Dynamic thermal management coating with temperature self-adaptive thermal radiation regulation and control performance as well as preparation method and application of dynamic thermal management coating
By introducing rod-shaped VO2 micro-nano powder and infrared transparent solvent into VO2 coatings, combined with an appropriate amount of binder, temperature adaptive thermal radiation regulation is achieved, and the problem of single performance regulation in the existing technology is solved, and dynamic thermal management is met The dual demands of thermal disguise improve safety and production ease.
Patent Information
- Application Number
- CN202411113628.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-08-14
AI Technical Summary
Existing VO2 coatings can only achieve single performance regulation in radiation refrigeration or thermal camouflage, and cannot meet the dual needs of dynamic thermal management and thermal camouflage.
Rod-shaped VO2 micro-nano powder is mixed with an appropriate amount of infrared transparent solvent and binder to prepare dynamic thermal management coatings with temperature adaptive thermal radiation regulation performance. By adjusting the distribution of functional phases and the content of functional particles in the coating, it can be realized on different substrates. The emissivity on the surface changes with ambient temperature.
Thermal drive adaptive thermal control on high reflectivity substrates and thermal drive adaptive thermal camouflage on high emissivity substrates are realized, which meets the needs of dynamic thermal management and infrared camouflage, reduces the probability of being discovered by the enemy, and increases the The safety of combat personnel is guaranteed, and the production conditions are loose and the cost is low.
Smart Images

Figure CN118879110A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of preparation of energy-saving and emission-reduction intelligent materials and infrared camouflage materials. Background Art
[0002] With the increasing attention paid to climate change worldwide, zero-energy thermal management materials represented by radiation cooling have received widespread attention. However, traditional radiation cooling materials mainly achieve passive cooling based on their inherent characteristics, which cannot meet the thermal management needs of environmental changes and are prone to overcooling or overheating, resulting in additional energy consumption. At the same time, with the rapid development of modern war reconnaissance technology and precision-guided weapons, infrared thermal imaging technology has been increasingly widely used and has become an important means used for battlefield detection and guided weapons, which has put forward higher requirements for stealth technology that hides the infrared radiation characteristics of targets. The currently commonly used static infrared camouflage will lose its stealth effect when the environment changes due to the inconsistency between the stealth material and the background spectral signal. The dynamic temperature adaptive control material introduces the concepts of adaptability and intelligent control, which can dynamically adjust its own optical properties to respond to external changes, and can dynamically adjust its performance according to changes in external conditions or user needs, thereby achieving efficient and flexible thermal management performance and thermal camouflage performance in a wider range of scenarios.
[0003] Although in recent years, researchers have achieved dynamic adjustability of radiation performance through responses such as temperature, humidity, voltage and mechanical force, and used the dynamic infrared emissivity of materials to respond to external stimuli, thereby dynamically stabilizing the temperature in a fluctuating thermal environment. However, most adaptive thermal control materials are prepared on rigid substrates through specially designed optical structures, which are costly and complex to design, and cannot flexibly select substrates according to the application environment. As a typical thermotropic phase change material, VO2 can achieve a sudden change of 3 to 4 orders of magnitude in conductivity before and after the phase change, and the emissivity shows a negative differential change, which is very suitable for preparing coatings with suitable application substrates to achieve positive differential emissivity performance / negative differential emissivity performance. However, the current common VO2 coatings can only perform temperature-adaptive thermal radiation regulation for a single performance, and only achieve amplitude regulation in radiation cooling or only achieve regulation in thermal camouflage. Summary of the invention
[0004] The present invention aims to solve the problem that the existing VO2 coating can only achieve amplitude regulation in radiation cooling or can only achieve regulation in thermal camouflage, and to provide a dynamic thermal management coating with temperature-adaptive thermal radiation regulation performance and its preparation method and application.
[0005] A dynamic thermal management coating with temperature-adaptive thermal radiation control performance is prepared by 1 to 1000 parts of rod-shaped VO2 micro-nano powder, 800 to 1000 parts of solvent, 20 to 30 parts of dispersant, 40 to 60 parts of defoaming agent, 1000 to 1999 parts of binder, 10 to 20 parts of thickener and 10 to 20 parts of leveling agent in parts by mass.
