polylactic acid can only degrade by about 20% within 80 days. These problems seriously limit its application in some fields. In view of this, a new polylactic acid film with good mechanical properties and biodegradability is provided, which is expected to expand the application of polylactic acid film and meet the market demand for environmentally friendly materials. Summary of the invention
[0003] The purpose of the present invention is to provide a biodegradable plastic film and a preparation method and application thereof. The plastic film has good mechanical properties and biodegradability and can be widely used in the fields of food preservation and agriculture.
[0004] To achieve the above object, the present invention provides the following technical solutions:
[0005] One of the technical solutions of the present invention:
[0006] A biodegradable plastic film comprises the following raw materials: 60% to 80% of polylactic acid, 15% to 5% of polycaprolactone, 15% to 5% of polyglycolide, and 10% of lanthanum-modified calcium carbonate;
[0007] Preferably, the biodegradable plastic film comprises the following raw materials: 70% polylactic acid, 10% polycaprolactone, 10% polyglycolide, and 10% lanthanum-modified calcium carbonate.
[0008] Furthermore, the preparation method of the lanthanum-modified calcium carbonate comprises the following steps:
[0009] 1) adding calcium carbonate, lanthanum chloride and calcium hydroxide into deionized water to react and obtain lanthanum hydroxide-calcium carbonate precipitate;
[0010] 2) calcining the lanthanum hydroxide-calcium carbonate precipitate obtained in step 1) to obtain a lanthanum oxide-calcium carbonate precipitate, i.e., the lanthanum-modified calcium carbonate.
[0011] Furthermore, in step 1), the molar ratio of calcium carbonate, lanthanum chloride and calcium hydroxide is (3-5):1:1.2;
[0012] Preferably, the molar ratio of calcium carbonate, lanthanum chloride and calcium hydroxide is 4:1:1.2.
[0013] Furthermore, in step 1), the reaction is carried out at 40 to 60° C. for 10 to 30 minutes;
[0014] Preferably, in step 1), the reaction is carried out at 50° C. for 20 min.
[0015] Furthermore, in step 2), the calcination treatment is calcined at 280-320° C. for 1.5-2.5 h;
[0016] Preferably, in step 2), the calcination treatment is performed at 300° C. for 2 h.
[0017] The second technical solution of the present invention:
[0018] The method for preparing the above-mentioned biodegradable plastic film comprises the following steps:
[0019] The biodegradable plastic film is obtained by mixing polylactic acid, polycaprolactone, polyglycolide and lanthanum-modified calcium carbonate, melting and extruding to form granules, and hot pressing to form a film.
[0020] Furthermore, the melt extrusion granulation is carried out by using a twin-screw extruder.
[0021] Furthermore, the temperature of the feed port of the twin-screw extruder is 50-80°C, the temperature of the screw is 230-250°C, and the temperature of the discharge port is 250-260°C.
[0022] Furthermore, the temperature of the hot pressing film forming is 250-260°C and the pressure is 50-70MPa;
[0023] Preferably, the pressure of the hot pressing film forming is 62 MPa.
[0024] The third technical solution of the present invention:
[0025] The above biodegradable plastic film is used in the fields of food packaging and agriculture.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] The biodegradable plastic film prepared by the present invention has excellent tensile strength and elongation at break, wherein the tensile strength can reach 54.2 MPa and the elongation at break can reach 6.1%, which are significantly improved compared with ordinary PLA films.
[0028] The biodegradable plastic film prepared by the present invention has excellent biodegradability, and its 10-day weight loss rate can reach 5.7%, the 20-day weight loss rate can reach 15.8%, the 40-day weight loss rate can reach 31.7%, and the 80-day weight loss rate can reach 67.8%, which is significantly improved compared with ordinary PLA films. DETAILED DESCRIPTION
[0029] Now, various exemplary embodiments of the present invention are described in detail, and this detailed description should not be considered as a limitation of the present invention, but should be understood as a more detailed description of certain aspects, characteristics and embodiments of the present invention. It should be understood that the terms described in the present invention are only for describing specific embodiments and are not used to limit the present invention.
