Preparation method of modified silicone rubber material

By introducing catechol groups and ferric ions into silicone rubber, the adhesion and cohesive properties of silicone rubber are enhanced, solving the problem of decreased adhesion performance of silicone rubber materials underwater, and achieving stable adhesion and sealing of modified silicone rubber materials.

CN118879076APending Publication Date: 2024-11-01CHINA SHIPBUILDING INDUSTRY CORPORATION NO725 RESEARCH INSTITUTE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411114157.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Existing silicone rubber materials exhibit decreased or failed adhesion performance underwater, making it difficult to maintain stable adhesion properties.

Method used

Modified silicone rubber materials are prepared by introducing catechol groups into silicone rubber to enhance adhesion and cohesion through non-covalent interactions and ferric ion modification.

Benefits of technology

It improves the adhesion stability and sealing performance of silicone rubber materials underwater, reduces peeling or delamination, and enhances the adsorption stability of the biomimetic adsorption structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004993159870000011
    Figure HDA0004993159870000011
  • Figure HDA0004993159870000012
    Figure HDA0004993159870000012
  • Figure HDA0004993159870000013
    Figure HDA0004993159870000013
Patent Text Reader

Abstract

The invention belongs to the technical field of preparation of silicone rubber materials, and particularly relates to a preparation method of a modified silicone rubber material capable of being repeatedly adhered in water, which comprises the following steps: reacting 3-glycidoxypropyltrimethoxysilane with dopamine hydrochloride to generate a KH560-DA compound, or reacting the KH560-DA compound with the dopamine hydrochloride to generate a modified silicone rubber material; isocyanatopropyltriethoxysilane and dopamine hydrochloride react to generate an IPTS-DA compound, then the IPTS-DA compound and anhydrous ferric trichloride are jointly doped into silicon rubber to prepare a modified silicon rubber material, and the adhesion performance of the modified silicon rubber is provided by synthesizing a silane coupling agent containing a catechol group. The cohesive force of the silicone rubber material is improved through ferric ions, the stripping or layering phenomenon under the action of external force is reduced, and the integrity of an adhesion interface is kept; by means of the strong non-covalent interaction of catechol groups and the cohesion effect of silicone rubber, the prepared silicone rubber material with the underwater adhesion performance can improve the sealing performance and the adsorption stability of a bionic adsorption structure prepared based on the material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical field:

[0001] The invention belongs to the technical field of silicone rubber material preparation, and specifically relates to a method for preparing a modified silicone rubber material that can repeatedly adhere in water, by means of the strong non-covalent interaction of catechol groups and the cohesive force of silicone rubber, to prepare a silicone rubber material with underwater adhesion performance. Background technology:

[0002] Adhesive materials often have good adhesion properties in the air. Once placed in an underwater environment, their adhesion properties will rapidly decrease or fail. Silicone rubber materials have been widely used underwater due to their excellent mechanical properties and chemical stability, especially bionic suction cup materials used for underwater adsorption. For example, Chinese patent 202410537048.X discloses a bionic octopus suction cup system with self-sensing adsorption force, which specifically includes the following contents: (1) preparing a bionic octopus suction cup according to the characteristics of the octopus suction cup; (2) implanting a sensor in the bionic octopus suction cup; (3) constructing a BP neural network based on the sensor data, specifically including: constructing a BP neural network: collecting four sensor data for four silicone materials of different hardness respectively, the input of the neural network prediction model is the output voltage value of the four sensors over time series, and the output of the neural network is the adsorption force perceived by the suction cup itself, so the input layer nodes of the neural network are determined to be 4 and the output layer nodes are 1; determining the hidden layer nodes: determining the value range of the hidden layer nodes according to the empirical formula of the hidden layer nodes, where m is the number of hidden layer nodes, l and k are respectively is the number of nodes in the input layer and the output layer, and a is an adjustment constant between 1 and 10; different numbers of network layer nodes are set in the prediction model, and the training is iterated 100 times. The number of hidden layer nodes is determined according to the error of the training parameters. The training indicators include mean square error and absolute error. The formulas of the two error indicators are as follows: The actual output of the BP neural network: The expected output of the network: d(n) = [d1, d2,,…,dj] After n iterations of the neural network, the error signal is defined as: ej(n) = dj(n)-Yj(n) Definition error: Total network error: The genetic algorithm optimizes the initial weights of the neural network, and selects, crosses, and mutates each individual fitness through the fitness function. The selected optimal individual is the optimal initial weight of the BP neural network; The genetic algorithm coding length calculation formula: S =

