Heat-conducting gel with low oil permeability and high heat conductivity and preparation process thereof
By using composite coupling agent in thermal gel for surface treatment and silicon gel preparation, the powder filling amount and thermal conductivity are improved, and the problems of poor thermal conductivity of thermal gel and condensate condensation are solved, and efficient thermal conductivity is achieved Performance and stability.
Patent Information
- Application Number
- CN202411110726.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing thermal gel powder filling rate is low, resulting in poor thermal conductivity, especially the problem of condensate condensation is prone to long-term working and high-temperature conditions.
Thermal gel formula with low permeability oil and high thermal conductivity includes vinyl silicone oil, hydrogen-containing silicone oil, platinum catalyst, cyclohexanyne alcohol, TMDO, MVC, white carbon black, alumina and diamond powder, and the surface is carried out by composite coupling agent. Treatment and preparation of silicon gels improve powder filling and thermal conductivity, and prevent silicone oil from precipitating and condensate coagulation.
It achieves higher thermal conductivity and low precipitation rate after curing, ensuring that condensate does not coagulate under high temperature conditions of 85°C, and improves the stability of the use of thermally conductive gel.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of thermal conductive gels, in particular to a thermal conductive gel with low oil permeability and high thermal conductivity and a preparation process thereof. Background Art
[0002] Thermally conductive gel, also known as thermal paste or thermally conductive silicone, is a viscous substance with high thermal conductivity. Thermally conductive gel is usually composed of three parts: thermally conductive filler, matrix material and additives. It is widely used in thermal management systems of electronic equipment. The main function of thermally conductive gel is to fill the gap between the radiator and the heat source, improve the heat conduction efficiency, and ensure that the electronic equipment maintains a stable temperature during operation, thereby improving performance and extending life. However, existing thermally conductive gels still have some disadvantages, such as low powder filling rate, resulting in poor thermal conductivity, especially under long-term work, which will seriously affect the thermal conductivity effect. At the same time, after being used under high temperature conditions for a long time, condensation of varying degrees will occur. For this reason, we propose a low-penetration oil and high-thermal conductivity thermally conductive gel and its preparation process. Summary of the invention
[0003] The object of the present invention is to provide a thermally conductive gel with low oil permeability and high thermal conductivity and a preparation process thereof, so as to solve the problems raised in the above background technology.
[0004] To achieve the above object, the present invention provides the following technical solutions:
[0005] A low-penetration oil-high thermal conductivity thermally conductive gel, comprising the following raw material components by weight: 60-80 parts of vinyl silicone oil, 20-50 parts of hydrogen-containing silicone oil, 1-5 parts of platinum catalyst, 0.1-3 parts of cyclohexynol, 0.1-3 parts of TMDO, 0.1-1 parts of MVC, 0.2-3 parts of white carbon black, 0.3-1.5 parts of composite coupling agent, 100-600 parts of aluminum oxide, 100-300 parts of spherical aluminum nitride, and 300-600 parts of diamond powder; wherein the composite coupling agent comprises 10%-50% of γ-methacryloxypropyltrimethoxysilane and 50%-90% of a modified compound; the modified compound is prepared by reacting itaconic acid and γ-(2,3-epoxypropoxy)propyltrimethoxysilane.
[0006] Preferably, the vinyl silicone oil comprises ① double-ended vinyl silicone oil with a viscosity of 20-500 mPa*s, and ② single-ended vinyl silicone oil with a viscosity of 70-300 mPa*s.
[0007] Preferably, the platinum catalyst is a complex of chloroplatinic acid and vinyl double-end, and the platinum content is 3000-8000ppm; the specific model is Heraeus CAST 5000ppm.
[0008] Preferably, the white carbon black is fumed white carbon black with a specific surface area of 80-150 m2 / g; the specific model is Wacker H18.
[0009] Preferably, the alumina is spherical alumina or single crystal alumina, and the particle size D50 is 0.4-40 μm.
[0010] Preferably, the diamond powder is a complete crystalline diamond powder with a particle size D50 of 30-120 μm.
