Preparation process of wear-resistant epoxy resin for floor paint

By adding carboxydiphenyl ether dicarboximide epoxy monomer to the aqueous epoxy resin, a new epoxy resin with excellent heat resistance and impact toughness is generated through imide cyclization, etherification and closed-loop reactions. , solves the problem of poor wear resistance of traditional water-based epoxy resins and achieves better mechanical and high temperature resistance.

CN118879153AInactive Publication Date: 2024-11-01GUANGDONG GREEN TREE CHEM CO LTD

Patent Information

Application Number
CN202410896461.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-04
Publication Date
2024-11-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional water-based epoxy resins have problems with low wear resistance and low strength in floor paint, which is difficult to meet the practical application needs.

Method used

It is used to include 65-80 parts by weight of aqueous epoxy resin, 20-35 parts by weight of carboxydiphenyl ether dicarboximide epoxy monomer, 2-5 parts by weight of color paste, 0.3-0.6 parts by weight of defoaming agent, 0.15- The preparation process of 0.4 parts by weight leveling agent and 0.2-0.4 parts by weight emulsifier is produced by imide cyclization, etherification and closed-loop reaction to produce a new epoxy resin with excellent heat resistance and impact toughness.

Benefits of technology

Improve the mechanical properties, wear resistance and high temperature resistance of epoxy resin, with hardness reaching 2-3H, tensile strength reaching 46.3-54.7MPa, friction mass loss rate is only 25.4-28.3g/m2, 5% mass loss The temperature reaches 387.9-398.7℃, and it is suitable for floor paint and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004929588340000021
    Figure BDA0004929588340000021
  • Figure BDA0004929588340000022
    Figure BDA0004929588340000022
  • Figure BDA0004929588340000031
    Figure BDA0004929588340000031
Patent Text Reader

Abstract

The invention belongs to the technical field of epoxy resin, and particularly relates to a preparation process of wear-resistant epoxy resin for floor paint, which comprises the following components in parts by weight: 65-80 parts of water-borne epoxy resin, 20-35 parts of carboxyl diphenyl ether dicarboximide epoxy monomer, 2-5 parts of color paste, 0.3-0.6 part of defoaming agent, 0.15-0.4 part of flatting agent and 0.2-0.4 part of emulsifier. The carboxyl diphenyl ether dicarboximide epoxy monomer disclosed by the invention contains a plurality of epoxy groups, and the carboxyl diphenyl ether dicarboximide epoxy monomer and epoxy resin are subjected to cross-linking curing reaction under the action of a curing agent, so that rigid and thermal decomposition-resistant benzimide is bonded into an epoxy resin matrix, and the mechanical property, wear resistance, high temperature resistance and other properties are improved. Better practical application is realized in the aspects of floor paint, coating and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of epoxy resins, and in particular relates to a preparation process of wear-resistant epoxy resin for floor paint. Background Art

[0002] Floor paint is a type of floor decoration material, primarily including epoxy floor paint, polyurethane floor paint, acrylic floor paint, and cement self-leveling floor paint. Water-based epoxy resins, which use water as a solvent and are environmentally friendly, have excellent curing, mechanical, corrosion, and insulation properties, making them widely used. However, traditional water-based epoxy resins suffer from poor wear resistance and low strength, hindering their practical application in areas such as floor paint.

[0003] The development of new, high-performance water-based epoxy resins and their floor coating materials is a research hotspot. Patent application number 202310697730.0 discloses a novel epoxy resin containing an imide moiety and its preparation method. By reacting a diimide diphenol compound with an epoxyhalopropane, the resulting epoxy resin containing an imide moiety exhibits excellent heat resistance and impact toughness. However, this epoxy resin has poor water solubility, making it unsuitable for use in water-based epoxy resins. Summary of the Invention

[0004] The technical problem solved by the present invention is to provide a preparation process of wear-resistant epoxy resin for floor paint, solve the problems of poor high temperature resistance and poor wear resistance of epoxy resin, and enable epoxy resin to have better practical application in floor paint.

[0005] In order to solve the above technical problems, the technical solution of the present invention is: a preparation process of a wear-resistant epoxy resin for floor paint, characterized in that the wear-resistant epoxy resin for floor paint includes 65-80 parts by weight of water-based epoxy resin, 20-35 parts by weight of carboxyl diphenyl ether dicarboximide epoxy monomer, 2-5 parts by weight of color paste, 0.3-0.6 parts by weight of defoaming agent, 0.15-0.4 parts by weight of leveling agent, and 0.2-0.4 parts by weight of emulsifier.