[0030] In addition, for the numerical range in the present invention, it is understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0031] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0032] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.
[0033] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0034] In the following embodiments, a method for preparing a biodegradable plastic film comprises the following steps:
[0035] 1) adding calcium carbonate, lanthanum chloride and calcium hydroxide into deionized water in a molar ratio of (3-5) : 1 : 1.2, reacting at 40-60° C. for 10-30 min to obtain a lanthanum hydroxide-calcium carbonate precipitate;
[0036] 2) calcining the lanthanum hydroxide-calcium carbonate precipitate obtained in step 1) at 280-320° C. for 1.5-2.5 h to obtain a lanthanum oxide-calcium carbonate precipitate, i.e., lanthanum-modified calcium carbonate;
[0037] 3) According to 60% to 80% of polylactic acid, 15% to 5% of polycaprolactone, 15% to 5% of polyglycolide, and 10% of lanthanum-modified calcium carbonate, polylactic acid, polycaprolactone, polyglycolide and lanthanum-modified calcium carbonate are mixed, and melt-extruded and granulated by a twin-screw extruder to obtain a biodegradable plastic film masterbatch;
[0038] Among them, the feed port temperature of the twin-screw extruder is 50-80°C, the screw temperature is 230-250°C, and the discharge port temperature is 250-260°C;
[0039] 4) The biodegradable plastic film masterbatch obtained in step 3) is hot-pressed into a film at a temperature of 250-260° C. and a pressure of 50-70 MPa to obtain the biodegradable plastic film.
[0040] Example 1
[0041] A biodegradable plastic film
[0042] 1) adding calcium carbonate, lanthanum chloride and calcium hydroxide into deionized water in a molar ratio of 4:1:1.2, reacting at 50° C. for 20 min to obtain a lanthanum hydroxide-calcium carbonate precipitate;
[0043] 2) calcining the lanthanum hydroxide-calcium carbonate precipitate obtained in step 1) at 300° C. for 2 h to obtain a lanthanum oxide-calcium carbonate precipitate, i.e., lanthanum-modified calcium carbonate;
[0044] 3) According to 60% of polylactic acid, 15% of polycaprolactone, 15% of polyglycolide and 10% of lanthanum-modified calcium carbonate, polylactic acid, polycaprolactone, polyglycolide and lanthanum-modified calcium carbonate are mixed, and melt-extruded and granulated by a twin-screw extruder to obtain a biodegradable plastic film masterbatch;
[0045] Among them, the feed port temperature of the twin-screw extruder is 65°C, the screw temperature is 240°C, and the discharge port temperature is 255°C;
[0046] 4) The biodegradable plastic film masterbatch obtained in step 3) is hot-pressed into a film at a temperature of 255° C. and a pressure of 62 MPa to obtain the biodegradable plastic film.
[0047] Example 2
[0048] A biodegradable plastic film
[0049] 1) adding calcium carbonate, lanthanum chloride and calcium hydroxide into deionized water in a molar ratio of 4:1:1.2, reacting at 50° C. for 20 min to obtain a lanthanum hydroxide-calcium carbonate precipitate;
[0050] 2) calcining the lanthanum hydroxide-calcium carbonate precipitate obtained in step 1) at 300° C. for 2 h to obtain a lanthanum oxide-calcium carbonate precipitate, i.e., lanthanum-modified calcium carbonate;
[0051] 3) According to 70% of polylactic acid, 10% of polycaprolactone, 10% of polyglycolide and 10% of lanthanum-modified calcium carbonate, polylactic acid, polycaprolactone, polyglycolide and lanthanum-modified calcium carbonate are mixed, and melt-extruded and granulated by a twin-screw extruder to obtain a biodegradable plastic film masterbatch;
[0052] Among them, the feed port temperature of the twin-screw extruder is 65°C, the screw temperature is 240°C, and the discharge port temperature is 255°C;
[0053] 4) The biodegradable plastic film masterbatch obtained in step 3) is hot-pressed into a film at a temperature of 255° C. and a pressure of 62 MPa to obtain the biodegradable plastic film.