[0011] A preparation process of a low-oil permeability and high-thermal-conductivity thermally conductive gel comprises the following steps:
[0012] Step 1: Prepare a modified compound. The preparation of the modified compound is a reaction of itaconic acid and an epoxysilane coupling agent: dissolve itaconic acid and γ-(2,3-epoxypropoxy)propyltrimethoxysilane in acetone, add triphenylphosphine, heat and reflux for 2 hours, and remove the solvent under reduced pressure to obtain a modified compound; specifically: dissolve 10-15 parts by weight of itaconic acid and 110-120 parts by weight of γ-(2,3-epoxypropoxy)propyltrimethoxysilane in 500 parts by weight of acetone, add 0.5-1 parts by weight of triphenylphosphine, heat and reflux with stirring for 2-4 hours, and remove the solvent under reduced pressure to obtain a modified compound;
[0013] Step 2: mixing to obtain a composite coupling agent;
[0014] Step 3: Use a composite coupling agent to perform surface treatment on all fillers; Specific scheme: Use a powder high-speed mixer, set the speed to 1200rpm, put in 100kg of powder, heat the mixer to 100°C, and spray a composite coupling agent diluted with alcohol in a ratio of 1:1 on top of the mixer by a spray method; wherein the composite coupling agent contains 10%-50% of γ-methacryloxypropyltrimethoxysilane and 50%-90% of a modified compound;
[0015] Step 4: Use various silicone oil monomers, catalysts, and inhibitors to prepare silicone gel of AB components. The specific examples are as follows: VS-100ML single-end vinyl silicone oil (A component 80, B component 20), VS-285CV double-end vinyl silicone oil (A component 10, B component 10), HH-010-130 end hydrogen-containing silicone oil (A component 0, B component 8), CE-30LV side content silicone oil (A component 0, B component 57), Heraeus CAST 5000ppm (A component 1.3, B component 0), cyclohexynol (A component 0, B component 0.2), TMDO (A component 0, B component 0.09);
[0016] Step 5: Add the powder obtained in step 3 to the gel of component A, the powder ratio is 93-98%, the gel ratio of component A is 7-2%, and vacuum heat at 130℃ for 1h; add the powder obtained in step 3 to the gel of component B, the powder ratio is the same as that of component A, and vacuum heat at 60℃ for 1h;
[0017] Step 6: After the AB components are cooled, they are mixed in a 1:1 ratio and poured into the gel tube through a filling device to obtain a thermally conductive gel.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] The thermally conductive gel with low oil permeability and high thermal conductivity and its preparation process, the thermally conductive gel of the present invention, the powder and the silicone oil form a good combination through the composite coupling agent, so as to achieve higher powder filling and achieve higher thermal conductivity. At the same time, the silicone oil precipitation rate is low after curing, and no condensate is condensed under the relatively strict high-temperature use condition of 85°C. DETAILED DESCRIPTION
[0020] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0021] Example 1
[0022] A thermally conductive gel with low oil permeability and high thermal conductivity comprises the following raw material components by weight: 60 parts of vinyl silicone oil, 20 parts of hydrogen-containing silicone oil, 1 part of platinum catalyst, 0.1 part of cyclohexynol, 0.1 part of TMDO, 0.1 part of MVC, 0.2 part of white carbon black, 0.3 part of composite coupling agent, 100 parts of alumina, 100 parts of spherical aluminum nitride, and 300 parts of diamond powder; wherein the composite coupling agent comprises 10%-50% of γ-methacryloxypropyltrimethoxysilane and 50%-90% of a modified compound; the modified compound is prepared by reacting itaconic acid and γ-(2,3-epoxypropoxy)propyltrimethoxysilane.