[0006] The structural formula of carboxyl diphenyl ether dicarboximide epoxy monomer is:

[0007]

[0008] The preparation process of wear-resistant epoxy resin for floor paint is as follows: add water-based epoxy resin, carboxyl diphenyl ether dicarboximide epoxy monomer, color paste, defoamer, leveling agent, emulsifier and water into a container, disperse them evenly, and obtain wear-resistant epoxy resin for floor paint.

[0009] Preferably, the preparation process of carboxyl diphenyl ether dicarboximide epoxy monomer is as follows:

[0010] (1) Add N,N-dimethylformamide, 4,4'-biphenyl ether dianhydride, and methyl 3-amino-5-hydroxybenzoate to a reaction flask, first react at 20-30°C for 2-3 hours, then at 115-125°C for 10-18 hours, dilute with water, extract with ethyl acetate, combine the organic phases, distill under reduced pressure, wash with acetone, and dry to obtain the intermediate. The reaction formula is as follows:

[0011]

[0012] (2) Add epichlorohydrin, intermediate, and catalyst to the reaction flask, carry out etherification reaction at 65-75°C for 5-8h, then remove epichlorohydrin by vacuum distillation, add toluene and sodium hydroxide component 1, carry out ring closure reaction at 60-75°C for 2-4h, add water, and remove toluene by vacuum distillation, then add methanol and supplement sodium hydroxide component 2, carry out hydrolysis reaction at 70-80°C for 8-12h, add hydrochloric acid solution to control the pH of the reaction solution to 4-5, filter, wash the filter cake with acetone, and dry to obtain carboxyl diphenyl ether dicarboximide epoxy monomer. The reaction formula is as follows:

[0013]

[0014] Preferably, in (1), the ratio of 4,4'-biphenyl ether dianhydride to 3-amino-5-hydroxybenzoic acid methyl ester is 1 mol:(1.9-2.2) mol.

[0015] Preferably, the ratio of epichlorohydrin, intermediate, catalyst, sodium hydroxide component 1, and sodium hydroxide component 2 in (2) is (15-20) mol:1 mol:(0.018-0.026) mol:(4-5) mol:(8-11) mol.

[0016] Preferably, the catalyst is tetrabutylammonium bromide or tetraethylammonium bromide.

[0017] The present invention has the following technical effects: 4,4'-biphenyl ether dianhydride and 3-amino-5-hydroxybenzoic acid methyl ester are subjected to an imide cyclization reaction, and then etherification and ring-closure reactions are carried out with epichlorohydrin, and sodium hydroxide is further added to carry out a hydrolysis reaction to obtain a novel carboxyl biphenyl ether dicarboximide epoxy monomer.

[0018] The present invention adds a carboxyl diphenyl ether dicarboximide epoxy monomer to a water-based epoxy resin. The carboxyl diphenyl ether dicarboximide epoxy monomer contains multiple hydrophilic carboxyl groups and has good hydrophilicity. In addition, an emulsifier, sodium dodecylbenzene sulfonate, is added, which has a good interface effect with the carboxyl diphenyl ether dicarboximide epoxy monomer, thereby further improving the dispersibility of the emulsion in the epoxy resin. The emulsion is uniform and stable, has no precipitation, and has good storage stability.

[0019] The carboxyl diphenyl ether dicarboximide epoxy monomer of the present invention contains multiple epoxy groups. Under the action of a curing agent, it undergoes a cross-linking and curing reaction with the epoxy resin, thereby bonding the rigid and heat-resistant benzimide to the epoxy resin matrix, thereby improving mechanical, wear-resistant, and high-temperature resistance properties. The epoxy resin hardness reaches 2-3H, the tensile strength reaches 46.3-54.7MPa, and the friction mass loss rate is only 25.4-28.3g / m 2 , and the temperature of 5% mass loss reaches 387.9-398.7℃. It has better practical applications in floor paint, coatings, etc. DETAILED DESCRIPTION

[0020] The technical solution of the present invention is further described below by way of specific embodiments. It should be understood by those skilled in the art that the embodiments are merely to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0021] The water-based epoxy resin used in the embodiment of the present invention is CYDW-100, the color paste is BASF Lucony 1 water-based color paste, the defoamer is TEGO8030, and the leveling agent is Hongrun HR-6115.

