SMC (sheet molding compound) material with high impact resistance and aging resistance for car hopper and preparation method of SMC material
By using specific resin combinations and component additions, SMC materials with high impact resistance and aging resistance are prepared, which solves the shortcomings of materials used in pickup truck beds in terms of high temperature resistance, corrosion resistance and impact resistance, and achieves the effect of no deformation and chemical corrosion resistance at high temperatures.
Patent Information
- Application Number
- CN202410919461.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-07-09
AI Technical Summary
Existing SMC materials used in pickup truck beds are insufficient in terms of high temperature resistance, corrosion resistance, and impact resistance, making it difficult to meet the requirements of pure electric vehicles for lightweight cargo boxes and outdoor use.
High-impact, aging-resistant SMC materials are prepared by combining phenolic vinyl resin, epoxy vinyl resin and unsaturated polyester resin, and adding corrosion-resistant plastic additives, curing agents, release agents, ceramic micro powders and alumina micro powders through a specific process, including mixing, coating and curing steps.
The prepared SMC material exhibits no deformation at 250℃ and possesses high impact toughness. It also demonstrates strong resistance to chemical corrosion, resisting corrosion from chemical reagents such as sulfuric acid, alcohol, diesel, brake fluid, and salt water.
Smart Images

Figure BDA0004936208610000051 
Figure BDA0004936208610000061 
Figure BDA0004936208610000081
Abstract
Description
Technical Field
[0001] The invention belongs to the field of composite materials for truck bodies, and specifically relates to a SMC material for truck bodies with high impact resistance and aging resistance and a preparation method thereof. Background Art
[0002] Sheet Molding Compound (SMC) is a thermosetting fiberglass molded composite material, the most common form of fiber reinforced plastics, which improves the comprehensive performance of composite materials by combining fibers with resins. SMC materials are usually made of thermosetting resins as the main raw materials, and thickeners, release agents, fillers and other additives are added to them, as well as glass fibers, to make SMC materials with different performances. According to the different performances of SMC materials, it can be applied in many industries, such as vehicles, construction, electronics and other industries. For vehicles, according to the performance requirements of different components, it can be divided into automotive exterior covers, engine protection panels, truck beds, etc.
[0003] Following the rapid development of electric vehicles around the world, pickup trucks built on pure electric platforms are also developing rapidly. Due to the characteristics of pure electric vehicles, the weight of the vehicle body needs to be greatly reduced, so SMC materials are gradually replacing traditional sheet metal materials to become the main material for pickup truck rear boxes.
[0004] Patent CN114350131B discloses an SMC material for pickup truck buckets, which mainly adds a scratch-resistant agent to the SMC material for pickup truck buckets, so that the surface brightness of the material changes less after being scratched, which is convenient for the use of pickup truck products. At the same time, adding a quick-curing composite agent to the SMC material for pickup truck buckets can greatly shorten the curing time of the material and improve production efficiency. However, since pickup truck buckets are often exposed to the outdoors, they have higher requirements for high temperature resistance / aging resistance. The buckets are often loaded with various types of goods, and have higher requirements for impact resistance and corrosion resistance. However, the above patents do not solve the needs of high temperature resistance, corrosion resistance, etc., and there is still a need to improve the impact resistance. Summary of the invention