[0003] n×l+l×m+l+m; Genetic algorithm fitness function: where n represents the total number of samples, oi represents the expected output value of the i-th sample data, and yi represents the actual output value of the network model of the i-th sample data; Selection function: where fi represents the individual fitness, Pi represents the probability of the individual being selected, and M represents the size of the selected population; Simulate binary crossover, first randomly select chromosomes from the population for crossover pairing, and then select a random position k to perform the following operation: b is a random number between [0, 1], and the paired chromosomes have the relationship x`k+y`k=xk+yk after crossover; Mutation operation, randomly find a chromosome X=(x1, x1, ...xk, ...xn) from the population and mutate its chromosome xk component according to a certain mutation probability. The mutated chromosome X`=(x1, x1, ...xk, ...xn) where ak and bk are the upper and lower bounds of the component, g is the current evolutionary number of the chromosome, and gmax is the maximum evolutionary number. The objective function value is recalculated for the updated chromosome until the global optimal chromosome and the optimal target are reached, and the next iteration is entered until the maximum number of iterations is reached; (4) Adsorption force measurement and neural network training and prediction: The optimal value obtained by the genetic algorithm optimization part is assigned to the BP neural network, and then the prediction result is obtained through training and testing; (5) Animal heart surface adsorption force verification: Select a suitable animal heart as an experimental object to predict the adsorption force, wherein the device includes a suction cup, a sensor and a data acquisition unit. The suction cup can be attached to the surface of biological tissue, and the adsorption force is predicted by the sensor and the neural network to evaluate the adsorption performance of the biological tissue surface. After the bionic suction cup is adsorbed on the surface of the object, as time goes by, water molecules slowly penetrate into the suction cup cavity through the adsorption interface, resulting in a gradual decrease in the adsorption force and final desorption. Based on this, a silicone rubber material with underwater adhesion properties was developed and designed to block water molecules on the adsorption interface from penetrating into the inner cavity, which is of great significance to improving the underwater adsorption stability of the bionic suction cup.

[0004] The adhesion performance of silicone rubber is not only related to adhesion, but also to cohesion. When rubber with strong cohesion forms an adhesion interface with other material surfaces, it can provide a more stable cohesive structure, which helps to maintain the integrity of the adhesion interface and reduce the probability of peeling or delamination under external force. Secondly, when rubber adheres to other materials, rubber with strong cohesion can more effectively transmit and disperse stress, avoid damage to the adhesion interface caused by stress concentration, and help maintain the stability and durability of the adhesion interface.

[0005] Mussels are a kind of crustacean marine organisms widely distributed in coastal and offshore areas. Studies have shown that the catechol structure in 3,4-dihydroxyphenylalanine (DOPA) in the byssus protein secreted by mussels can produce strong non-covalent interactions with the substrate, including: (1) forming bidentate hydrogen bonds with the substrate; (2) producing coordination bonds with metals, metal ions and metal oxides; (3) forming cation-π interactions with metal ions and forming π-π interactions with polymers with benzene rings in their molecular structure.

[0006] Therefore, a compound with 3,4-dihydroxyphenylalanine (DOPA) function is introduced into the silicone rubber matrix, such as a silane coupling agent containing a catechol group after modification, to exert a strong non-covalent interaction between the catechol group and the substrate and enhance the adhesion performance. At the same time, the introduction of trivalent iron ions into silicone rubber changes the cohesion of silicone rubber, thereby changing the mechanical strength, improving stability, maintaining the integrity of the adhesion interface, and reducing the peeling or delamination phenomenon under the action of external forces. Summary of the invention:

[0007] The purpose of the present invention is to overcome the shortcomings of the prior art and to develop a method for preparing a modified silicone rubber material so as to improve the sealing performance of a bionic adsorption structure prepared based on silicone rubber material and enhance the adsorption stability of the bionic adsorption structure.