[0022] Example 1

[0023] (1) Add 35 mL of N,N-dimethylformamide, 20 mmol of 4,4'-biphenyl ether dianhydride, and 44 mol of 3-amino-5-hydroxybenzoic acid methyl ester to the reaction flask, first react at 30°C for 2 hours, then at 120°C for 12 hours, add water to dilute, extract with ethyl acetate, combine the organic phases, distill under reduced pressure, wash with acetone, and dry to obtain the intermediate. The structural formula is as follows

[0024] (2) Add 180 mmol of epichlorohydrin, 10 mmol of the intermediate, and 0.2 mmol of the catalyst tetrabutylammonium bromide to the reaction flask, carry out etherification reaction at 75°C for 4 hours, then remove epichlorohydrin by vacuum distillation, add 40 mL of toluene and 40 mmol of sodium hydroxide, carry out ring closure reaction at 60°C for 3 hours, add 35 mL of water, and remove toluene by vacuum distillation, then add 35 mL of methanol and supplement with 100 mmol of sodium hydroxide, carry out hydrolysis reaction at 75°C for 8 hours, add hydrochloric acid solution to control the pH of the reaction solution to 5, filter, wash the filter cake with acetone, and dry to obtain carboxyl diphenyl ether dicarboximide epoxy monomer. The structural formula is as follows:

[0025]

[0026] (3) Add 800g of water-based epoxy resin, 200g of carboxyl diphenyl ether dicarboximide epoxy monomer, 50g of color paste, 4g of defoamer, 3g of leveling agent, 2g of emulsifier sodium dodecylbenzene sulfonate, and 1000mL of water into a container and disperse them evenly to obtain a wear-resistant epoxy resin for floor paint.

[0027] Example 2

[0028] (1) Add 40 mL of N,N-dimethylformamide, 20 mmol of 4,4'-biphenyl ether dianhydride, and 44 mol of 3-amino-5-hydroxybenzoic acid methyl ester to a reaction flask, first react at 25°C for 2 hours, then at 115°C for 18 hours, add water to dilute, extract with ethyl acetate, combine the organic phases, distill under reduced pressure, wash with acetone, and dry to obtain the intermediate.

[0029] (2) Add 150 mmol of epichlorohydrin, 10 mmol of the intermediate, and 0.26 mmol of the catalyst tetraethylammonium bromide to the reaction flask, carry out etherification reaction at 65°C for 8 hours, then remove the epichlorohydrin by vacuum distillation, add 60 mL of toluene and 50 mmol of sodium hydroxide, carry out ring closure reaction at 75°C for 2 hours, add 30 mL of water, and remove the toluene by vacuum distillation, then add 30 mL of methanol and supplement with 80 mmol of sodium hydroxide, carry out hydrolysis reaction at 70°C for 10 hours, add hydrochloric acid solution to control the pH of the reaction solution to 4, filter, wash the filter cake with acetone, and dry to obtain carboxyl diphenyl ether dicarboximide epoxy monomer.

[0030] (3) Add 750g of water-based epoxy resin, 250g of carboxyl diphenyl ether dicarboximide epoxy monomer, 20g of color paste, 3g of defoamer, 4g of leveling agent, 2.5g of emulsifier sodium dodecylbenzene sulfonate, and 1000mL of water into the container and disperse them evenly to obtain a wear-resistant epoxy resin for floor paint.

[0031] Example 3

[0032] (1) Add 30 mL of N,N-dimethylformamide, 20 mmol of 4,4'-biphenyl ether dianhydride, and 38 mol of methyl 3-amino-5-hydroxybenzoate to a reaction flask, first react at 20°C for 3 hours, then at 125°C for 12 hours, add water to dilute, extract with ethyl acetate, combine the organic phases, distill under reduced pressure, wash with acetone, and dry to obtain the intermediate.

[0033] (2) Add 200 mmol of epichlorohydrin, 10 mmol of the intermediate, and 0.18 mmol of the catalyst tetrabutylammonium bromide to the reaction flask, carry out etherification reaction at 70°C for 5 hours, then remove the epichlorohydrin by vacuum distillation, add 35 mL of toluene and 40 mmol of sodium hydroxide, carry out ring closure reaction at 60°C for 4 hours, add 40 mL of water, and remove the toluene by vacuum distillation, then add 40 mL of methanol and supplement with 110 mmol of sodium hydroxide, carry out hydrolysis reaction at 80°C for 8 hours, add hydrochloric acid solution to control the pH of the reaction solution to 5, filter, wash the filter cake with acetone, and dry to obtain carboxyl diphenyl ether dicarboximide epoxy monomer.

