Polylactic acid-based foaming material and preparation method thereof
By adding polybutylene terephthalate and epoxy chain extender to the PLA foaming material, the problem of cell collapse caused by insufficient melt strength of PLA is solved, and polylactic acid-based foaming material is realized The efficient preparation of the material improves the melt flow rate and cell density.
Patent Information
- Application Number
- CN202411388228.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-08
- Publication Date
- 2024-11-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Low melt strength of PLA at high temperatures leads to problems of cell collapse and merger during foaming.
Using the combination of polylactic acid, polyadipate, butylene terephthalate, chain extender, foaming agent and nucleating agent, the polylactic acid-based foaming material prepared by the hot pressing foaming process, adjusting the polylactic acid and Mass ratio of polyadipate butylene terephthalate and epoxy chain extenders such as Joncryl ADR-4370F are used to improve melt flow rate and solution strength.
The average diameter and density of the cell of polylactic acid-based foaming material are optimized, which avoids cell collapse and merger, and improves the foamability and compatibility of the material.
Smart Images

Figure CN118879052A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of foam material preparation, and in particular to a polylactic acid-based foam material and a preparation method thereof. Background Art
[0002] Polylactic acid (PLA) is a biodegradable thermoplastic polymer obtained by polycondensation of lactic acid or ring-opening polymerization of lactide, and is derived from renewable resources such as corn, potatoes, and sugar cane. Polymer foaming technology can reduce the weight of materials, save raw material resources, and give materials sound insulation, heat insulation, cushioning and other properties. Since PLA is a linear polymer polyester with high rigidity and high tensile strength, PLA foam has been studied in recent years as a replacement for traditional polymer foam.
[0003] However, the melt strength of PLA decreases sharply with increasing temperature, which causes the collapse and merging of PLA cells during the foaming process. Therefore, improving the melt strength characteristics of PLA is crucial for the foaming of PLA. Summary of the invention
[0004] 1. Technical issues to be resolved In view of the deficiencies in the prior art, the present invention provides a polylactic acid-based foaming material and a preparation method thereof, which solves the technical problem that the PLA has low melt strength at high temperatures, resulting in collapse and merging of cells during the foaming process.
[0005] (II) Technical solution To achieve the above objectives, the present invention is implemented through the following technical solutions: On the one hand, the present invention provides a polylactic acid-based foaming material, comprising the following components: polylactic acid, polybutylene adipate terephthalate, a chain extender, a foaming agent, and a nucleating agent, wherein the weight average molecular weight of the polylactic acid is 2.0×105~5.0×105 g / mol, and the content of dextrorotatory lactic acid is 1.2~1.6%, wherein the mass ratio of polylactic acid to polybutylene adipate terephthalate is (70~90):(10~30).
[0006] Preferably, the chain extender is selected from any one of 1,4-butanediol, 1,6-hexanediol, glycerol, trimethylolpropane, diethylene glycol, triethylene glycol, neopentyl glycol, sorbitol, diethylaminoethanol, ethylenediamine, N,N-dihydroxy(diisopropyl)aniline, and ADR.
[0007] Preferably, the foaming agent includes any one of an azo compound, a sulfonylhydrazide compound, and a nitroso compound.
[0008] Preferably, the azo compound is selected from any one of azodicarbonamide, azobisisobutyronitrile, difluorobisisoheptylnitrile, diisopropyl azodicarboxylate, and diethyl azodicarboxylate.
[0009] Preferably, the nucleating agent comprises an inorganic nucleating agent.
[0010] Preferably, the inorganic nucleating agent is selected from any one of talc, calcium carbonate, silicon dioxide, alum, titanium dioxide, calcium oxide and mica.
[0011] Preferably, the average diameter of the pores of the polylactic acid-based foaming material is 47-51 μm, and the pore density is 3.0×106-4.0×106.