[0008] In order to achieve the above-mentioned purpose, the process of the modified silicone rubber material preparation method of the present invention is as follows: firstly, a silane coupling agent containing a catechol structure is modified to prepare a bionic accelerator, and then the bionic accelerator and anhydrous ferric chloride (FeCl3) are co-added to silicone rubber to prepare a modified silicone rubber material that can be repeatedly adhered in water;

[0009] Among them, bionic accelerators include the following two types:

[0010] One is a KH560-DA compound generated by the reaction of 3-glycidyloxypropyltrimethoxysilane (KH560) and dopamine hydrochloride (DA);

[0011] The other is an IPTS-DA compound generated by the reaction of isocyanatepropyltriethoxysilane (IPTS) and dopamine hydrochloride (DA).

[0012] The specific process is as follows:

[0013] (1) Preparation of biomimetic accelerator

[0014] First, N,N-dimethylformamide (DMF) is used to dissolve dopamine hydrochloride DA to obtain a DMF solution;

[0015] Then, 3-glycidyloxypropyltrimethoxysilane (KH560) or isocyanatepropyltriethoxysilane (IPTS) was added to the DMF solution and nitrogen was bubbled into it;

[0016] Finally, the biomimetic promoter is obtained by heating under a nitrogen atmosphere, stirring and reacting, and rotary evaporation;

[0017] (2) Preparation of modified silicone rubber

[0018] First, the bionic accelerator is added to the silicone rubber, stirred, and after the mixture is evenly mixed, anhydrous ferric chloride is added and stirred to obtain a mixed silicone rubber;

[0019] Then, add the curing agent into the mixed silicone rubber, stir, mix evenly, and evacuate;

[0020] Finally, the vacuumed mixed silicone rubber is heated to solidify it, thereby obtaining the modified silicone rubber;

[0021] Wherein, the concentration of DMF solution is 0.07-0.30 g / mL;

[0022] The mass ratio of dopamine hydrochloride to 3-glycidyloxypropyltrimethoxysilane (KH560) or isocyanatepropyltriethoxysilane (IPTS) is 0.5-1:1;

[0023] The mass ratio of biomimetic accelerator to silicone rubber is 1:50-200;

[0024] The mass ratio of anhydrous ferric chloride to silicone rubber is 1:100-500;

[0025] The mass ratio of curing agent to silicone rubber is 1:10;

[0026] The stirring reaction temperature in step (1) is 70° C. and the time is 4 h;

[0027] The heating temperature in step (2) is 80° C. and the curing time is 6 hours.

[0028] The mechanical properties and adhesion properties of the modified silicone rubber material of the present invention are regulated by adjusting the ratio of a silane coupling agent containing a catechol structure to anhydrous ferric chloride.

[0029] Compared with the prior art, the present invention first generates a KH560-DA compound based on the reaction of 3-glycidyloxypropyltrimethoxysilane (KH560) and dopamine hydrochloride (DA), or generates an IPTS-DA compound based on the reaction of isocyanatepropyltriethoxysilane (IPTS) and dopamine hydrochloride (DA), and then adds the IPTS-DA compound and anhydrous ferric chloride (FeCl3) into silicone rubber to prepare a modified silicone rubber material that can be repeatedly adhered in water, provides adhesion performance of the modified silicone rubber by synthesizing a silane coupling agent containing a catechol group, improves the cohesion of the silicone rubber material by trivalent iron ions, reduces peeling or delamination under the action of external force, maintains the integrity of the adhesion interface, and thus improves the adhesion stability of the silicone rubber material; the scientific principle is reliable, and the silicone rubber material with underwater adhesion performance is prepared by means of the strong non-covalent interaction of the catechol group and the cohesion of the silicone rubber, which can improve the sealing performance of a bionic adsorption structure prepared based on the material and enhance the adsorption stability of the bionic adsorption structure. Description of the drawings:

[0030] Figure 1 This is the reaction formula involved in step (1) of Example 1 of the present invention.

[0031] Figure 2 This is a physical picture of the bionic accelerator involved in Example 2 of the present invention.

[0032] Figure 3 Schematic diagram showing the comparison of the peel strength of the modified silicone rubber prepared in Example 3 of the present invention in air and water.

[0033] Figure 4 This is a schematic diagram of the modified silicone rubber prepared in Example 4 of the present invention adsorbing a stainless steel sheet in water.

[0034] Figure 5 This is the reaction formula involved in step (1) of Example 5 of the present invention.

[0035] Figure 6 This is a physical picture of the bionic accelerator involved in Example 6 of the present invention.