[0034] (3) The preparation process of wear-resistant epoxy resin for floor paint is as follows: add 700g water-based epoxy resin, 300g carboxyl diphenyl ether dicarboximide epoxy monomer, 40g color paste, 6g defoamer, 1.5g leveling agent, 3g emulsifier sodium dodecylbenzene sulfonate, and 1000mL water into a container, disperse evenly, and obtain wear-resistant epoxy resin for floor paint.

[0035] Example 4

[0036] (1) Add 30 mL of N,N-dimethylformamide, 20 mmol of 4,4'-biphenyl ether dianhydride, and 40 mol of methyl 3-amino-5-hydroxybenzoate to a reaction flask, first react at 20°C for 3 hours, then at 125°C for 10 hours, add water to dilute, extract with ethyl acetate, combine the organic phases, distill under reduced pressure, wash with acetone, and dry to obtain the intermediate.

[0037] (2) Add 150 mmol of epichlorohydrin, 10 mmol of the intermediate, and 0.2 mmol of the catalyst tetrabutylammonium bromide to the reaction flask, carry out etherification reaction at 75°C for 6 hours, then remove the epichlorohydrin by vacuum distillation, add 40 mL of toluene and 40 mmol of sodium hydroxide, carry out ring-closure reaction at 60°C for 4 hours, add 35 mL of water, and remove the toluene by vacuum distillation, then add 35 mL of methanol and supplement with 100 mmol of sodium hydroxide, carry out hydrolysis reaction at 75°C for 12 hours, add hydrochloric acid solution to control the pH of the reaction solution to 4, filter, wash the filter cake with acetone, and dry to obtain carboxyl diphenyl ether dicarboximide epoxy monomer.

[0038] (3) Add 650g of water-based epoxy resin, 350g of carboxyl diphenyl ether dicarboximide epoxy monomer, 20g of color paste, 5g of defoamer, 2g of leveling agent, 4g of emulsifier sodium dodecylbenzene sulfonate, and 1000mL of water into the container and disperse them evenly to obtain a wear-resistant epoxy resin for floor paint.

[0039] Comparative Example 1

[0040] The difference between Comparative Example 1 and Example 1 is that no carboxyl diphenyl ether dicarboximide epoxy monomer is added.

[0041] Add 800g of water-based epoxy resin, 50g of color paste, 4g of defoamer, 3g of leveling agent, 2g of emulsifier sodium dodecylbenzenesulfonate, and 1000mL of water into a container and disperse them evenly to obtain a wear-resistant epoxy resin for floor paint.

[0042] Comparative Example 2

[0043] The difference between Comparative Example 2 and Example 1 is that the intermediate Replace carboxyl diphenyl ether dicarboximide epoxy monomer.

[0044] Add 800g of water-based epoxy resin, 200g of intermediate, 50g of color paste, 4g of defoamer, 3g of leveling agent, 2g of emulsifier sodium dodecylbenzene sulfonate, and 1000mL of water into a container and disperse them evenly to obtain a wear-resistant epoxy resin for floor paint.

[0045] Comparative Example 3

[0046] The difference between Comparative Example 3 and Example 1 is that the intermediate product of the ring-closure reaction is Replace carboxyl diphenyl ether dicarboximide epoxy monomer.

[0047] (1) Add 180 mmol of epichlorohydrin, 10 mmol of the intermediate, and 0.2 mmol of the catalyst tetrabutylammonium bromide to a reaction flask, carry out etherification reaction at 75°C for 4 hours, then remove epichlorohydrin by vacuum distillation, add 40 mL of toluene and 40 mmol of sodium hydroxide, carry out ring closure reaction at 60°C for 3 hours, filter, and vacuum distill the filtrate, wash with acetone, and dry to obtain the ring closure reaction intermediate product.

[0048] (2) Add 800g of water-based epoxy resin, 200g of closed-loop reaction intermediate product, 50g of color paste, 4g of defoamer, 3g of leveling agent, 2g of emulsifier sodium dodecylbenzene sulfonate, and 1000mL of water into a container and disperse them evenly to obtain a wear-resistant epoxy resin for floor paint.

[0049] Storage stability test of epoxy resin: Place the floor paint with wear-resistant epoxy resin at room temperature for 6 months and observe the emulsion condition.