[0023] Wherein: the vinyl silicone oil comprises ① double-end vinyl silicone oil with a viscosity of 300mpa*s, ② single-end vinyl silicone oil with a viscosity of 100mpa*s, specifically, the double-end vinyl silicone oil has a viscosity of 300mpa*s, the single-end vinyl silicone oil has a content of 100mpa*s, and the addition ratio of the two is 100:40; the hydrogen-containing silicone oil comprises ① end-side hydrogen-containing silicone oil with a viscosity of 10-100mpa*s and a hydrogen content of 1-10mmol / g, and ② end-side hydrogen-containing silicone oil with a viscosity of 30mpa*s and a hydrogen content of 0.75mmol / g;
[0024] Specifically, the ratio of the viscosity of the end-side hydrogen-containing silicone oil to the end-side hydrogen-containing silicone oil is 20:100;
[0025] The platinum catalyst is a complex of chloroplatinic acid and vinyl double-end, with a platinum content of 3000-8000ppm; the specific model is Heraeus CAST 5000ppm;
[0026] The white carbon black is fumed white carbon black with a specific surface area of 80-150m2 / g; the specific model is Wacker H18;
[0027] The alumina is spherical alumina or single crystal alumina, with a particle size D50 of 0.4-40 μm, and the spherical alumina models are Yaduma AO-502, DENKA DAW-3, DAW-10, and DAW-45. The single crystal alumina is Sumitomo AA-04, AA-3, and AA-10; the aluminum nitride is spherical aluminum nitride, with a particle size D50 of 30-120 μm; the models are Jinyi New Materials AN-50, AN-80, and AN-120;
[0028] The diamond powder is a complete crystal diamond powder with a particle size D50 of 30-120 μm and a model of Yanjiao Polaris MBD6-30, MBD6-40 and MBD6-120.
[0029] A preparation process of a low-penetration oil-high thermal conductivity thermally conductive gel, characterized in that it comprises the following steps:
[0030] Step 1: Prepare a modified compound. The preparation of the modified compound is a reaction of itaconic acid and an epoxysilane coupling agent: dissolve itaconic acid and γ-(2,3-epoxypropoxy)propyltrimethoxysilane in acetone, add triphenylphosphine, heat and reflux for 2 hours, and remove the solvent under reduced pressure to obtain a modified compound; specifically: dissolve 10-15 parts by weight of itaconic acid and 110-120 parts by weight of γ-(2,3-epoxypropoxy)propyltrimethoxysilane in 500 parts by weight of acetone, add 0.5-1 parts by weight of triphenylphosphine, heat and reflux with stirring for 2-4 hours, and remove the solvent under reduced pressure to obtain a modified compound;
[0031] Step 2: Mixing to obtain a composite coupling agent. The mechanism of action of the composite coupling agent: The two substances of the composite coupling agent act synergistically, have a good coating effect on diamond, can reduce the oil absorption value of the filler, obtain a higher filling amount in the thermal conductive gel, and obtain higher thermal conductivity; at the same time, it can react with silicone oil to make the silicone oil and powder well combined after the thermal conductive gel is cured, and it is not easy to oil out, and it also reduces the volatilization of small molecule silicone oil;
[0032] Step 3: Use a composite coupling agent to perform surface treatment on all fillers; Specific scheme: Use a powder high-speed mixer, set the speed to 1200rpm, put in 100kg of powder, heat the mixer to 100°C, and spray a composite coupling agent diluted with alcohol in a ratio of 1:1 on top of the mixer by a spray method; wherein the composite coupling agent contains 10%-50% of γ-methacryloxypropyltrimethoxysilane and 50%-90% of a modified compound;
[0033] Step 4: Use various silicone oil monomers, catalysts, and inhibitors to prepare silicone gel of AB components. The specific examples are as follows: VS-100ML single-end vinyl silicone oil (A component 80, B component 20), VS-285CV double-end vinyl silicone oil (A component 10, B component 10), HH-010-130 end hydrogen-containing silicone oil (A component 0, B component 8), CE-30LV side content silicone oil (A component 0, B component 57), Heraeus CAST 5000ppm (A component 1.3, B component 0), cyclohexynol (A component 0, B component 0.2), TMDO (A component 0, B component 0.09);
[0034] Step 5: Add the powder obtained in step 3 to the gel of component A, the powder ratio is 93-98%, the gel ratio of component A is 7-2%, and vacuum heat at 130℃ for 1h; add the powder obtained in step 3 to the gel of component B, the powder ratio is the same as that of component A, and vacuum heat at 60℃ for 1h;
[0035] Step 6: After the AB components are cooled, they are mixed in a 1:1 ratio and poured into a gel tube through a filling device to obtain a thermal conductive gel.