[0005] The present invention provides a high impact resistance and aging resistance SMC material for a truck bucket, which has the advantages of high impact resistance / impact toughness, aging resistance (especially good heat resistance), strong corrosion resistance (especially strong chemical corrosion resistance to sulfuric acid, alcohol, diesel, brake fluid, coolant, salt water, etc.);
[0006] The present invention provides an SMC material, which includes any one or more of phenolic vinyl resin, epoxy vinyl resin, unsaturated polyester resin, corrosion-resistant plastic additive, curing agent, release agent, ceramic powder, alumina powder, thickener, and glass fiber;
[0007] In the present invention, the unsaturated polyester resin is selected from isophthalic acid neopentyl glycol unsaturated polyester resin, o-phthalic acid neopentyl glycol unsaturated polyester resin, terephthalic acid neopentyl glycol unsaturated polyester resin or isophthalic acid propylene glycol unsaturated polyester resin, preferably isophthalic acid neopentyl glycol unsaturated polyester resin;
[0008] In the present invention, the corrosion-resistant plastic additive is selected from one or both of PE powder and polytetrafluoroethylene powder;
[0009] In the present invention, the curing agent is selected from one or both of tert-butyl perbenzoate and dicumyl peroxide, preferably tert-butyl perbenzoate;
[0010] In the present invention, the release agent is selected from one or both of zinc stearate and calcium stearate, preferably zinc stearate;
[0011] In the present invention, the thickener is selected from one or more of magnesium oxide, calcium oxide, magnesium hydroxide, and calcium hydroxide, preferably magnesium oxide;
[0012] In the present invention, the glass fiber is selected from 10-30 mm glass fiber (alkali-free chopped), preferably 25 mm;
[0013] In the present invention, the SMC material comprises 4-10 parts by weight of phenolic vinyl resin;
[0014] and or,
[0015] In the present invention, the SMC material comprises 4-10 parts by weight of epoxy vinyl resin;
[0016] and or,
[0017] In the present invention, the SMC material comprises 4-20 parts by weight of unsaturated polyester resin, preferably 5-20 parts by weight, and more preferably 10-15 parts by weight;
[0018] and or,
[0019] In the present invention, the SMC material includes 6-20 parts by weight of a corrosion-resistant plastic additive; preferably includes 3-10 parts by weight of PE powder, and or includes 3-10 parts by weight of polytetrafluoroethylene powder;
[0020] and or,
[0021] In the present invention, the SMC material includes 0.3-2 parts by weight of a curing agent;
[0022] and or,
[0023] In the present invention, the SMC material includes 1-3 parts by weight of a release agent;
[0024] and or,
[0025] In the present invention, the SMC material comprises 10-20 parts by weight of ceramic powder;
[0026] and or,
[0027] In the present invention, the SMC material comprises 10-20 parts by weight of alumina powder;
[0028] and or,
[0029] In the present invention, the SMC material includes 1-5 parts by weight of a thickener;
[0030] and or,
[0031] In the present invention, the SMC material comprises 40-60 parts by weight of glass fiber;
[0032] In the present invention, in the SMC material, the weight ratio of the phenolic vinyl resin, the epoxy vinyl resin and the unsaturated polyester resin can be 1:1:0.5-2, preferably 1:1:1-1.5;
[0033] The present invention also provides a method for preparing an SMC material, comprising the following steps:
[0034] 3) mixing phenolic vinyl resin, epoxy vinyl resin, unsaturated polyester resin, corrosion-resistant plastic additive, curing agent, release agent, ceramic micropowder and alumina micropowder uniformly, and then adding thickener and mixing uniformly to obtain resin paste;
[0035] 4) The resin paste is coated on the upper and lower polyethylene films, the glass fibers are uniformly deposited on the resin paste, and the lower film carrying the fibers and the upper film are rolled, rolled, and aged to obtain the SMC material;
[0036] In the present invention, the aging temperature is 40-60°C, preferably 50°C;
[0037] In the present invention, the aging time is 12-48 hours, preferably 24 hours.