[0050] Table 1 Stability of epoxy resin emulsion

[0051] Emulsion stability Example 1 The emulsion is uniform and stable without precipitation Example 2 The emulsion is uniform and stable without precipitation Example 3 The emulsion is uniform and stable without precipitation Example 4 The emulsion is uniform and stable without precipitation Comparative Example 1 The emulsion is uniform and stable without precipitation Comparative Example 2 There is obvious sediment Comparative Example 3 There is obvious sediment

[0052] As can be seen from Table 1, the epoxy resin emulsions of Examples 1-4 are uniform and stable, free of precipitation, and have good dispersibility and storage stability. This is because the carboxyl diphenyl ether dicarboximide epoxy monomer contains multiple hydrophilic carboxyl groups, which makes it have good hydrophilicity, and the addition of the emulsifier sodium dodecylbenzene sulfonate has a good interfacial effect with the carboxyl diphenyl ether dicarboximide epoxy monomer, further improving its dispersibility in the epoxy resin, and the emulsion is uniform and stable without precipitation.

[0053] In Comparative Example 1, no carboxyl diphenyl ether dicarboximide epoxy monomer was added, and the emulsion was uniform and stable without precipitation.

[0054] The intermediate added in Comparative Example 2 and the ring-closure reaction intermediate product added in Comparative Example 3 do not contain carboxyl groups, have poor hydrophilicity, are poorly dispersible in the aqueous epoxy resin emulsion, easily form precipitates, and result in poor storage stability of the emulsion.

[0055] To a wear-resistant epoxy resin for floor paint, 360g of a cycloaliphatic amine curing agent (Baxxodur EC330) and 72g of alkyl glycidyl ether (AGE) diluent were added. The mixture was cured at 25°C for 24h and then at 80°C for 6h. The hardness of the epoxy resin film was tested according to GB / T 6739-2022. The tensile strength of the epoxy resin casting was tested according to GB / T 2567-2021.

[0056] The wear resistance of epoxy resin castings was tested using a friction and wear tester. A 45 steel ring was used as the wear partner, the load was 19.6N, and the friction speed was 200r / min. The mass loss rate was calculated. The lower the mass loss rate, the better the wear resistance.

[0057] Mass loss rate = (m-m1) / (L×d). m is the mass of the test block before wear, m1 is the mass of the test block after wear, L is the width of the test block, and d is the width of the wear scar.

[0058] 5 mg of the epoxy resin casting was weighed and placed in a thermogravimetric analyzer. The thermal decomposition temperature was measured in a nitrogen atmosphere by heating from room temperature to 700° C. at a heating rate of 10° C. / min.

[0059] Table 2 Epoxy resin performance test

[0060]

[0061] As shown in Table 2, the epoxy resin hardness of Examples 1-4 reaches 2-3H, the tensile strength reaches 46.3-54.7 MPa, and the friction mass loss rate is only 25.4-28.3 g / m 2The material exhibits excellent mechanical properties, wear resistance, and high-temperature resistance, with a 5% mass loss temperature of 387.9-398.7°C. This is due to the addition of a carboxydiphenyl ether dicarboximide epoxy monomer, which contains multiple epoxy groups. Under the action of a curing agent, it undergoes a cross-linking and curing reaction with the epoxy resin, thereby bonding the rigid and thermally decomposition-resistant phenylimide to the epoxy resin matrix, thereby improving mechanical, wear resistance, and high-temperature resistance.

[0062] Comparative Example 1 did not add carboxyl diphenyl ether dicarboximide epoxy monomer, the hardness and tensile strength of the epoxy resin were low, and the mass loss rate reached 32.6g / m 2 , the wear resistance is poor, and the temperature of 5% mass loss is 372.4℃, and the high temperature resistance is not good.

[0063] The intermediate added in Comparative Example 2 It does not contain epoxy groups and is difficult to undergo cross-linking and curing reaction with epoxy resin, and has little effect on the hardness, tensile strength and thermal decomposition temperature of epoxy resin.

[0064] The intermediate product of the ring-closure reaction added in Comparative Example 3 It contains epoxy groups and can undergo a cross-linking and curing reaction with epoxy resin under the action of a curing agent, thereby bonding the rigid and thermally decomposition-resistant phenylimide to the epoxy resin matrix, which is beneficial to improving mechanical, wear-resistant and high-temperature resistance properties.