[0054] Example 3
[0055] A biodegradable plastic film
[0056] 1) adding calcium carbonate, lanthanum chloride and calcium hydroxide into deionized water in a molar ratio of 4:1:1.2, reacting at 50° C. for 20 min to obtain a lanthanum hydroxide-calcium carbonate precipitate;
[0057] 2) calcining the lanthanum hydroxide-calcium carbonate precipitate obtained in step 1) at 300° C. for 2 h to obtain a lanthanum oxide-calcium carbonate precipitate, i.e., lanthanum-modified calcium carbonate;
[0058] 3) According to 80% of polylactic acid, 5% of polycaprolactone, 5% of polyglycolide and 10% of lanthanum-modified calcium carbonate, polylactic acid, polycaprolactone, polyglycolide and lanthanum-modified calcium carbonate are mixed, and melt-extruded and granulated by a twin-screw extruder to obtain a biodegradable plastic film masterbatch;
[0059] Among them, the feed port temperature of the twin-screw extruder is 65°C, the screw temperature is 240°C, and the discharge port temperature is 255°C;
[0060] 4) The biodegradable plastic film masterbatch obtained in step 3) is hot-pressed into a film at a temperature of 255° C. and a pressure of 62 MPa to obtain the biodegradable plastic film.
[0061] Example 4
[0062] A biodegradable plastic film
[0063] 1) adding calcium carbonate, lanthanum chloride and calcium hydroxide into deionized water in a molar ratio of 4:1:1.2, reacting at 50° C. for 20 min to obtain a lanthanum hydroxide-calcium carbonate precipitate;
[0064] 2) calcining the lanthanum hydroxide-calcium carbonate precipitate obtained in step 1) at 300° C. for 2 h to obtain a lanthanum oxide-calcium carbonate precipitate, i.e., lanthanum-modified calcium carbonate;
[0065] 3) According to 70% of polylactic acid, 10% of polycaprolactone, 10% of polyglycolide and 10% of lanthanum-modified calcium carbonate, polylactic acid, polycaprolactone, polyglycolide and lanthanum-modified calcium carbonate are mixed, and melt-extruded and granulated by a twin-screw extruder to obtain a biodegradable plastic film masterbatch;
[0066] Among them, the feed port temperature of the twin-screw extruder is 65°C, the screw temperature is 240°C, and the discharge port temperature is 255°C;
[0067] 4) The biodegradable plastic film masterbatch obtained in step 3) is hot-pressed into a film at a temperature of 255° C. and a pressure of 50 MPa to obtain the biodegradable plastic film.
[0068] Example 5
[0069] A biodegradable plastic film
[0070] 1) adding calcium carbonate, lanthanum chloride and calcium hydroxide into deionized water in a molar ratio of 4:1:1.2, reacting at 50° C. for 20 min to obtain a lanthanum hydroxide-calcium carbonate precipitate;
[0071] 2) calcining the lanthanum hydroxide-calcium carbonate precipitate obtained in step 1) at 300° C. for 2 h to obtain a lanthanum oxide-calcium carbonate precipitate, i.e., lanthanum-modified calcium carbonate;
[0072] 3) According to 70% of polylactic acid, 10% of polycaprolactone, 10% of polyglycolide and 10% of lanthanum-modified calcium carbonate, polylactic acid, polycaprolactone, polyglycolide and lanthanum-modified calcium carbonate are mixed, and melt-extruded and granulated by a twin-screw extruder to obtain a biodegradable plastic film masterbatch;
[0073] Among them, the feed port temperature of the twin-screw extruder is 65°C, the screw temperature is 240°C, and the discharge port temperature is 255°C;
[0074] 4) The biodegradable plastic film masterbatch obtained in step 3) is hot-pressed into a film at a temperature of 255° C. and a pressure of 70 MPa to obtain the biodegradable plastic film.