[0006] A method for preparing a dynamic thermal management coating with temperature-adaptive thermal radiation control performance is carried out according to the following steps:
[0007] 1. Preparation of rod-shaped VO2 micro-nano powder:
[0008] Vanadium pentoxide powder and oxalic acid dihydrate powder are sequentially added to deionized water, and fully mixed under magnetic stirring until the solution changes from yellow to green and finally to dark blue to obtain a mixture, and the mixture is hydrothermally reacted at a temperature of 220°C to 240°C for 1h to 6h, and after cooling to room temperature, washed and centrifuged to obtain a dark black precipitate, namely VO2(B); the dark black precipitate is dried, and then heat-treated in an argon atmosphere at a temperature of 500°C to 550°C for 30min to 2h to obtain a rod-shaped VO2 micro-nano powder, namely VO2(M);
[0009] The mass ratio of the vanadium pentoxide powder to the oxalic acid dihydrate powder is 1:(1.25-1.6); the mass ratio of the vanadium pentoxide powder to the volume of deionized water is 1g:(40-50)mL;
[0010] 2. Preparation of VO2 coating:
[0011] Weigh 1 to 1000 parts of rod-shaped VO2 micro-nano powder, 800 to 1000 parts of solvent, 20 to 30 parts of dispersant, 40 to 60 parts of defoaming agent, 1000 to 1999 parts of binder, 10 to 20 parts of thickener and 10 to 20 parts of leveling agent by mass; mix 1 to 1000 parts of rod-shaped VO2 micro-nano powder, 800 to 1000 parts of solvent, 20 to 30 parts of dispersant and 40 to 60 parts of defoaming agent evenly, and then pre-disperse to obtain a pre-dispersed slurry, and then add 1000 to 1999 parts of binder, 10 to 20 parts of thickener and 10 to 20 parts of leveling agent to the pre-dispersed slurry for dispersion to obtain a dynamic thermal management coating with temperature-adaptive thermal radiation regulation performance.
[0012] An application of a dynamic thermal management coating with temperature-adaptive thermal radiation regulation performance, which is coated on a highly reflective substrate and a highly emissive substrate; when coated on a highly reflective substrate, thermally driven adaptive thermal control is achieved; when coated on a highly emissive substrate, thermally driven adaptive thermal camouflage is achieved.
[0013] The beneficial effects of the present invention are:
[0014] The present invention selects a VO2 rod-shaped structure that can play a role in dynamic thermal management and thermal camouflage as the functional phase. Compared with the commonly used spherical and linear shapes, the rod-shaped structure is in an intermediate state and has the functions of both states. Therefore, the distribution of the functional phase in the coating can be adjusted and the overlapping structure of the functional phase in the coating can be controlled to achieve the switching between the positive differential emissivity performance and the negative differential emissivity performance.
[0015] At low temperatures, VO2(M) is in an insulating state, the functional layer is in a highly infrared transparent state, and the overall effect is dominated by the substrate. At high temperatures, VO2 transforms into an R phase, high-content VO2 rod-shaped particles overlap each other, transforming into a metal phase with high reflectivity, reducing the emissivity, and meeting the requirements of infrared camouflage; low-content VO2 rod-shaped particles are adjacent to form antennas, using the interval photon resonance phenomenon to increase the emissivity, meeting the requirements of intelligent thermal control.
[0016] It can be seen that the present invention utilizes the characteristic of sudden change in conductivity of VO2 powder before and after phase change, and mixes it with an appropriate amount of infrared transparent solvent and binder to prepare a heat-driven adaptive thermal radiation regulating coating. According to the substrate coated with the coating and the change in the content of functional particles in the coating, a heat-driven adaptive thermal control coating can be obtained, whose emissivity on a high-reflectivity substrate can be reversibly converted as the ambient temperature changes, which manifests as a positive differential emissivity change; or a heat-driven adaptive thermal camouflage coating whose emissivity on a high-emissivity substrate can be reversibly converted as the ambient temperature changes, which manifests as a negative differential emissivity change.