[0065] Those skilled in the art will appreciate that, based on the teachings of this specification, some modifications or adjustments may be made to the present invention, and these modifications or adjustments should also be within the scope defined by the claims of the present invention.

Claims

1. A preparation process of a wear-resistant epoxy resin for floor paint, characterized in that: The wear-resistant epoxy resin for floor paint comprises 65-80 parts by weight of waterborne epoxy resin, 20-35 parts by weight of carboxyl biphenyl ether dicarboximide epoxy monomer, 2-5 parts by weight of color paste, 0.3-0.6 parts by weight of defoamer, 0.15-0.4 parts by weight of leveling agent, and 0.2-0.4 parts by weight of emulsifier; The structural formula of the carboxyl diphenyl ether dicarboximide epoxy monomer is: The preparation process of the wear-resistant epoxy resin for floor paint is as follows: add water-based epoxy resin, carboxyl diphenyl ether dicarboximide epoxy monomer, color paste, defoamer, leveling agent, emulsifier and water into a container, disperse evenly, and obtain the wear-resistant epoxy resin for floor paint.

2. The preparation process of the wear-resistant epoxy resin for floor paint according to claim 1, characterized in that: The preparation process of the carboxyl diphenyl ether dicarboximide epoxy monomer is as follows: (1) Add N,N-dimethylformamide, 4,4'-biphenyl ether dianhydride, and 3-amino-5-hydroxybenzoic acid methyl ester to a reaction flask, add water to dilute after the reaction, extract with ethyl acetate, combine the organic phases, distill under reduced pressure, wash with acetone, and dry to obtain an intermediate; (2) Add epichlorohydrin, an intermediate, and a catalyst to a reaction flask to carry out an etherification reaction, then remove epichlorohydrin by distillation under reduced pressure, add toluene and sodium hydroxide component 1 to carry out a ring-closing reaction, add water, and remove toluene by distillation under reduced pressure, then add methanol, and supplement sodium hydroxide component 2 to carry out a hydrolysis reaction, add hydrochloric acid solution to control the pH of the reaction solution to 4-5, filter with suction, wash the filter cake with acetone, and dry to obtain a carboxydiphenyl ether dicarboximide epoxy monomer.

3. The preparation process of the wear-resistant epoxy resin for floor paint according to claim 2, characterized in that: In the above (1), the ratio of 4,4'-biphenyl ether dianhydride to 3-amino-5-hydroxybenzoic acid methyl ester is 1 mol:(1.9-2.2) mol.

4. The preparation process of the wear-resistant epoxy resin for floor paint according to claim 2, characterized in that: The reaction in (1) is first carried out at 20-30°C for 2-3 hours, and then at 115-125°C for 10-18 hours.

5. The preparation process of the wear-resistant epoxy resin for floor paint according to claim 2, characterized in that: The ratio of epichlorohydrin, intermediate, catalyst, sodium hydroxide component 1 and sodium hydroxide component 2 in (2) is (15-20) mol: 1 mol: (0.018-0.026) mol: (4-5) mol: (8-11) mol.

6. The preparation process of the wear-resistant epoxy resin for floor paint according to claim 5, characterized in that: The catalyst is tetrabutylammonium bromide or tetraethylammonium bromide.

7. The preparation process of the wear-resistant epoxy resin for floor paint according to claim 2, characterized in that: The temperature of the etherification reaction in (2) is 65-75°C, and the reaction time is 5-8h.

8. The preparation process of the wear-resistant epoxy resin for floor paint according to claim 2, characterized in that: The temperature of the ring-closing reaction in (2) is 60-75°C, and the reaction time is 2-4h.

9. The preparation process of the wear-resistant epoxy resin for floor paint according to claim 2, characterized in that: The temperature of the hydrolysis reaction in (2) is 70-80°C, and the reaction time is 8-12h.

Citation Information

Patent Citations

  • Novel epoxy resin containing imide element and preparation method thereof

    CN116854679A

  • Isocyanurate epoxy compound having alkoxysilyl group, method of preparing same, composition including same, cured product of the composition, and use of the composition

    CN103906753A

  • Super-wear-resistant waterborne dual-component epoxy floor coating

    CN108102509A

  • FPC electromagnetic shielding film with polyimide film as insulating layer and preparation method thereof

    CN108976457A

  • Heavy-duty anti-corrosion environment-friendly water-based industrial coating and preparation method thereof

    CN113527985A

Cited By

  • Imide derivative monomer containing electroactive group as well as preparation method and application of imide derivative monomer