[0075] Example 6
[0076] A biodegradable plastic film
[0077] 1) adding calcium carbonate, lanthanum chloride and calcium hydroxide into deionized water in a molar ratio of 3:1:1.2, reacting at 50° C. for 20 min to obtain a lanthanum hydroxide-calcium carbonate precipitate;
[0078] 2) calcining the lanthanum hydroxide-calcium carbonate precipitate obtained in step 1) at 300° C. for 2 h to obtain a lanthanum oxide-calcium carbonate precipitate, i.e., lanthanum-modified calcium carbonate;
[0079] 3) According to 70% of polylactic acid, 10% of polycaprolactone, 10% of polyglycolide and 10% of lanthanum-modified calcium carbonate, polylactic acid, polycaprolactone, polyglycolide and lanthanum-modified calcium carbonate are mixed, and melt-extruded and granulated by a twin-screw extruder to obtain a biodegradable plastic film masterbatch;
[0080] Among them, the feed port temperature of the twin-screw extruder is 65°C, the screw temperature is 240°C, and the discharge port temperature is 255°C;
[0081] 4) The biodegradable plastic film masterbatch obtained in step 3) is hot-pressed into a film at a temperature of 255° C. and a pressure of 62 MPa to obtain the biodegradable plastic film.
[0082] Example 7
[0083] A biodegradable plastic film
[0084] 1) adding calcium carbonate, lanthanum chloride and calcium hydroxide into deionized water in a molar ratio of 5:1:1.2, reacting at 50° C. for 20 min to obtain a lanthanum hydroxide-calcium carbonate precipitate;
[0085] 2) calcining the lanthanum hydroxide-calcium carbonate precipitate obtained in step 1) at 300° C. for 2 h to obtain a lanthanum oxide-calcium carbonate precipitate, i.e., lanthanum-modified calcium carbonate;
[0086] 3) According to 70% of polylactic acid, 10% of polycaprolactone, 10% of polyglycolide and 10% of lanthanum-modified calcium carbonate, polylactic acid, polycaprolactone, polyglycolide and lanthanum-modified calcium carbonate are mixed, and melt-extruded and granulated by a twin-screw extruder to obtain a biodegradable plastic film masterbatch;
[0087] Among them, the feed port temperature of the twin-screw extruder is 65°C, the screw temperature is 240°C, and the discharge port temperature is 255°C;
[0088] 4) The biodegradable plastic film masterbatch obtained in step 3) is hot-pressed into a film at a temperature of 255° C. and a pressure of 62 MPa to obtain the biodegradable plastic film.
[0089] Comparative Example 1
[0090] A biodegradable plastic film
[0091] 1) adding calcium carbonate, lanthanum chloride and calcium hydroxide into deionized water in a molar ratio of 4:1:1.2, reacting at 50° C. for 20 min to obtain a lanthanum hydroxide-calcium carbonate precipitate;
[0092] 2) calcining the lanthanum hydroxide-calcium carbonate precipitate obtained in step 1) at 300° C. for 2 h to obtain a lanthanum oxide-calcium carbonate precipitate, i.e., lanthanum-modified calcium carbonate;
[0093] 3) According to 70% of polylactic acid, 20% of polyglycolide and 10% of lanthanum-modified calcium carbonate, polylactic acid, polyglycolide and lanthanum-modified calcium carbonate are mixed, and melt-extruded and granulated by a twin-screw extruder to obtain a biodegradable plastic film masterbatch;
[0094] Among them, the feed port temperature of the twin-screw extruder is 65°C, the screw temperature is 240°C, and the discharge port temperature is 255°C;
[0095] 4) The biodegradable plastic film masterbatch obtained in step 3) is hot-pressed into a film at a temperature of 255° C. and a pressure of 62 MPa to obtain the biodegradable plastic film.