[0036] Figure 7 Schematic diagram showing the comparison of the peel strength of the modified silicone rubber prepared in Example 7 of the present invention in air and water.

[0037] Figure 8 This is a schematic diagram of the modified silicone rubber prepared in Example 8 of the present invention adsorbing a stainless steel sheet in water. Specific implementation method:

[0038] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments.

[0039] Embodiment 1:

[0040] The specific process of the modified silicone rubber material preparation method involved in this embodiment is as follows:

[0041] (1) Preparation of biomimetic accelerator

[0042] First, dopamine hydrochloride (DA) was added into a three-necked flask, and N,N-dimethylformamide (DMF) was drawn to dissolve DA to obtain a DMF solution;

[0043] Then, 3-glycidyloxypropyltrimethoxysilane (KH560) was added to the DMF solution, and nitrogen was bubbled in to remove air;

[0044] Finally, the mixture was heated and stirred under a nitrogen atmosphere, and after the reaction was completed, the DMF solution was removed by rotary evaporation. The obtained yellow viscous product was the biomimetic accelerator: KH560-DA.

[0045] (2) Preparation of modified silicone rubber

[0046] First, add KH560-DA to silicone rubber, stir, and after mixing evenly, add anhydrous ferric chloride and stir to obtain mixed silicone rubber;

[0047] Then, the curing agent is added to the mixed silicone rubber, stirred, mixed evenly, and vacuumed to remove the air mixed in the mixed silicone rubber;

[0048] Finally, the mixed silicone rubber from which air has been removed is placed in a vacuum drying oven, heated, and cured to obtain the modified silicone rubber.

[0049] The reaction formula of step (1) involved in this embodiment is as follows Figure 1 shown.

[0050] Embodiment 2:

[0051] The specific process of the modified silicone rubber material preparation method involved in this embodiment is as follows:

[0052] (1) Place 3.78 g of dopamine hydrochloride in a 100 mL three-necked flask, and add 20 mL of DMF to dissolve the dopamine hydrochloride;

[0053] 4.72 g of 3-glycidyloxypropyltrimethoxysilane was added into a three-necked flask, nitrogen was bubbled, and the mixture was stirred at 70°C for 4 h under a nitrogen atmosphere;

[0054] The solution was spin dried to obtain Figure 2 The orange-yellow viscous liquid shown: KH560-DA;

[0055] (2) Add 0.2 g of KH560-DA to 20 g of silicone rubber, stir to mix evenly, then add 0.05 g of anhydrous ferric chloride, stir to obtain a mixed silicone rubber;

[0056] Add 2g of curing agent to the mixed silicone rubber, stir, mix evenly, and place in a vacuum pump to evacuate;

[0057] The mixed silicone rubber from which air has been removed is placed in a vacuum drying oven, heated to 80° C., and cured for 6 hours to obtain a modified silicone rubber.

[0058] Embodiment 3:

[0059] The specific process of the modified silicone rubber material preparation method involved in this embodiment is as follows:

[0060] (1) Place 3.78 g of dopamine hydrochloride in a 100 mL three-necked flask, and add 20 mL of DMF to dissolve the dopamine hydrochloride;

[0061] 4.72 g of 3-glycidyloxypropyltrimethoxysilane was added into a three-necked flask, nitrogen was bubbled, and the mixture was stirred at 70°C for 4 h under a nitrogen atmosphere;

[0062] The solution was spin-dried to obtain an orange-yellow viscous liquid: KH560-DA;

[0063] (2) Add 0.2 g of KH560-DA to 20 g of silicone rubber, stir to mix evenly, then add 0.1 g of anhydrous ferric chloride, stir to obtain a mixed silicone rubber;

[0064] Add 2g of curing agent to the mixed silicone rubber, stir, mix evenly, and place in a vacuum pump to evacuate;

[0065] The mixed silicone rubber from which air has been removed is placed in a vacuum drying oven, heated to 80°C, and cured for 6 hours to obtain a modified silicone rubber. The peel strength comparison of the modified silicone rubber in air and water is as follows: Figure 3 shown.