[0036] Example 2
[0037] A thermally conductive gel with low oil permeability and high thermal conductivity comprises the following raw material components by weight: 70 parts of vinyl silicone oil, 35 parts of hydrogenated silicone oil, 3.5 parts of platinum catalyst, 2 parts of cyclohexynol, 2 parts of TMDO, 0.6 parts of MVC, 2.1 parts of white carbon black, 0.9 parts of composite coupling agent, 350 parts of alumina, 200 parts of spherical aluminum nitride, and 400 parts of diamond powder; wherein the composite coupling agent comprises 10%-50% of γ-methacryloxypropyltrimethoxysilane and 50%-90% of a modified compound; the modified compound is prepared by reacting itaconic acid and γ-(2,3-epoxypropoxy)propyltrimethoxysilane.
[0038] Wherein: the vinyl silicone oil comprises ① double-end vinyl silicone oil with a viscosity of 300mpa*s, ② single-end vinyl silicone oil with a viscosity of 100mpa*s, specifically, the double-end vinyl silicone oil has a viscosity of 300mpa*s, the single-end vinyl silicone oil has a content of 100mpa*s, and the addition ratio of the two is 100:40; the hydrogen-containing silicone oil comprises ① end-side hydrogen-containing silicone oil with a viscosity of 10-100mpa*s and a hydrogen content of 1-10mmol / g, and ② end-side hydrogen-containing silicone oil with a viscosity of 30mpa*s and a hydrogen content of 0.75mmol / g;
[0039] Specifically, the ratio of the viscosity of the end-side hydrogen-containing silicone oil to the end-side hydrogen-containing silicone oil is 20:100;
[0040] The platinum catalyst is a complex of chloroplatinic acid and vinyl double-end, with a platinum content of 3000-8000ppm; the specific model is Heraeus CAST 5000ppm;
[0041] The white carbon black is fumed white carbon black with a specific surface area of 80-150m2 / g; the specific model is Wacker H18;
[0042] The alumina is spherical alumina or single crystal alumina, with a particle size D50 of 0.4-40 μm, and the spherical alumina models are Yaduma AO-502, DENKA DAW-3, DAW-10, and DAW-45. The single crystal alumina is Sumitomo AA-04, AA-3, and AA-10; the aluminum nitride is spherical aluminum nitride, with a particle size D50 of 30-120 μm; the models are Jinyi New Materials AN-50, AN-80, and AN-120;
[0043] The diamond powder is a complete crystal diamond powder with a particle size D50 of 30-120 μm and a model of Yanjiao Polaris MBD6-30, MBD6-40 and MBD6-120.