[0038] The invention selects different unsaturated polyester resins and applies them to the system of phenolic vinyl resin and epoxy vinyl resin, so that the prepared SMC material and the molded product thereof have high impact toughness, wherein the use of isophenyl neopentyl glycol unsaturated polyester resin as the unsaturated polyester resin has the best effect, and the use amount or proportion of the isophenyl neopentyl glycol unsaturated polyester resin will also affect the impact toughness performance; the SMC material and the molded product thereof have high heat resistance, and have no deformation / slight deformation and no cracking under the test condition of 250°C; in addition, the SMC material and the molded product thereof have extremely high chemical corrosion resistance, and have good tolerance to sulfuric acid, alcohol, diesel, brake fluid, coolant, salt water and the like. DETAILED DESCRIPTION
[0039] Example 1
[0040] Serial number raw material Weight 1 Phenolic vinyl resin 10 2 Epoxy vinyl resin 10 3 Isophenylene neopentyl glycol unsaturated polyester resin 10 4 PE powder 3 5 Polytetrafluoroethylene powder 5 6 Tert-butyl perbenzoate (curing agent) 2 7 Zinc stearate (release agent) 2 8 Ceramic powder 10 9 Alumina powder 10 10 Magnesium oxide (thickener) 5 11 Glass fiber (25mm) 60
[0041] In a high-speed shear mixer (1500r / min), add phenolic vinyl resin, epoxy vinyl resin, isophenyl neopentyl glycol unsaturated polyester resin, PE powder, polytetrafluoroethylene powder, tert-butyl perbenzoate, zinc stearate, ceramic powder, aluminum oxide powder, and aluminum oxide powder in order by weight ratio, mix and stir for 8 minutes, then add magnesium oxide, continue stirring for 10 minutes, and control the system temperature not to exceed 45°C to form a resin paste;
[0042] The resin paste is poured into the upper and lower glue tables of the SMC compound machine, the compound machine is turned on, the upper and lower substrate polyethylene films are unwound, and the scrapers on the upper and lower glue tables evenly coat the resin paste on the upper and lower substrate polyethylene films. When the PET film on the lower glue table passes through the fiber sedimentation area, the glass fiber (25mm) is evenly settled on the resin composition, and the mass ratio of fiber to resin paste is controlled to be 60:67. The lower film carrying the fiber and the upper film pass through the pressure roller to make the resin paste and the glass fiber penetrate and mix together, and then the air is removed by the rolling roller to make the resin paste and the fiber fully infiltrated, and then the SMC material is obtained by winding and ripening at 50°C for 24h.
[0043] Example 2
[0044] Serial number raw material Weight 1 Phenolic vinyl resin 10 2 Epoxy vinyl resin 10 3 Neopentyl glycol unsaturated polyester resin 10 4 PE powder 3 5 Polytetrafluoroethylene powder 5 6 Tert-butyl perbenzoate (curing agent) 2 7 Zinc stearate (release agent) 2 8 Ceramic powder 10 9 Alumina powder 10 10 Magnesium oxide (thickener) 5 11 Glass fiber (25mm) 60
[0045] The SMC material was prepared by a method similar to that in Example 1.
[0046] Example 3
[0047] Serial number raw material Weight 1 Phenolic vinyl resin 10 2 Epoxy vinyl resin 10 3 Terephthalate unsaturated polyester resin 10 4 PE powder 3 5 Polytetrafluoroethylene powder 5 6 Tert-butyl perbenzoate (curing agent) 2 7 Zinc stearate (release agent) 2 8 Ceramic powder 10 9 Alumina powder 10 10 Magnesium oxide (thickener) 5 11 Glass fiber (25mm) 60
[0048] The SMC material was prepared by a method similar to that in Example 1.
[0049] Example 4
[0050] Serial number raw material Weight 1 Phenolic vinyl resin 10 2 Epoxy vinyl resin 10 3 Isopropyl alcohol unsaturated polyester resin 10 4 PE powder 3 5 Polytetrafluoroethylene powder 5 6 Tert-butyl perbenzoate (curing agent) 2 7 Zinc stearate (release agent) 2 8 Ceramic powder 10 9 Alumina powder 10 10 Magnesium oxide (thickener) 5 11 Glass fiber (25mm) 60
[0051] The SMC material was prepared by a method similar to that in Example 1.
[0052] Example 5
[0053]
[0054]
[0055] In a high-speed shear mixer (1500r / min), add phenolic vinyl resin, epoxy vinyl resin, isophenyl neopentyl glycol unsaturated polyester resin, PE powder, polytetrafluoroethylene powder, tert-butyl perbenzoate, zinc stearate, ceramic powder, aluminum oxide powder, and aluminum oxide powder in order by weight ratio, mix and stir for 8 minutes, then add magnesium oxide, continue stirring for 10 minutes, and control the system temperature not to exceed 45°C to form a resin paste;
[0056] Pour the resin paste into the upper and lower glue tables of the SMC compound machine, start the compound machine, unwind the upper and lower substrate polyethylene films, and evenly coat the resin paste on the upper and lower substrate polyethylene films with the scrapers on the upper and lower glue tables. When the PET film on the lower glue table passes through the fiber sedimentation area, the glass fiber (25mm) is evenly settled on the resin composition, and the mass ratio of fiber to resin paste is controlled to be 60:62. The lower film carrying the fiber and the upper film pass through the pressure roller to make the resin paste and the glass fiber penetrate and mix together, and then the air is removed by the rolling roller to make the resin paste and the fiber fully infiltrated, and then the SMC material is obtained by winding and ripening at 50°C for 24h.