[0017] Therefore, the present invention can achieve the maintenance of the temperature requirements of combatants in terms of dynamic thermal management by simply adjusting the concentration of the coating, and reduce the probability of being discovered by the enemy in terms of infrared camouflage, thereby greatly improving the safety of combatants. The temperature-adaptive thermal radiation control coating involved in the present invention has loose preparation conditions and is easy to mass produce, and has low production costs and application environment requirements. It is suitable for realizing dynamic control of infrared radiation characteristics according to environmental requirements, improving the autonomous thermal control ability of materials, and achieving energy saving / camouflage effects.
[0018] The present invention is used for a dynamic thermal management coating with temperature self-adapting thermal radiation control performance, and a preparation method and application thereof. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 TEM images of the rod-shaped VO2 nanopowder prepared in step 1 of Example 1, (a) low-resolution image, (b) high-resolution image, (c) SAED pattern;
[0020] Figure 2This is the SEM image of the rod-shaped VO2 nanopowder prepared in step 1 of Example 1. DETAILED DESCRIPTION
[0021] Specific implementation method 1: This implementation method is a dynamic thermal management coating with temperature-adaptive thermal radiation control performance, which is prepared by 1 to 1000 parts of rod-shaped VO2 micro-nano powder, 800 to 1000 parts of solvent, 20 to 30 parts of dispersant, 40 to 60 parts of defoaming agent, 1000 to 1999 parts of binder, 10 to 20 parts of thickener and 10 to 20 parts of leveling agent.
[0022] The beneficial effects of this embodiment are:
[0023] This embodiment selects a VO2 rod-shaped structure that can play a role in dynamic thermal management and thermal camouflage as the functional phase. Compared with the commonly used spherical and linear shapes, the rod-shaped structure is in an intermediate state and has the functions of both states. Therefore, the distribution of the functional phase in the coating can be adjusted and the overlapping structure of the functional phase in the coating can be controlled to achieve switching between positive differential emissivity performance and negative differential emissivity performance.
[0024] At low temperatures, VO2(M) is in an insulating state, the functional layer is in a highly infrared transparent state, and the overall effect is dominated by the substrate. At high temperatures, VO2 transforms into an R phase, high-content VO2 rod-shaped particles overlap each other, transforming into a metal phase with high reflectivity, reducing the emissivity, and meeting the requirements of infrared camouflage; low-content VO2 rod-shaped particles are adjacent to form antennas, using the interval photon resonance phenomenon to increase the emissivity, meeting the requirements of intelligent thermal control.
[0025] It can be seen that the present embodiment utilizes the characteristic of sudden change in conductivity of VO2 powder before and after phase change, and mixes it with appropriate amount of infrared transparent solvent and binder to prepare heat-driven adaptive thermal radiation regulating coating. According to the substrate coated with the coating and the change in the content of functional particles in the coating, a heat-driven adaptive thermal control coating can be obtained, whose emissivity on a high reflectivity substrate can be reversibly converted as the ambient temperature changes, which is manifested as a positive differential emissivity change; or a heat-driven adaptive thermal camouflage coating whose emissivity on a high emissivity substrate can be reversibly converted as the ambient temperature changes, which is manifested as a negative differential emissivity change.
[0026] Therefore, this embodiment can achieve the maintenance of the temperature requirements of combatants in terms of dynamic thermal management by simply adjusting the concentration of the coating, and reduce the probability of being discovered by the enemy in terms of infrared camouflage, thereby greatly improving the safety of combatants. The temperature-adaptive thermal radiation control coating involved in this embodiment has loose preparation conditions and is easy to mass produce, and has low production costs and application environment requirements. It is suitable for realizing dynamic control of infrared radiation characteristics according to environmental requirements, improving the autonomous thermal control ability of materials, and achieving energy saving / camouflage effects.
[0027] Specific implementation method 2: This implementation method is different from specific implementation method 1 in that the solvent is water, xylene, an alcohol solvent, a ketone solvent, an ester solvent or dichloromethane. Other aspects are the same as those of specific implementation method 1.