[0096] Comparative Example 2
[0097] A biodegradable plastic film
[0098] 1) adding calcium carbonate, lanthanum chloride and calcium hydroxide into deionized water in a molar ratio of 4:1:1.2, reacting at 50° C. for 20 min to obtain a lanthanum hydroxide-calcium carbonate precipitate;
[0099] 2) calcining the lanthanum hydroxide-calcium carbonate precipitate obtained in step 1) at 300° C. for 2 h to obtain a lanthanum oxide-calcium carbonate precipitate, i.e., lanthanum-modified calcium carbonate;
[0100] 3) According to 70% of polylactic acid, 20% of polycaprolactone and 10% of lanthanum-modified calcium carbonate, polylactic acid, polycaprolactone and lanthanum-modified calcium carbonate are mixed, and melt-extruded and granulated by a twin-screw extruder to obtain a biodegradable plastic film masterbatch;
[0101] Among them, the feed port temperature of the twin-screw extruder is 65°C, the screw temperature is 240°C, and the discharge port temperature is 255°C;
[0102] 4) The biodegradable plastic film masterbatch obtained in step 3) is hot-pressed into a film at a temperature of 255° C. and a pressure of 62 MPa to obtain the biodegradable plastic film.
[0103] Comparative Example 3
[0104] A biodegradable plastic film
[0105] 1) According to 70% of polylactic acid, 15% of polycaprolactone and 15% of polyglycolide, polylactic acid, polycaprolactone and polyglycolide are mixed, and melt-extruded and granulated by a twin-screw extruder to obtain a biodegradable plastic film masterbatch;
[0106] Among them, the feed port temperature of the twin-screw extruder is 65°C, the screw temperature is 240°C, and the discharge port temperature is 255°C;
[0107] 2) The biodegradable plastic film masterbatch obtained in step 1) is hot-pressed into a film at a temperature of 255° C. and a pressure of 62 MPa to obtain the biodegradable plastic film.
[0108] Comparative Example 4
[0109] A biodegradable plastic film
[0110] 1) adding calcium carbonate, lanthanum chloride and calcium hydroxide into deionized water in a molar ratio of 4:1:1.2, reacting at 30° C. for 20 min to obtain a lanthanum hydroxide-calcium carbonate precipitate;
[0111] 2) calcining the lanthanum hydroxide-calcium carbonate precipitate obtained in step 1) at 300° C. for 2 h to obtain a lanthanum oxide-calcium carbonate precipitate, i.e., lanthanum-modified calcium carbonate;
[0112] 3) According to 70% of polylactic acid, 10% of polycaprolactone, 10% of polyglycolide and 10% of lanthanum-modified calcium carbonate, polylactic acid, polycaprolactone, polyglycolide and lanthanum-modified calcium carbonate are mixed, and melt-extruded and granulated by a twin-screw extruder to obtain a biodegradable plastic film masterbatch;
[0113] Among them, the feed port temperature of the twin-screw extruder is 65°C, the screw temperature is 240°C, and the discharge port temperature is 255°C;
[0114] 4) The biodegradable plastic film masterbatch obtained in step 3) is hot-pressed into a film at a temperature of 255° C. and a pressure of 62 MPa to obtain the biodegradable plastic film.
[0115] Comparative Example 5
[0116] A biodegradable plastic film
[0117] 1) adding calcium carbonate, lanthanum chloride and calcium hydroxide into deionized water in a molar ratio of 4:1:1.2, reacting at 70° C. for 20 min to obtain a lanthanum hydroxide-calcium carbonate precipitate;
[0118] 2) calcining the lanthanum hydroxide-calcium carbonate precipitate obtained in step 1) at 300° C. for 2 h to obtain a lanthanum oxide-calcium carbonate precipitate, i.e., lanthanum-modified calcium carbonate;
[0119] 3) According to 70% of polylactic acid, 10% of polycaprolactone, 10% of polyglycolide and 10% of lanthanum-modified calcium carbonate, polylactic acid, polycaprolactone, polyglycolide and lanthanum-modified calcium carbonate are mixed, and melt-extruded and granulated by a twin-screw extruder to obtain a biodegradable plastic film masterbatch;
[0120] Among them, the feed port temperature of the twin-screw extruder is 65°C, the screw temperature is 240°C, and the discharge port temperature is 255°C;
[0121] 4) The biodegradable plastic film masterbatch obtained in step 3) is hot-pressed into a film at a temperature of 255° C. and a pressure of 62 MPa to obtain the biodegradable plastic film.