[0012] On the other hand, the present invention provides a method for preparing the polylactic acid-based foam material, comprising the following steps: S1. Mix polylactic acid, polybutylene adipate terephthalate and a chain extender at 170° C. to 190° C., then add a foaming agent and a nucleating agent and mix them evenly to prepare a blended pre-foamed masterbatch, wherein the mass ratio of the polylactic acid to polybutylene adipate terephthalate is (70 to 90): (10 to 30), and the amounts of the chain extender, foaming agent and nucleating agent are (0.1 to 0.4) phr, (2 to 4) phr and (2 to 4) phr respectively; S2. Hot-pressing and foaming the blended pre-foamed masterbatch at 190° C. to 210° C. and 10 MPa to 20 MPa, and then cooling and taking out to obtain a polylactic acid-based foamed material.
[0013] (III) Beneficial effects The present invention provides a polylactic acid-based foam material and a preparation method thereof. Compared with the prior art, the present invention has the following beneficial effects: The invention provides a polylactic acid-based foaming material, comprising polybutylene adipate terephthalate. Under the condition that the mass ratio of polylactic acid to polybutylene adipate terephthalate is (70-90):(10-30), the prepared polylactic acid-based foaming material has a moderate melt flow rate, moderate melt strength, an average cell diameter of 47.0 μm-51.0 μm, and a cell density of 3.0×106 cells / cm3-4.0×106 cells / cm3. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0015] Figure 1 is a cross-sectional morphology diagram of the polylactic acid-based foam material prepared in Example 1; Figure 2 This is a pore size distribution diagram of the polylactic acid-based foam material prepared in Example 1. DETAILED DESCRIPTION
[0016] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention are clearly and completely described. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0017] In order to better understand the above technical solution, the above technical solution will be described in detail below in conjunction with the accompanying drawings and specific implementation methods. Example 1
[0018] This embodiment provides a method for preparing a polylactic acid-based foam material, comprising the following steps: S1. Polylactic acid (PLA) with a weight average molecular weight of 3.0×105 g / mol and a dextrorotatory lactic acid content of 1.4%, polybutylene adipate terephthalate (PBAT), and Joncryl ADR-4370F were mixed in an internal mixer, and the mixture was mixed at 180°C for 10 min with a stirring speed of 60 r / min. Then, azodicarbonamide (ADC), a foaming agent, and nano-SiO2, a nucleating agent, were added to the internal mixer and mixed for 8 min to prepare a PLA / PBAT blended pre-foamed masterbatch, wherein the mass ratio of PLA to PBAT was 80:20, and the amounts of ADR, ADC, and SiO2 were 0.3 phr, 3 phr, and 3 phr, respectively, that is, 0.3 parts of ADR, 3 parts of ADC, and 3 parts of SiO2 were added to every 100 parts (by mass) of PLA / PBAT mixture.
[0019] S2. Use a hot press to heat-press and foam the PLA / PBAT blended pre-foamed masterbatch prepared by mixing at 200°C and 15 MPa. The hot press process is heated for 8 minutes and maintained at pressure for 2 minutes, and then cooling water is passed to cool the material to below 30°C to obtain PLA / PBAT blended foamed specimens. Example 2
[0020] This embodiment provides a method for preparing a polylactic acid-based foam material, comprising the following steps: S1. Polylactic acid (PLA), polybutylene adipate terephthalate (PBAT) and Joncryl ADR-4370F were mixed in an internal mixer, and the mixture was mixed at 170°C for 10 min with a stirring speed of 60 r / min. Then, azodicarbonamide (ADC) as a foaming agent and nano-SiO2 as a nucleating agent were added to the internal mixer and the mixture was mixed for 8 min to prepare a PLA / PBAT blended pre-foamed masterbatch, wherein the mass ratio of PLA to PBAT was 90:10, and the amounts of ADR, ADC and SiO2 were 0.3 phr, 3 phr and 3 phr, respectively.