[0028] The solvent in the coating of this specific embodiment not only plays a role in dissolving the film-forming substances in the coating and adjusting the viscosity of the coating, but also ensures that the VO2 powder is evenly dispersed, which is more conducive to the coating evenly covering the surface of the object.
[0029] Specific implementation method 3: This implementation method is different from specific implementation method 1 or 2 in that: the binder is a solvent-based resin or a water-soluble resin; the solvent-based resin is a Karton resin, a polyamide resin, a phenolic resin or a vinyl resin; the water-soluble resin is a water-based polyurethane, an acrylic resin or an epoxy resin. The rest is the same as specific implementation method 1 or 2.
[0030] The binder of this specific embodiment is infrared transparent in the coating, which acts to bind various substances in the coating and attach them to the coated surface, and gives the coating sufficient mechanical strength to resist wear, scratches and other physical damage. At the same time, it also gives the coating weather resistance, chemical resistance, etc., and prolongs the service life of the coating.
[0031] Specific embodiment 4: This embodiment differs from specific embodiments 1 to 3 in that: the dispersant is a polystyrene maleic anhydride copolymer, a general-purpose silicone dispersant, or a POP polyether dispersant; the defoamer is an organosilicon defoamer or a polyether-modified polysiloxane defoamer. The rest is the same as specific embodiments 1 to 3.
[0032] Specific embodiment 5: This embodiment differs from specific embodiments 1 to 4 in that: the thickener is polyethylene oxide, polypropylene oxide or hydroxyethyl cellulose; the leveling agent is polyether modified polysiloxane, polyacrylate or alkyl or phenyl modified polysiloxane. Other aspects are the same as specific embodiments 1 to 4.
[0033] Specific implementation method 6: This implementation method is a method for preparing a dynamic thermal management coating with temperature adaptive thermal radiation control performance, which is carried out according to the following steps:
[0034] 1. Preparation of rod-shaped VO2 micro-nano powder:
[0035] Vanadium pentoxide powder and oxalic acid dihydrate powder are sequentially added to deionized water, and fully mixed under magnetic stirring until the solution changes from yellow to green and finally to dark blue to obtain a mixture, and the mixture is hydrothermally reacted at a temperature of 220°C to 240°C for 1h to 6h, and after cooling to room temperature, washed and centrifuged to obtain a dark black precipitate, namely VO2(B); the dark black precipitate is dried, and then heat-treated in an argon atmosphere at a temperature of 500°C to 550°C for 30min to 2h to obtain a rod-shaped VO2 micro-nano powder, namely VO2(M);
[0036] The mass ratio of the vanadium pentoxide powder to the oxalic acid dihydrate powder is 1:(1.25-1.6); the mass ratio of the vanadium pentoxide powder to the volume of deionized water is 1g:(40-50)mL;
[0037] 2. Preparation of VO2 coating:
[0038] Weigh 1 to 1000 parts of rod-shaped VO2 micro-nano powder, 800 to 1000 parts of solvent, 20 to 30 parts of dispersant, 40 to 60 parts of defoaming agent, 1000 to 1999 parts of binder, 10 to 20 parts of thickener and 10 to 20 parts of leveling agent by mass; mix 1 to 1000 parts of rod-shaped VO2 micro-nano powder, 800 to 1000 parts of solvent, 20 to 30 parts of dispersant and 40 to 60 parts of defoaming agent evenly, and then pre-disperse to obtain a pre-dispersed slurry, and then add 1000 to 1999 parts of binder, 10 to 20 parts of thickener and 10 to 20 parts of leveling agent to the pre-dispersed slurry for dispersion to obtain a dynamic thermal management coating with temperature-adaptive thermal radiation regulation performance.
[0039] Specific embodiment 7: This embodiment is different from specific embodiment 6 in that: the washing and centrifugation described in step 1 is to wash twice with deionized water, and then centrifuge for 8min to 10min at a speed of 6000 rpm to 8000 rpm; the drying described in step 1 is to dry for 4h to 8h at a temperature of 60℃ to 80℃. The rest is the same as specific embodiment 6.