[0066] Embodiment 4:

[0067] The specific process of the modified silicone rubber material preparation method involved in this embodiment is as follows:

[0068] (1) Place 3.78 g of dopamine hydrochloride in a 100 mL three-necked flask, and add 20 mL of DMF to dissolve the dopamine hydrochloride;

[0069] 4.72 g of 3-glycidyloxypropyltrimethoxysilane was added into a three-necked flask, nitrogen was bubbled, and the mixture was stirred at 70°C for 4 h under a nitrogen atmosphere;

[0070] The solution was spin-dried to obtain an orange-yellow viscous liquid: KH560-DA;

[0071] (2) Add 0.4 g of KH560-DA to 20 g of silicone rubber, stir to mix evenly, then add 0.05 g of anhydrous ferric chloride, stir to obtain a mixed silicone rubber;

[0072] Add 2g of curing agent to the mixed silicone rubber, stir, mix evenly, and place in a vacuum pump to evacuate;

[0073] The mixed silicone rubber from which air is removed is placed in a vacuum drying oven, heated to 80° C., and cured for 6 hours to obtain a modified silicone rubber. The modified silicone rubber is as follows: Figure 4 As shown, it can easily stick to a stainless steel sheet weighing 200g in water.

[0074] Embodiment 5:

[0075] The specific process of the modified silicone rubber material preparation method involved in this embodiment is as follows:

[0076] (1) Preparation of biomimetic accelerator

[0077] First, dopamine hydrochloride (DA) was added into a three-necked flask, and N,N-dimethylformamide (DMF) was drawn to dissolve DA to obtain a DMF solution;

[0078] Then, isocyanatepropyltriethoxysilane (IPTS) was added to the DMF solution, and nitrogen was bubbled in to remove air;

[0079] Finally, the mixture was heated and stirred under a nitrogen atmosphere, and after the reaction was completed, the DMF solution was removed by rotary evaporation. The obtained yellow viscous product was the biomimetic promoter: IPTS-DA.

[0080] (2) Preparation of modified silicone rubber

[0081] First, add IPTS-DA to silicone rubber, stir, and after mixing evenly, add anhydrous ferric chloride and stir to obtain mixed silicone rubber;

[0082] Then, the curing agent is added to the mixed silicone rubber, stirred, mixed evenly, and vacuumed to remove the air mixed in the mixed silicone rubber;

[0083] Finally, the mixed silicone rubber from which air has been removed is placed in a vacuum drying oven, heated, and cured to obtain the modified silicone rubber.

[0084] The reaction formula of step (1) involved in this embodiment is as follows Figure 5 shown.

[0085] Embodiment 6:

[0086] The specific process of the modified silicone rubber material preparation method involved in this embodiment is as follows:

[0087] (1) Place 3.78 g of dopamine hydrochloride in a 100 mL three-necked flask, and add 20 mL of DMF to dissolve the dopamine hydrochloride;

[0088] 4.94 g of isocyanatepropyltriethoxysilane was added into a three-necked flask, nitrogen was bubbled, and the mixture was stirred at 70°C for 4 h under nitrogen atmosphere;

[0089] The solution was spin dried to obtain Figure 6 The orange-yellow viscous liquid shown: IPTS-DA;

[0090] (2) adding 0.2 g of IPTS-DA to 20 g of silicone rubber and stirring to mix evenly, then adding 0.05 g of anhydrous ferric chloride and stirring to obtain a mixed silicone rubber;

[0091] Add 2g of curing agent to the mixed silicone rubber, stir, mix evenly, and place in a vacuum pump to evacuate;

[0092] The mixed silicone rubber from which air has been removed is placed in a vacuum drying oven, heated to 80° C., and cured for 6 hours to obtain a modified silicone rubber.

[0093] Embodiment 7:

[0094] The specific process of the modified silicone rubber material preparation method involved in this embodiment is as follows:

[0095] (1) Place 3.78 g of dopamine hydrochloride in a 100 mL three-necked flask, and add 20 mL of DMF to dissolve the dopamine hydrochloride;

[0096] 4.94 g of isocyanatepropyltriethoxysilane was added into a three-necked flask, nitrogen was bubbled, and the mixture was stirred at 70°C for 4 h under nitrogen atmosphere;

[0097] The solution was spin-dried to obtain an orange-yellow viscous liquid: IPTS-DA;

[0098] (2) adding 0.2 g of IPTS-DA to 20 g of silicone rubber and stirring to mix evenly, then adding 0.1 g of anhydrous ferric chloride and stirring to obtain a mixed silicone rubber;

[0099] Add 2g of curing agent to the mixed silicone rubber, stir, mix evenly, and place in a vacuum pump to evacuate;

[0100] The mixed silicone rubber from which air has been removed is placed in a vacuum drying oven, heated to 80°C, and cured for 6 hours to obtain a modified silicone rubber. The peel strength comparison of the modified silicone rubber in air and water is as follows: Figure 7 shown.