[0021] S2. Use a hot press to heat-press and foam the PLA / PBAT blended pre-foamed masterbatch prepared by mixing at 190°C and 10 MPa. The hot press process is heated for 8 minutes and maintained at pressure for 2 minutes, and then cooling water is passed to cool the material to below 30°C to obtain PLA / PBAT blended foamed specimens. Example 3
[0022] This embodiment provides a method for preparing a polylactic acid-based foam material, comprising the following steps: S1. Polylactic acid (PLA), polybutylene adipate terephthalate (PBAT) and Joncryl ADR-4370F were mixed in an internal mixer, and the mixture was mixed at 190°C for 10 min with a stirring speed of 60 r / min. Then, azodicarbonamide (ADC) as a blowing agent and nano-SiO2 as a nucleating agent were added to the internal mixer and the mixture was mixed for 8 min to prepare a PLA / PBAT blended pre-foamed masterbatch, wherein the mass ratio of PLA to PBAT was 70:30, and the amounts of ADR, ADC and SiO2 were 0.4 phr, 4 phr and 4 phr, respectively.
[0023] S2. Use a hot press to heat and foam the PLA / PBAT blended pre-foamed masterbatch prepared by mixing at 210°C and 20MPa. The hot press process is heated for 8 minutes and maintained at pressure for 2 minutes, and then cooling water is passed to cool the material to below 30°C to obtain PLA / PBAT blended foamed specimens.
[0024] Comparative Example 1 The difference between this comparative example and Example 1 is that the mass ratio of PLA to PBAT is 100:0, and the rest is the same as Example 1.
[0025] Comparative Example 2 The difference between this comparative example and Example 1 is that the mass ratio of PLA to PBAT is 50:50, and the rest is the same as Example 1.
[0026] Comparative Example 3 The difference between this comparative example and Example 1 is that the mass ratio of PLA to PBAT is 60:40, and the rest is the same as Example 1.
[0027] The cell morphology of the PLA / PBAT blended foamed strips of Example 1 was observed using a cold field emission scanning electron microscope (SEM). Figure 1 ,Depend on Figure 1 It can be seen that the PLA / PBAT blended foamed strips prepared in Example 1 have a smaller average cell diameter and a higher cell density. Figure 2 is a pore size distribution diagram of the PLA / PBAT blended foamed strip prepared in Example 1, as shown in Figure 2 As shown in Figure 3, the peak of the cell size distribution appears in the range of 40~50μm, and the cell size distribution basically conforms to the normal distribution.
[0028] The melt flow rate, average cell diameter, and cell density of the PLA / PBAT blended foamed strips prepared in the examples and comparative examples were tested. The test method is as follows. The test results are shown in Table 1.
[0029] Melt flow rate: The melt flow rate of the polylactic acid foamed strip of Example 1 was tested according to GB / T 3682-2000. The test temperature was set at 190° C., the load was 2.16 kg, and samples were taken every 10 seconds. A total of 10 samples were taken and weighed, and the average value was taken.
[0030] Average cell diameter and cell density: The prepared specimen with a size of 80 mm × 10 mm × 4 mm was completely immersed in liquid nitrogen and cooled for 30 minutes, and then quickly quenched and broken. The cell morphology of the PLA / PBAT blended foam material was observed using a cold field emission scanning electron microscope (SEM). Before SEM observation, a layer of platinum was evenly sputtered on all fracture surfaces, the acceleration voltage was 5.0 kV, and secondary electron imaging was selected.
[0031] Nanomeasurer software was used to analyze the diameter of the pores in the SEM images. The average diameter of the pores in the micrographs (D0) was calculated according to formula (1-1):
[0032] Among them, n i The equivalent diameter of the circumference is d i and i is greater than 100.
[0033] Cell density (N) is the number of cells per unit volume of the foamed material and is calculated using formula (1-2):
[0034] Where n and A are the number and area of cells in the micrograph, respectively (cm2 ), Φ is the volume expansion ratio, calculated using formula (1-3),
[0035] Among them, ρ s and ρ f are the densities of solid and foam samples, respectively.
[0036] Table 1 Performance test results of polylactic acid foam materials of examples and comparative examples
[0037] From Table 1, it can be seen from Examples 1 to 3 and Comparative Example 1 that, under the conditions of a temperature of 190°C and a load of 2.16 kg, the melt flow rate of the strip prepared without PBAT is 30.12 g / 10 min. The addition of PBAT reduces the melt flow rate of the strip and increases the melt strength of the strip, thereby avoiding the collapse and merging of the cells of PLA during the foaming process, so that the average diameter of the cells of the strip reaches 47.73 μm to 50.03 μm, and the cell density reaches 3.11×106 / cm3 to 3.91×106 / cm3. However, when the amount of PBAT added is increased to a mass ratio of PLA to PBAT of 60:40 and 50:50, although the melt flow rate of the strip is very low, the average diameter of the cells and the cell density are relatively small. This may be because the melt strength of the strip is too high, making it difficult for the cells to nucleate and grow, resulting in a relatively small average diameter of the cells and the cell density.