[0040] Specific embodiment eight: This embodiment differs from specific embodiment six or seven in that: the pre-dispersion in step two is specifically carried out at a rotation speed of 600 to 800 rpm for 30 to 40 minutes; the dispersion in step two is specifically carried out at a rotation speed of 600 to 800 rpm for 20 to 30 minutes. The rest is the same as specific embodiment six or seven.
[0041] Specific embodiment nine: This embodiment is an application of a dynamic thermal management coating with temperature-adaptive thermal radiation regulation performance, which is coated on a highly reflective substrate and a highly emissive substrate; when coated on a highly reflective substrate, thermally driven adaptive thermal control is achieved; when coated on a highly emissive substrate, thermally driven adaptive thermal camouflage is achieved.
[0042] Specific embodiment 10: This embodiment differs from specific embodiment 9 in that: the coating thickness is 0.7 mm to 1 mm on a high reflective substrate and a high emissive substrate; the high reflectivity substrate is Al, Au, Ag, Mg, Ni, Zn or Cu; the high emissivity substrate is SiC, Fe2O3, SiO2 or polyimide. The rest is the same as specific embodiment 9.
[0043] The following examples are used to verify the beneficial effects of the present invention:
[0044] Embodiment 1:
[0045] A dynamic thermal management coating with temperature-adaptive thermal radiation control performance, which is prepared by 1 part of rod-shaped VO2 micro-nano powder, 1000 parts of solvent, 30 parts of dispersant, 60 parts of defoamer, 1999 parts of binder, 20 parts of thickener and 20 parts of leveling agent in terms of mass fraction;
[0046] The solvent is water.
[0047] The adhesive is water-based polyurethane, the manufacturer is Shanghai MacLean Biochemical Technology Co., Ltd., and the model is A909856.
[0048] The dispersant is polystyrene maleic anhydride copolymer, Shanghai MacLean Biochemical Technology Co., Ltd., S909954;
[0049] The defoamer is DOWSILACP-3073 defoamer compound produced by Shanghai Buding Chemical Co., Ltd.
[0050] The thickener is polyethylene oxide, Shanghai Aladdin Biochemical Technology Co., Ltd., P432440;
[0051] The leveling agent is HY-5030 produced by Beijing Maier Chemical.
[0052] The preparation method of the above-mentioned dynamic thermal management coating with temperature-adaptive thermal radiation control performance is carried out according to the following steps:
[0053] 1. Preparation of rod-shaped VO2 micro-nano powder:
[0054] 1.2 g of vanadium pentoxide powder (V2O5) and 1.6642 g of oxalic acid dihydrate powder (H2C2O4·2H2O) were added to 60 mL of deionized water in sequence, and the mixture was fully mixed under magnetic stirring until the solution changed from yellow to green and finally to dark blue to obtain a mixture. The mixture was hydrothermally reacted at 240°C for 3 h. After cooling to room temperature, the mixture was washed twice with deionized water, and then centrifuged at a speed of 6000 rpm for 8 min to obtain a dark black precipitate, namely VO2(B); the dark black precipitate was dried at 80°C for 6 h, and then heat-treated in an argon atmosphere at 500°C for 2 h to obtain a rod-shaped VO2 micro-nano powder, namely VO2(M);
[0055] 2. Preparation of VO2 coating:
[0056] Weigh 1 part of rod-shaped VO2 micro-nano powder, 1000 parts of solvent, 30 parts of dispersant, 60 parts of defoaming agent, 1999 parts of binder, 20 parts of thickener and 20 parts of leveling agent by mass; mix 1 part of rod-shaped VO2 micro-nano powder, 1000 parts of solvent, 30 parts of dispersant and 60 parts of defoaming agent evenly, then pre-disperse for 30 minutes at a speed of 600 rpm to obtain a pre-dispersed slurry, then add 1999 parts of binder, 20 parts of thickener and 20 parts of leveling agent to the pre-dispersed slurry, disperse for 20 minutes at a speed of 800 rpm to obtain a dynamic thermal management coating with temperature-adaptive thermal radiation regulation performance, namely VO2 coating.