[0057] Example 6
[0058] Serial number raw material Weight 1 Phenolic vinyl resin 10 2 Epoxy vinyl resin 10 3 Isophenylene neopentyl glycol unsaturated polyester resin 15 4 PE powder 3 5 Polytetrafluoroethylene powder 5 6 Tert-butyl perbenzoate (curing agent) 2 7 Zinc stearate (release agent) 2 8 Ceramic powder 10 9 Alumina powder 10 10 Magnesium oxide (thickener) 5 11 Glass fiber (25mm) 60
[0059] In a high-speed shear mixer (1500r / min), add phenolic vinyl resin, epoxy vinyl resin, isophenyl neopentyl glycol unsaturated polyester resin, PE powder, polytetrafluoroethylene powder, tert-butyl perbenzoate, zinc stearate, ceramic powder, aluminum oxide powder, and aluminum oxide powder in order by weight ratio, mix and stir for 8 minutes, then add magnesium oxide, continue stirring for 10 minutes, and control the system temperature not to exceed 45°C to form a resin paste;
[0060] Pour the resin paste into the upper and lower glue tables of the SMC compound machine, start the compound machine, unwind the upper and lower substrate polyethylene films, and evenly coat the resin paste on the upper and lower substrate polyethylene films with the scrapers on the upper and lower glue tables. When the PET film on the lower glue table passes through the fiber sedimentation area, the glass fiber (25mm) is evenly settled on the resin composition, and the mass ratio of fiber to resin paste is controlled to be 60:72. The lower film carrying the fiber and the upper film pass through the pressure roller to make the resin paste and the glass fiber penetrate and mix together, and then the air is removed by the rolling roller to make the resin paste and the fiber fully infiltrated, and then the SMC material is obtained by winding and ripening at 50°C for 24h.
[0061] Example 7
[0062] Serial number raw material Weight 1 Phenolic vinyl resin 10 2 Epoxy vinyl resin 10 3 Isophenylene neopentyl glycol unsaturated polyester resin 20 4 PE powder 3 5 Polytetrafluoroethylene powder 5 6 Tert-butyl perbenzoate (curing agent) 2 7 Zinc stearate (release agent) 2 8 Ceramic powder 10 9 Alumina powder 10 10 Magnesium oxide (thickener) 5 11 Glass fiber (25mm) 60
[0063] In a high-speed shear mixer (1500r / min), add phenolic vinyl resin, epoxy vinyl resin, isophenyl neopentyl glycol unsaturated polyester resin, PE powder, polytetrafluoroethylene powder, tert-butyl perbenzoate, zinc stearate, ceramic powder, aluminum oxide powder, and aluminum oxide powder in order by weight ratio, mix and stir for 8 minutes, then add magnesium oxide, continue stirring for 10 minutes, and control the system temperature not to exceed 45°C to form a resin paste;
[0064] The resin paste is poured into the upper and lower glue tables of the SMC compound machine, the compound machine is turned on, the upper and lower substrate polyethylene films are unwound, and the scrapers on the upper and lower glue tables evenly coat the resin paste on the upper and lower substrate polyethylene films. When the PET film on the lower glue table passes through the fiber sedimentation area, the glass fiber (25mm) is evenly settled on the resin composition, and the mass ratio of fiber to resin paste is controlled to be 60:77. The lower film carrying the fiber and the upper film pass through the pressure roller to make the resin paste and the glass fiber penetrate and mix together, and then the air is removed by the rolling roller to make the resin paste and the fiber fully infiltrated, and then the SMC material is obtained by winding and ripening at 50°C for 24h.
[0065] Application Example 1
[0066] The SMC material obtained in the above example was pressed at 140°C with a pressure of 1000 T / m 2 , the time is 30s / mm, and finally the SMC material molded product is obtained.