[0038] In summary, compared with the prior art, the present invention has the following beneficial effects: The present invention provides a polylactic acid-based foaming material, which includes an epoxy chain extender Joncryl ADR-4370F, which can increase the relative molecular weight of the polymer, thereby improving the melt strength of the polymer matrix and enhancing the foamability of the material; and can also increase the compatibility between PLA and PBAT through the reaction of epoxy groups with hydroxyl groups and carboxyl groups on the PLA and PBAT molecular chains, thereby further enhancing the foamability of the material.
[0039] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.
[0040] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A polylactic acid-based foaming material, characterized in that: The invention comprises polylactic acid, polybutylene adipate terephthalate, a chain extender, a foaming agent, and a nucleating agent, wherein the weight average molecular weight of the polylactic acid is 2.0×10 5 ~5.0×10 5 g / mol, and the content of right-lactic acid is 1.2-1.6%.
2. The polylactic acid-based foam material according to claim 1, characterized in that: The chain extender is selected from any one of 1,4-butanediol, 1,6-hexanediol, glycerol, trimethylolpropane, diethylene glycol, triethylene glycol, neopentyl glycol, sorbitol, diethylaminoethanol, ethylenediamine, N,N-dihydroxy (diisopropyl) aniline, and epoxy chain extender.
3. The polylactic acid-based foam material according to claim 1, characterized in that: The foaming agent includes any one of azo compounds, sulfonyl hydrazide compounds and nitroso compounds.
4. The polylactic acid-based foam material according to claim 3, characterized in that: The azo compound is selected from any one of azodicarbonamide, azobisisobutyronitrile, difluorobisisoheptylnitrile, diisopropyl azodicarboxylate and diethyl azodicarboxylate.
5. The polylactic acid-based foam material according to claim 1, characterized in that: The nucleating agent includes an inorganic nucleating agent.
6. The polylactic acid-based foam material according to claim 5, characterized in that: The inorganic nucleating agent is selected from any one of talc, calcium carbonate, silicon dioxide, alum, titanium dioxide, calcium oxide and mica.
7. The polylactic acid-based foam material according to claim 1, characterized in that: The mass ratio of the polylactic acid to polybutylene adipate terephthalate is 70-90:10-30.
8. The polylactic acid-based foam material according to claim 1, characterized in that: The average diameter of the pores of the polylactic acid-based foaming material is 47.0 to 51.0 μm, and the pore density is 3.0×10 6 ~4.0×10 6 .
9. A method for preparing a polylactic acid-based foam material according to any one of claims 1 to 8, characterized in that: The steps include: S1, polylactic acid, polybutylene adipate terephthalate, and a chain extender are mixed at 170° C. to 190° C., and then a foaming agent and a nucleating agent are added and mixed uniformly to prepare a blended pre-foamed masterbatch, wherein the mass ratio of the polylactic acid to polybutylene adipate terephthalate is 70 to 90:10 to 30, and the amounts of the chain extender, foaming agent, and nucleating agent are 0.1 to 0.4 phr, 2 to 4 phr, and 2 to 4 phr, respectively; S2. Hot-pressing and foaming the blended pre-foamed masterbatch at 190° C. to 210° C. and 10 MPa to 20 MPa, and then cooling and taking out to obtain a polylactic acid-based foamed material.
Citation Information
Patent Citations
Polylactic acid foaming material and preparation method thereof
CN101619158A
Food-grade heat-resistant PLA (polylactic acid) foaming material and preparation method thereof
CN113214618A
Full-biodegradable modified PBAT foamed sheet, and preparation method and application thereof
CN113549305A
Preparation method of light high-strength polylactic acid biomass foaming particles
CN114957773A
Polylactic Acid Foam Composition
US20110263732A1