[0044] A preparation process of a low-penetration oil-high thermal conductivity thermally conductive gel, characterized in that it comprises the following steps:
[0045] Step 1: Prepare a modified compound. The preparation of the modified compound is a reaction of itaconic acid and an epoxysilane coupling agent: dissolve itaconic acid and γ-(2,3-epoxypropoxy)propyltrimethoxysilane in acetone, add triphenylphosphine, heat and reflux for 2 hours, and remove the solvent under reduced pressure to obtain a modified compound; specifically: dissolve 10-15 parts by weight of itaconic acid and 110-120 parts by weight of γ-(2,3-epoxypropoxy)propyltrimethoxysilane in 500 parts by weight of acetone, add 0.5-1 parts by weight of triphenylphosphine, heat and reflux with stirring for 2-4 hours, and remove the solvent under reduced pressure to obtain a modified compound;
[0046] Step 2: Mixing to obtain a composite coupling agent. The mechanism of action of the composite coupling agent: The two substances of the composite coupling agent act synergistically, have a good coating effect on diamond, can reduce the oil absorption value of the filler, obtain a higher filling amount in the thermal conductive gel, and obtain higher thermal conductivity; at the same time, it can react with silicone oil to make the silicone oil and powder well combined after the thermal conductive gel is cured, and it is not easy to oil out, and it also reduces the volatilization of small molecule silicone oil;
[0047] Step 3: Use a composite coupling agent to perform surface treatment on all fillers; Specific scheme: Use a powder high-speed mixer, set the speed to 1200rpm, put in 100kg of powder, heat the mixer to 100°C, and spray a composite coupling agent diluted with alcohol in a ratio of 1:1 on top of the mixer by a spray method; wherein the composite coupling agent contains 10%-50% of γ-methacryloxypropyltrimethoxysilane and 50%-90% of a modified compound;
[0048] Step 4: Use various silicone oil monomers, catalysts, and inhibitors to prepare silicone gel of AB components. The specific examples are as follows: VS-100ML single-end vinyl silicone oil (A component 80, B component 20), VS-285CV double-end vinyl silicone oil (A component 10, B component 10), HH-010-130 end hydrogen-containing silicone oil (A component 0, B component 8), CE-30LV side content silicone oil (A component 0, B component 57), Heraeus CAST 5000ppm (A component 1.3, B component 0), cyclohexynol (A component 0, B component 0.2), TMDO (A component 0, B component 0.09);
[0049] Step 5: Add the powder obtained in step 3 to the gel of component A, the powder ratio is 93-98%, the gel ratio of component A is 7-2%, and vacuum heat at 130℃ for 1h; add the powder obtained in step 3 to the gel of component B, the powder ratio is the same as that of component A, and vacuum heat at 60℃ for 1h;
[0050] Step 6: After the AB components are cooled, they are mixed in a 1:1 ratio and poured into a gel tube through a filling device to obtain a thermal conductive gel.
[0051] Example 3
[0052] A thermally conductive gel with low oil permeability and high thermal conductivity comprises the following raw material components by weight: 80 parts of vinyl silicone oil, 50 parts of hydrogenated silicone oil, 5 parts of platinum catalyst, 3 parts of cyclohexynol, 3 parts of TMDO, 1 part of MVC, 3 parts of white carbon black, 1.5 parts of composite coupling agent, 600 parts of alumina, 300 parts of spherical aluminum nitride, and 600 parts of diamond powder; wherein the composite coupling agent comprises 10%-50% of γ-methacryloxypropyltrimethoxysilane and 50%-90% of a modified compound; the modified compound is prepared by reacting itaconic acid and γ-(2,3-epoxypropoxy)propyltrimethoxysilane.
[0053] Wherein: the vinyl silicone oil comprises ① double-end vinyl silicone oil with a viscosity of 300mpa*s, ② single-end vinyl silicone oil with a viscosity of 100mpa*s, specifically, the double-end vinyl silicone oil has a viscosity of 300mpa*s, the single-end vinyl silicone oil has a content of 100mpa*s, and the addition ratio of the two is 100:40; the hydrogen-containing silicone oil comprises ① end-side hydrogen-containing silicone oil with a viscosity of 10-100mpa*s and a hydrogen content of 1-10mmol / g, and ② end-side hydrogen-containing silicone oil with a viscosity of 30mpa*s and a hydrogen content of 0.75mmol / g;
[0054] Specifically, the ratio of the viscosity of the end-side hydrogen-containing silicone oil to the end-side hydrogen-containing silicone oil is 20:100;
[0055] The platinum catalyst is a complex of chloroplatinic acid and vinyl double-end, with a platinum content of 3000-8000ppm; the specific model is Heraeus CAST 5000ppm;
[0056] The white carbon black is fumed white carbon black with a specific surface area of 80-150m2 / g; the specific model is Wacker H18;
[0057] The alumina is spherical alumina or single crystal alumina, with a particle size D50 of 0.4-40 μm, and the spherical alumina models are Yaduma AO-502, DENKA DAW-3, DAW-10, and DAW-45. The single crystal alumina is Sumitomo AA-04, AA-3, and AA-10; the aluminum nitride is spherical aluminum nitride, with a particle size D50 of 30-120 μm; the models are Jinyi New Materials AN-50, AN-80, and AN-120;
[0058] The diamond powder is a complete crystal diamond powder with a particle size D50 of 30-120 μm and a model of Yanjiao Polaris MBD6-30, MBD6-40 and MBD6-120.