[0122] Comparative Example 6
[0123] A biodegradable plastic film
[0124] 1) adding calcium carbonate, lanthanum chloride and calcium hydroxide into deionized water in a molar ratio of 4:1:1.2, reacting at 50° C. for 20 min to obtain a lanthanum hydroxide-calcium carbonate precipitate;
[0125] 2) calcining the lanthanum hydroxide-calcium carbonate precipitate obtained in step 1) at 250° C. for 2 h to obtain a lanthanum oxide-calcium carbonate precipitate, i.e., lanthanum-modified calcium carbonate;
[0126] 3) According to 70% of polylactic acid, 10% of polycaprolactone, 10% of polyglycolide and 10% of lanthanum-modified calcium carbonate, polylactic acid, polycaprolactone, polyglycolide and lanthanum-modified calcium carbonate are mixed, and melt-extruded and granulated by a twin-screw extruder to obtain a biodegradable plastic film masterbatch;
[0127] Among them, the feed port temperature of the twin-screw extruder is 65°C, the screw temperature is 240°C, and the discharge port temperature is 255°C;
[0128] 4) The biodegradable plastic film masterbatch obtained in step 3) is hot-pressed into a film at a temperature of 255° C. and a pressure of 62 MPa to obtain the biodegradable plastic film.
[0129] Comparative Example 7
[0130] A biodegradable plastic film
[0131] 1) adding calcium carbonate, lanthanum chloride and calcium hydroxide into deionized water in a molar ratio of 4:1:1.2, reacting at 50° C. for 20 min to obtain a lanthanum hydroxide-calcium carbonate precipitate;
[0132] 2) calcining the lanthanum hydroxide-calcium carbonate precipitate obtained in step 1) at 350° C. for 2 h to obtain a lanthanum oxide-calcium carbonate precipitate, i.e., lanthanum-modified calcium carbonate;
[0133] 3) According to 70% of polylactic acid, 10% of polycaprolactone, 10% of polyglycolide and 10% of lanthanum-modified calcium carbonate, polylactic acid, polycaprolactone, polyglycolide and lanthanum-modified calcium carbonate are mixed, and melt-extruded and granulated by a twin-screw extruder to obtain a biodegradable plastic film masterbatch;
[0134] Among them, the feed port temperature of the twin-screw extruder is 65°C, the screw temperature is 240°C, and the discharge port temperature is 255°C;
[0135] 4) The biodegradable plastic film masterbatch obtained in step 3) is hot-pressed into a film at a temperature of 255° C. and a pressure of 62 MPa to obtain the biodegradable plastic film.
[0136] Effect verification
[0137] 1. Mechanical properties
[0138] According to GB / T1040.3-2006, the tensile strength and elongation at break of the biodegradable plastic films prepared in Examples 1 to 7 and Comparative Examples 1 to 7 were tested, and the test results are shown in Table 1;
[0139] Table 1 Mechanical properties
[0140] Tensile strength / MPa Elongation at break / % Tensile strength / MPa Elongation at break / % Example 1 53.7 5.8 Comparative Example 1 45.9 5.2 Example 2 54.2 6.1 Comparative Example 2 46.2 5.3 Example 3 53.8 5.9 Comparative Example 3 42.5 4.5 Example 4 49.7 5.6 Comparative Example 4 48.5 5.1 Example 5 51.1 5.4 Comparative Example 5 48.1 4.9 Example 6 52.5 5.5 Comparative Example 6 47.8 4.7 Example 7 52.1 5.7 Comparative Example 7 48.3 5.2
[0141] It can be seen from the data in Table 1 that the biodegradable plastic film prepared by the present invention has excellent tensile strength and elongation at break, and its tensile strength can reach 54.2MPa, and its elongation at break can reach 6.1%, which is significantly improved compared with ordinary PLA film (tensile strength of about 40MPa, elongation at break of about 4%);
[0142] It can be seen from Examples 1 to 7 and Comparative Examples 1 to 7 that changing the proportion of polylactic acid, polycaprolactone and polyglycolide in the biodegradable plastic film, changing the pressure of hot pressing film forming, omitting the addition of polycaprolactone, polyglycolide or lanthanum-modified calcium carbonate, changing the molar ratio of calcium carbonate, lanthanum chloride and calcium hydroxide, changing the reaction temperature and calcination temperature when preparing lanthanum-modified calcium carbonate, will all reduce the mechanical properties of the biodegradable plastic film to a certain extent.