[0101] Embodiment 8:

[0102] The specific process of the modified silicone rubber material preparation method involved in this embodiment is as follows:

[0103] (1) Place 3.78 g of dopamine hydrochloride in a 100 mL three-necked flask, and add 20 mL of DMF to dissolve the dopamine hydrochloride;

[0104] 4.94 g of isocyanatepropyltriethoxysilane was added into a three-necked flask, nitrogen was bubbled, and the mixture was stirred at 70°C for 4 h under nitrogen atmosphere;

[0105] The solution was spin-dried to obtain an orange-yellow viscous liquid: IPTS-DA;

[0106] (2) adding 0.4 g of IPTS-DA to 20 g of silicone rubber and stirring to mix evenly, then adding 0.05 g of anhydrous ferric chloride and stirring to obtain a mixed silicone rubber;

[0107] Add 2g of curing agent to the mixed silicone rubber, stir, mix evenly, and place in a vacuum pump to evacuate;

[0108] The mixed silicone rubber from which air is removed is placed in a vacuum drying oven, heated to 80° C., and cured for 6 hours to obtain a modified silicone rubber. The modified silicone rubber is as follows: Figure 8 As shown, it can easily stick to a stainless steel sheet weighing 200g in water.

Claims

1. A method for preparing a modified silicone rubber material, characterized in that: The process is: firstly modify the silane coupling agent containing catechol structure to obtain bionic accelerator, then add the bionic accelerator and anhydrous ferric chloride into silicone rubber to obtain modified silicone rubber material which can be repeatedly adhered in water.

2. The method for preparing a modified silicone rubber material according to claim 1, characterized in that: The mechanical properties and adhesion properties are controlled by adjusting the ratio of the silane coupling agent containing a catechol structure to anhydrous ferric chloride.

3. A method for preparing a modified silicone rubber material according to claim 1 or 2, characterized in that: The bionic accelerator is a KH560-DA compound generated by the reaction of 3-glycidyloxypropyltrimethoxysilane and dopamine hydrochloride.

4. A method for preparing a modified silicone rubber material according to claim 1 or 2, characterized in that: The biomimetic accelerator is an IPTS-DA compound generated by the reaction of isocyanatepropyltriethoxysilane and dopamine hydrochloride.

5. A method for preparing a modified silicone rubber material according to claim 1 or 2, characterized in that: The specific process is as follows: (1) Preparation of biomimetic accelerator First, dopamine hydrochloride is dissolved in N,N-dimethylformamide to obtain a DMF solution; Then, 3-glycidyloxypropyltrimethoxysilane or isocyanatepropyltriethoxysilane was added to the DMF solution, and nitrogen was bubbled into the solution; Finally, the biomimetic promoter is obtained by heating under a nitrogen atmosphere, stirring and reacting, and rotary evaporation; (2) Preparation of modified silicone rubber First, the bionic accelerator is added to the silicone rubber, stirred, and after the mixture is evenly mixed, anhydrous ferric chloride is added and stirred to obtain a mixed silicone rubber; Then, add the curing agent into the mixed silicone rubber, stir, mix evenly, and evacuate; Finally, the vacuumed mixed silicone rubber is heated to obtain modified silicone rubber.

6. The method for preparing a modified silicone rubber material according to claim 5, characterized in that: The concentration of DMF solution is 0.07-0.30 g / mL; The mass ratio of dopamine hydrochloride to 3-glycidyloxypropyltrimethoxysilane or isocyanatepropyltriethoxysilane is 0.5-1:1; The mass ratio of biomimetic accelerator to silicone rubber is 1:50-200; The mass ratio of anhydrous ferric chloride to silicone rubber is 1:100-500; The mass ratio of curing agent to silicone rubber is 1:

10.

7. The method for preparing a modified silicone rubber material according to claim 6, characterized in that: The stirring reaction temperature in step (1) is 70° C. and the time is 4 h.

8. The method for preparing a modified silicone rubber material according to claim 7, characterized in that: The heating temperature in step (2) is 80° C. and the curing time is 6 hours.