[0057] The above-mentioned dynamic thermal management coating with temperature-adaptive thermal radiation control performance is applied by coating the VO2 coating on a highly reflective substrate with a coating thickness of 0.82 mm, leveling for 10 minutes after coating, and finally drying at a temperature of 80°C for 30 minutes to obtain a heat-driven adaptive thermal control device;
[0058] The high reflectivity substrate is Al.
[0059] The infrared radiation temperature of the heat-driven adaptive thermal control device in the 8-14μm wavelength range was recorded in the temperature range of 30℃ to 100℃, and the emissivity varied from 0.2 to 0.57.
[0060] Embodiment 2: This embodiment is different from Embodiment 1 in that: a dynamic thermal management coating with temperature-adaptive thermal radiation control performance is prepared by 2 parts of rod-shaped VO2 micro-nano powder, 1000 parts of solvent, 30 parts of dispersant, 60 parts of defoamer, 1990 parts of binder, 20 parts of thickener and 20 parts of leveling agent by mass; the above-mentioned dynamic thermal management coating with temperature-adaptive thermal radiation control performance is applied to a highly reflective substrate with a coating thickness of 0.80 mm, and then leveled for 10 minutes after coating, and finally dried at a temperature of 80°C for 30 minutes to obtain a heat-driven adaptive thermal control device. The rest is the same as Embodiment 1.
[0061] The addition of functional phases increases the difference in emissivity change, recording the infrared radiation temperature of the heat-driven adaptive thermal control device in the 8-14μm wavelength range within the temperature range of 30℃ to 100℃, and the emissivity changes from 0.34 to 0.84.
[0062] Embodiment 3: This embodiment is different from Embodiment 1 in that: a dynamic thermal management coating with temperature-adaptive thermal radiation control performance is prepared by 20 parts of rod-shaped VO2 micro-nano powder, 1000 parts of solvent, 30 parts of dispersant, 60 parts of defoamer, 1950 parts of binder, 20 parts of thickener and 20 parts of leveling agent by mass; the above-mentioned dynamic thermal management coating with temperature-adaptive thermal radiation control performance is applied to a highly reflective substrate with a coating thickness of 0.83mm, and the coating is leveled for 10 minutes after coating, and finally dried at a temperature of 80°C for 30 minutes to obtain a heat-driven adaptive thermal control device. The rest is the same as Embodiment 1.
[0063] The further increase of functional phases will reduce the performance of negative differential emissivity. The infrared radiation temperature of the heat-driven adaptive thermal control device in the wavelength range of 8-14μm is recorded in the temperature range of 30℃ to 100℃, and the emissivity changes from 0.66 to 0.97.
[0064] Embodiment 4: This embodiment is different from Embodiment 1 in that: a dynamic thermal management coating with temperature-adaptive thermal radiation control performance is prepared by 200 parts of rod-shaped VO2 micro-nano powder, 1000 parts of solvent, 26 parts of dispersant, 60 parts of defoamer, 1800 parts of binder, 18 parts of thickener and 18 parts of leveling agent by mass; the above-mentioned dynamic thermal management coating with temperature-adaptive thermal radiation control performance is applied to the high-emissivity substrate with a coating thickness of 0.81 mm, and the coating is leveled for 10 minutes after coating, and finally dried at a temperature of 80°C for 30 minutes to obtain a heat-driven adaptive thermal camouflage device; the high-emissivity substrate is SiO2. The rest is the same as Embodiment 1.
[0065] With further increase of functional phase content, positive differential emissivity performance turns into negative differential emissivity performance, and the infrared radiation temperature of thermally driven adaptive thermal camouflage device in 8-14μm wavelength range is recorded in the temperature range of 30℃ to 100℃, and the emissivity changes from 0.95 to 0.85.
[0066] Embodiment 5: This embodiment is different from Embodiment 1 in that: a dynamic thermal management coating with temperature-adaptive thermal radiation control performance is prepared by 500 parts of rod-shaped VO2 micro-nano powder, 900 parts of solvent, 20 parts of dispersant, 50 parts of defoamer, 1500 parts of binder, 14 parts of thickener and 14 parts of leveling agent by mass; the above-mentioned dynamic thermal management coating with temperature-adaptive thermal radiation control performance is applied to the high-emissivity substrate with a coating thickness of 0.85mm, and the coating is leveled for 10 minutes after coating, and finally dried at a temperature of 80°C for 30 minutes to obtain a heat-driven adaptive thermal camouflage device; the high-emissivity substrate is SiO2. The rest is the same as Embodiment 1.