[0143] 2. Biodegradability
[0144] According to GB / T19811-2005, the biodegradable plastic films prepared in Examples 1 to 7 and Comparative Examples 1 to 7 were subjected to a simulated soil burial degradation experiment, and the weight loss rates at different times were detected. The test results are shown in Table 2.
[0145] Table 2 Biodegradability
[0146]
[0147]
[0148] It can be seen from the data in Table 2 that the biodegradable plastic film prepared by the present invention has excellent biodegradability, and its 10d weight loss rate can reach 5.7%, 20d weight loss rate can reach 15.8%, 40d weight loss rate can reach 31.7%, and 80d weight loss rate can reach 67.8%, which is significantly improved compared with ordinary PLA film (10d weight loss rate is about 3%, 20d weight loss rate is about 5%, 40d weight loss rate is about 10%, and 80d weight loss rate is about 20%).
[0149] It can be seen from Examples 1 to 7 and Comparative Examples 1 to 7 that changing the proportion of polylactic acid, polycaprolactone and polyglycolide in the biodegradable plastic film, changing the pressure of hot pressing film forming, omitting the addition of polycaprolactone, polyglycolide or lanthanum-modified calcium carbonate, changing the molar ratio of calcium carbonate, lanthanum chloride and calcium hydroxide, changing the reaction temperature and calcination temperature when preparing lanthanum-modified calcium carbonate, will all reduce the biodegradability of the biodegradable plastic film to a certain extent.
[0150] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the specific implementation methods of the present invention can still be modified or replaced by equivalents. Any modification or equivalent replacement that does not depart from the spirit and scope of the present invention should be covered within the scope of protection of the claims of the present invention.
Claims
1. A biodegradable plastic film, characterized in that: The invention comprises the following raw materials: 60% to 80% of polylactic acid, 15% to 5% of polycaprolactone, 15% to 5% of polyglycolide and 10% of lanthanum-modified calcium carbonate.
2. A biodegradable plastic film according to claim 1, characterized in that: The preparation method of the lanthanum-modified calcium carbonate comprises the following steps: 1) adding calcium carbonate, lanthanum chloride and calcium hydroxide into deionized water to react and obtain lanthanum hydroxide-calcium carbonate precipitate; 2) calcining the lanthanum hydroxide-calcium carbonate precipitate obtained in step 1) to obtain a lanthanum oxide-calcium carbonate precipitate, i.e., the lanthanum-modified calcium carbonate.
3. A biodegradable plastic film according to claim 2, characterized in that: In step 1), the molar ratio of calcium carbonate, lanthanum chloride and calcium hydroxide is (3-5):1:1.
2.
4. A biodegradable plastic film according to claim 2, characterized in that: In step 1), the reaction is carried out at 40-60° C. for 10-30 min.
5. The biodegradable plastic film according to claim 2, characterized in that: In step 2), the calcination treatment is performed at 280-320° C. for 1.5-2.5 h.
6. A method for preparing a biodegradable plastic film according to any one of claims 1 to 5, characterized in that: The following steps are involved: Polylactic acid, polycaprolactone, polyglycolide and lanthanum-modified calcium carbonate are mixed, melt-extruded into granules, and hot-pressed into films to obtain the biodegradable plastic film.
7. The preparation method according to claim 6, characterized in that: The melt extrusion granulation is carried out by using a twin-screw extruder.
8. The preparation method according to claim 7, characterized in that: The temperature of the feed port of the twin-screw extruder is 50-80°C, the temperature of the screw is 230-250°C, and the temperature of the discharge port is 250-260°C.
9. The preparation method according to claim 6, characterized in that: The temperature of the hot pressing film forming is 250-260° C., and the pressure is 50-70 MPa.
10. Use of the biodegradable plastic film according to any one of claims 1 to 5 in the field of food packaging and agriculture.