[0059] A preparation process of a low-penetration oil-high thermal conductivity thermally conductive gel, characterized in that it comprises the following steps:
[0060] Step 1: Prepare a modified compound. The preparation of the modified compound is a reaction of itaconic acid and an epoxysilane coupling agent: dissolve itaconic acid and γ-(2,3-epoxypropoxy)propyltrimethoxysilane in acetone, add triphenylphosphine, heat and reflux for 2 hours, and remove the solvent under reduced pressure to obtain a modified compound; specifically: dissolve 10-15 parts by weight of itaconic acid and 110-120 parts by weight of γ-(2,3-epoxypropoxy)propyltrimethoxysilane in 500 parts by weight of acetone, add 0.5-1 parts by weight of triphenylphosphine, heat and reflux with stirring for 2-4 hours, and remove the solvent under reduced pressure to obtain a modified compound;
[0061] Step 2: Mixing to obtain a composite coupling agent. The mechanism of action of the composite coupling agent: The two substances of the composite coupling agent act synergistically, have a good coating effect on diamond, can reduce the oil absorption value of the filler, obtain a higher filling amount in the thermal conductive gel, and obtain higher thermal conductivity; at the same time, it can react with silicone oil to make the silicone oil and powder well combined after the thermal conductive gel is cured, and it is not easy to oil out, and it also reduces the volatilization of small molecule silicone oil;
[0062] Step 3: Use a composite coupling agent to perform surface treatment on all fillers; Specific scheme: Use a powder high-speed mixer, set the speed to 1200rpm, put in 100kg of powder, heat the mixer to 100°C, and spray a composite coupling agent diluted with alcohol in a ratio of 1:1 on top of the mixer by a spray method; wherein the composite coupling agent contains 10%-50% of γ-methacryloxypropyltrimethoxysilane and 50%-90% of a modified compound;
[0063] Step 4: Use various silicone oil monomers, catalysts, and inhibitors to prepare silicone gel of AB components. The specific examples are as follows: VS-100ML single-end vinyl silicone oil (A component 80, B component 20), VS-285CV double-end vinyl silicone oil (A component 10, B component 10), HH-010-130 end hydrogen-containing silicone oil (A component 0, B component 8), CE-30LV side content silicone oil (A component 0, B component 57), Heraeus CAST 5000ppm (A component 1.3, B component 0), cyclohexynol (A component 0, B component 0.2), TMDO (A component 0, B component 0.09);
[0064] Step 5: Add the powder obtained in step 3 to the gel of component A, the powder ratio is 93-98%, the gel ratio of component A is 7-2%, and vacuum heat at 130℃ for 1h; add the powder obtained in step 3 to the gel of component B, the powder ratio is the same as that of component A, and vacuum heat at 60℃ for 1h;
[0065] Step 6: After the AB components are cooled, they are mixed in a 1:1 ratio and poured into a gel tube through a filling device to obtain a thermal conductive gel.
[0066] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A low-penetration oil-high thermal conductivity thermally conductive gel, characterized in that: The invention comprises the following raw material components by weight: 60-80 parts of vinyl silicone oil, 20-50 parts of hydrogen-containing silicone oil, 1-5 parts of platinum catalyst, 0.1-3 parts of cyclohexynol, 0.1-3 parts of TMDO, 0.1-1 parts of MVC, 0.2-3 parts of white carbon black, 0.3-1.5 parts of composite coupling agent, 100-600 parts of alumina, 100-300 parts of spherical aluminum nitride, and 300-600 parts of diamond powder; wherein the composite coupling agent comprises 10%-50% of γ-methacryloxypropyltrimethoxysilane and 50%-90% of modified compound; the modified compound is prepared by reacting itaconic acid and γ-(2,3-epoxypropoxy)propyltrimethoxysilane.