[0067] The infrared radiation temperature of the heat-driven adaptive thermal camouflage device in the wavelength range of 8-14μm was recorded in the temperature range of 30℃ to 100℃, and the emissivity changed from 0.98 to 0.81.
[0068] Example 6: This example is different from Example 1 in that: a dynamic thermal management coating with temperature-adaptive thermal radiation control performance is prepared by 1000 parts of rod-shaped VO2 micro-nano powder, 800 parts of solvent, 20 parts of dispersant, 40 parts of defoamer, 1000 parts of binder, 10 parts of thickener and 10 parts of leveling agent by mass; the above-mentioned dynamic thermal management coating with temperature-adaptive thermal radiation control performance is applied to the high-emissivity substrate with a coating thickness of 0.87mm, and the coating is leveled for 10 minutes after coating, and finally dried at a temperature of 80°C for 30 minutes to obtain a heat-driven adaptive thermal camouflage device; the high-emissivity substrate is SiO2. Others are the same as Example 1.
[0069] The infrared radiation temperature of the heat-driven adaptive thermal camouflage device in the 8-14μm wavelength range was recorded in the temperature range of 30℃ to 100℃, and the emissivity changed from 0.97 to 0.69.
[0070] Figure 1 TEM images of the rod-shaped VO2 nanopowder prepared in step 1 of Example 1, (a) low-resolution image, (b) high-resolution image, (c) SAED pattern. As can be seen from the figure, the length of these nanorods is between 500nm and 1200nm, and the width is between 57nm and 120nm. In addition, obvious lattice planes ( Figure 1b), the plane spacing is d = 0.3221nm, which is equivalent to the (011) plane of monoclinic VO2. The obvious lattice edge also shows that the synthesized VO2 has a high crystallinity. According to the selected area electron diffraction (SAED) pattern ( Figure 1 c), the bright diffraction spots show that the (011), (202), (100) and (210) planes of the M-phase VO2 have good crystallinity, thus confirming the polycrystalline nature of the VO2 nanorods.
[0071] Figure 2 This is the SEM image of the rod-shaped VO2 nanopowder prepared in step 1 of Example 1; Figure 2 (a) It can be seen that the prepared VO2 presents a uniform and complete nanorod shape as a whole, which corresponds to the TEM results.
Claims
1. A dynamic thermal management coating with temperature adaptive thermal radiation control performance, characterized in that It is prepared from 1 to 1000 parts of rod-shaped VO2 micro-nano powder, 800 to 1000 parts of solvent, 20 to 30 parts of dispersant, 40 to 60 parts of defoamer, 1000 to 1999 parts of binder, 10 to 20 parts of thickener and 10 to 20 parts of leveling agent by mass.
2. A dynamic thermal management coating with temperature adaptive thermal radiation control performance according to claim 1, characterized in that The solvent is water, xylene, alcohol solvent, ketone solvent, ester solvent or dichloromethane.
3. The dynamic thermal management coating with temperature adaptive thermal radiation control performance according to claim 2, characterized in that The binder is a solvent-based resin or a water-soluble resin; the solvent-based resin is a Karton resin, a polyamide resin, a phenolic resin or a vinyl resin; the water-soluble resin is a water-based polyurethane, an acrylic resin or an epoxy resin.
4. The dynamic thermal management coating with temperature adaptive thermal radiation control performance according to claim 1, characterized in that The dispersant is a polystyrene maleic anhydride copolymer, a general-purpose organic silicon dispersant or a POP polyether dispersant; and the defoamer is an organic silicon defoamer or a polyether-modified polysiloxane defoamer.
5. The dynamic thermal management coating with temperature adaptive thermal radiation control performance according to claim 1, characterized in that The thickener is polyethylene oxide, polypropylene oxide or hydroxyethyl cellulose; the leveling agent is polyether modified polysiloxane, polyacrylate or alkyl or phenyl modified polysiloxane.