[0067] The impact toughness of the molded products was tested according to GB / T1451-2005. The test results are as follows:
[0068]
[0069] The molded product was placed at 250℃ for 2 hours to test its heat resistance. The test results are as follows:
[0070]
[0071] The embodiments described above are only preferred implementations of the present invention. It should be pointed out that a person skilled in the art can make several improvements without departing from the principles of the present invention, and these improvements should also be regarded as within the scope of protection of the present invention.
Claims
1. A SMC material, comprising any one or more of phenolic vinyl resin, epoxy vinyl resin, unsaturated polyester resin, corrosion-resistant plastic additive, curing agent, release agent, ceramic powder, alumina powder, thickener, and glass fiber.
2. The SMC material according to claim 1, characterized in that: The unsaturated polyester resin is selected from isophenylene glycol unsaturated polyester resin, orthophenylene glycol unsaturated polyester resin, paraphenylene glycol unsaturated polyester resin or isophenylene glycol unsaturated polyester resin.
3. The SMC material according to claim 2, characterized in that: The unsaturated polyester resin is selected from isophenyl neopentyl glycol unsaturated polyester resin.
4. The SMC material according to any one of claims 1 to 3, characterized in that: The corrosion-resistant plastic additive is selected from one or both of PE powder and polytetrafluoroethylene powder; and or, The curing agent is selected from one or both of tert-butyl perbenzoate and dicumyl peroxide, preferably tert-butyl perbenzoate; and or, The release agent is selected from one or both of zinc stearate and calcium stearate, preferably zinc stearate; and or, The thickener is selected from one or more of magnesium oxide, calcium oxide, magnesium hydroxide, and calcium hydroxide, preferably magnesium oxide; and or, The glass fiber is selected from glass fibers with a diameter of 10-30 mm.
5. The SMC material according to any one of claims 1 to 4, characterized in that: The SMC material comprises 4-10 parts by weight of phenolic vinyl resin; and or, The SMC material comprises 4-10 parts by weight of epoxy vinyl resin; and or, The SMC material comprises 4-20 parts by weight of unsaturated polyester resin, preferably 5-20 parts by weight, more preferably 10-15 parts by weight; and or, The SMC material includes 6-20 parts by weight of corrosion-resistant plastic additives; preferably includes 3-10 parts by weight of PE powder, and or includes 3-10 parts by weight of polytetrafluoroethylene powder; and or, The SMC material includes 0.3-2 parts by weight of a curing agent; and or, The SMC material includes 1-3 parts by weight of a release agent; and or, The SMC material includes 10-20 parts by weight of ceramic powder; and or, The SMC material includes 10-20 parts by weight of aluminum oxide powder; and or, The SMC material includes 1-5 parts by weight of a thickener; and or, The SMC material includes 40-60 parts by weight of glass fiber.
6. The SMC material according to any one of claims 1 to 5, characterized in that: In the SMC material, the weight ratio of phenolic vinyl resin, epoxy vinyl resin and unsaturated polyester resin is 1:1:0.5-2.
7. The SMC material according to claim 6, characterized in that: In the SMC material, the weight ratio of phenolic vinyl resin, epoxy vinyl resin and unsaturated polyester resin is 1:1:1-1.
5.
8. A method for preparing the SMC material according to any one of claims 1 to 7, characterized in that: The steps include: 1) mixing phenolic vinyl resin, epoxy vinyl resin, unsaturated polyester resin, corrosion-resistant plastic additive, curing agent, release agent, ceramic micropowder and alumina micropowder uniformly, and then adding thickener and mixing uniformly to obtain resin paste; 2) The resin paste is coated on the upper and lower polyethylene films, the glass fibers are uniformly deposited on the resin paste, and the lower film and the upper film carrying the fibers are rolled, wound, and aged to obtain the SMC material.
Citation Information
Patent Citations
Self-priming coil coating compositions and method
CA2464241A1
Resin composition for high water resistance sheet molding compound, high water resistance sheet molding compound, and high water resistance bathtub
CN102746466A
SMC polyester moulding compound as well as preparation method and application thereof
CN110951227A
SMC material with high hiding rate and high gloss and preparation method thereof
CN114085510A
Sheet molding compound, its manufacturing method and molded article using sheet molding compound