2. A thermally conductive gel with low oil permeability and high thermal conductivity according to claim 1, characterized in that: The vinyl silicone oil comprises ① double-ended vinyl silicone oil with a viscosity of 20-500 mpa*s and ② single-ended vinyl silicone oil with a viscosity of 70-300 mpa*s.
3. The low-oil permeability and high-thermal-conductivity thermally conductive gel according to claim 1, characterized in that: The platinum catalyst is a complex of chloroplatinic acid and vinyl double-end, and the platinum content is 3000-8000ppm; the specific model is Heraeus CAST5000ppm.
4. The low-oil permeability and high-thermal-conductivity thermally conductive gel according to claim 1, characterized in that: The white carbon black is fumed white carbon black with a specific surface area of 80-150m2 / g; the specific model is Wacker H18.
5. The low-oil permeability and high-thermal-conductivity thermally conductive gel according to claim 1, characterized in that: The alumina is spherical alumina or single crystal alumina, and the particle size D50 is 0.4-40 μm.
6. The low-oil permeability and high-thermal-conductivity thermally conductive gel according to claim 1, characterized in that: The diamond powder is a complete crystal diamond powder with a particle size D50 of 30-120 μm.
7. A process for preparing a low-penetration oil-high thermally conductive thermally conductive gel according to any one of claims 1 to 6, characterized in that: The steps include: Step 1: Prepare a modified compound. The preparation of the modified compound is a reaction of itaconic acid and an epoxysilane coupling agent: dissolve itaconic acid and γ-(2,3-epoxypropoxy)propyltrimethoxysilane in acetone, add triphenylphosphine, heat and reflux for 2 hours, and remove the solvent under reduced pressure to obtain a modified compound; specifically: dissolve 10-15 parts by weight of itaconic acid and 110-120 parts by weight of γ-(2,3-epoxypropoxy)propyltrimethoxysilane in 500 parts by weight of acetone, add 0.5-1 parts by weight of triphenylphosphine, heat and reflux with stirring for 2-4 hours, and remove the solvent under reduced pressure to obtain a modified compound; Step 2: mixing to obtain a composite coupling agent; Step 3: Use a composite coupling agent to perform surface treatment on all fillers; Specific scheme: Use a powder high-speed mixer, set the speed to 1200rpm, put in 100kg of powder, heat the mixer to 100°C, and spray a composite coupling agent diluted with alcohol in a ratio of 1:1 on top of the mixer by a spray method; wherein the composite coupling agent contains 10%-50% of γ-methacryloxypropyltrimethoxysilane and 50%-90% of a modified compound; Step 4: Use various silicone oil monomers, catalysts, and inhibitors to prepare silicone gel of AB components. The specific examples are as follows: VS-100ML single-end vinyl silicone oil (A component 80, B component 20), VS-285CV double-end vinyl silicone oil (A component 10, B component 10), HH-010-130 end hydrogen-containing silicone oil (A component 0, B component 8), CE-30LV side content silicone oil (A component 0, B component 57), Heraeus CAST 5000ppm (A component 1.3, B component 0), cyclohexynol (A component 0, B component 0.2), TMDO (A component 0, B component 0.09); Step 5: Add the powder obtained in step 3 to the gel of component A, the powder ratio is 93-98%, the gel ratio of component A is 7-2%, and vacuum heat at 130℃ for 1h; add the powder obtained in step 3 to the gel of component B, the powder ratio is the same as that of component A, and vacuum heat at 60℃ for 1h; Step 6: After the AB components are cooled, they are mixed in a 1:1 ratio and poured into a gel tube through a filling device to obtain a thermal conductive gel.
Citation Information
Cited By
Low-oil-permeability single-component heat-conducting gel and preparation method thereof