6. The method for preparing a dynamic thermal management coating having temperature adaptive thermal radiation control performance according to claim 1, characterized in that It is carried out in the following steps:
1. Preparation of rod-shaped VO2 micro-nano powder: Vanadium pentoxide powder and oxalic acid dihydrate powder are sequentially added to deionized water, and fully mixed under magnetic stirring until the solution changes from yellow to green and finally to dark blue to obtain a mixture, and the mixture is hydrothermally reacted at a temperature of 220°C to 240°C for 1h to 6h, and after cooling to room temperature, washed and centrifuged to obtain a dark black precipitate, namely VO2(B); the dark black precipitate is dried, and then heat-treated in an argon atmosphere at a temperature of 500°C to 550°C for 30min to 2h to obtain a rod-shaped VO2 micro-nano powder, namely VO2(M); The mass ratio of the vanadium pentoxide powder to the oxalic acid dihydrate powder is 1:(1.25-1.6); the mass ratio of the vanadium pentoxide powder to the volume of deionized water is 1g:(40-50)mL; 2. Preparation of VO2 coating: Weigh 1 to 1000 parts of rod-shaped VO2 micro-nano powder, 800 to 1000 parts of solvent, 20 to 30 parts of dispersant, 40 to 60 parts of defoaming agent, 1000 to 1999 parts of binder, 10 to 20 parts of thickener and 10 to 20 parts of leveling agent by mass; mix 1 to 1000 parts of rod-shaped VO2 micro-nano powder, 800 to 1000 parts of solvent, 20 to 30 parts of dispersant and 40 to 60 parts of defoaming agent evenly, and then pre-disperse to obtain a pre-dispersed slurry, and then add 1000 to 1999 parts of binder, 10 to 20 parts of thickener and 10 to 20 parts of leveling agent to the pre-dispersed slurry for dispersion to obtain a dynamic thermal management coating with temperature-adaptive thermal radiation regulation performance.
7. The method for preparing a dynamic thermal management coating having temperature adaptive thermal radiation control performance according to claim 6, characterized in that The washing and centrifugation described in step 1 specifically involves washing twice with deionized water, and then centrifuging for 8 min to 10 min at a rotation speed of 6000 rpm to 8000 rpm; the drying described in step 1 specifically involves drying for 4 h to 8 h at a temperature of 60° C. to 80° C.
8. The method for preparing a dynamic thermal management coating having temperature-adaptive thermal radiation control performance according to claim 6, characterized in that The pre-dispersion in step 2 is specifically carried out at a rotation speed of 600 to 800 rpm for 30 to 40 minutes; the dispersion in step 2 is specifically carried out at a rotation speed of 600 to 800 rpm for 20 to 30 minutes.
9. The application of a dynamic thermal management coating with temperature adaptive thermal radiation control performance as claimed in claim 1, characterized in that It is coated on highly reflective substrates and highly emissive substrates; When coated on a highly reflective substrate, thermally driven adaptive thermal control is achieved; When coated on a highly emissive substrate, thermally driven adaptive thermal camouflage is achieved.
10. The use of a dynamic thermal management coating with temperature adaptive thermal radiation control performance as claimed in claim 9, characterized in that The coating thickness is 0.7mm to 1mm and is applied on a high-reflection substrate and a high-emission substrate; the high-reflectivity substrate is Al, Au, Ag, Mg, Ni, Zn or Cu; the high-emission substrate is SiC, Fe2O3, SiO2 or polyimide.
Citation Information
Patent Citations
Self-adaptive thermal camouflage coating and preparation method thereof
CN107189552A
Flexible film with adjustable infrared emissivity and preparation method thereof
CN111077603A
Thermally-induced variable-emissivity intelligent temperature control coating based on VO2 core-shell structure
CN113185863A
High-transparency self-adaptive emissivity modulation coating as well as preparation method and application thereof
CN114918119A
Dynamic thermal radiation reconfigurable device based on vanadium dioxide and preparation method thereof
CN117434776A