Self-repairing easy-to-clean coating material as well as preparation method and application thereof
Through the combination of catechin-modified perfluoropolyether siloxane and polydopamine microcapsules, coatings with high hardness, hydrophobicity, antibacteriality and self-healing properties have been developed, solving existing easy-to-clean coatings in kitchens It is difficult to completely remove stubborn oil stains and insufficient durability in electrical products, which significantly improves the product's performance and life.
Patent Information
- Application Number
- CN202411212578.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-08-30
AI Technical Summary
The existing easy-to-clean coating is difficult to completely remove stubborn oil stains in kitchen appliances, and is easily damaged by oxidizing substances such as light and ozone. The single superhydrophobic performance is not enough to meet the increasing demands of the use environment.
Self-healing and easy-to-clean coating material combined with catechin-modified perfluoropolyether siloxane and polydopamine microcapsules is formed with high levels of antibacterial modification of catechin and hydrophobic effect of polyalkyl organometallic salts. Coatings with hardness, excellent hydrophobicity, antibacteriality and self-healing properties.
It significantly improves the service performance and service life of kitchen appliances. The coating has self-healing function under high temperature conditions, maintains excellent hydrophobicity and antibacterial properties, and can effectively resist external environmental influences.
Smart Images

Figure BDA0005020669770000041 
Figure BDA0005020669770000101 
Figure BDA0005020669770000111
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of coatings, and in particular relates to a self-repairing and easy-to-clean coating material and a preparation method and application thereof. Background Art
[0002] Kitchen appliances are in a heavy oil fume environment for a long time, and are exposed to oil fume, acidic and alkaline ingredients, seasonings and other pollutants for a long time. It is very easy for grease or food residues to adhere to the surface and inner cavity of kitchen appliances. Over time, they will become a breeding ground for microorganisms such as bacteria and mold, which will produce odor, pose a serious health hazard, and the user experience is extremely poor.
[0003] Stainless steel is a common substrate for kitchen appliances. How to make the stainless steel surface easy to clean is the goal pursued by the industry. At present, the common easy-to-clean coating technology mainly includes hydrophobic non-stick coatings. Hydrophobic non-stick coatings include fluorocarbon coatings, UV light-cured fluorocarbon coatings, silicone coatings, etc. The resin structure of these coatings contains rich fluorosilicon groups, which tend to migrate to the surface after the coating is cured. The fluorosilicon groups that migrate to the surface have lower surface energy. This type of coating uses this low surface energy characteristic to achieve the effect of low adhesion to oil stains.
[0004] However, the oil contact angle of existing low surface energy coatings on the market is mostly less than 90°, and they are not truly oleophobic, so oil stains will still adhere to the surface, and it is difficult to thoroughly clean stubborn oil stains such as those on the stainless steel surface of range hoods. In addition, during the use of hydrophobic and easy-to-clean coatings, their surfaces are extremely susceptible to chemical damage caused by oxidizing substances such as light and ozone, as well as coating damage caused by external forces, resulting in failure. At the same time, with the rapid development of science and technology, coating materials with only a single super-hydrophobic and easy-to-clean property can no longer meet the increasingly improved product use environment.
[0005] Based on the above problems, in order to improve the overall performance of kitchen appliances, it is of great practical significance to develop a self-healing and easy-to-clean coating material that has excellent hydrophobicity, wipe resistance and antibacterial properties after curing to form a coating. Summary of the invention
[0006] In view of the deficiencies in the prior art, the object of the present invention is to provide a self-repairing and easy-to-clean coating material and a preparation method and application thereof. The self-repairing and easy-to-clean coating material has excellent bonding properties with a stainless steel substrate, and the coating formed after curing has high hardness, excellent hydrophobicity, scratch resistance, antibacterial properties and self-repairing properties, thereby effectively protecting the stainless steel substrate and improving the performance and service life of kitchen appliances.
[0007] To achieve this object, the present invention adopts the following technical solutions:
[0008] In a first aspect, the present invention provides a self-repairing and easy-to-clean coating material, wherein the self-repairing and easy-to-clean coating material comprises catechin-modified perfluoropolyether siloxane, polydopamine microcapsules and fluorine solvent A;
[0009] The shell material of the polydopamine microcapsule comprises polydopamine, and the core material comprises polyalkyl organic metal salt.
[0010] First, the self-repairing easy-to-clean coating material provided by the present invention includes catechin-modified perfluoropolyether siloxane; wherein perfluoropolyether siloxane generally refers to a type of polymer whose main chain contains repeated COC ether bonds and in which all hydrogen atoms in the main chain are replaced by fluorine atoms. The special molecular structure gives it extremely low surface tension (about 11-22 mN / m), good hydrophobic and oleophobic properties, low friction coefficient and other characteristics. It is used as a substrate and modified with natural catechin as an antibacterial agent to prepare catechin-modified perfluoropolyether siloxane, which can effectively improve the antibacterial properties of the coating, and further improve the hydrophobic and oleophobic properties and scratch resistance of the surface of the coating material;
[0011] Secondly, the self-repairing easy-to-clean coating material provided by the present invention also includes polydopamine microcapsules, and the shell material of the polydopamine microcapsules is limited to include polydopamine, and the core material includes an organic metal salt; it is understood that the microcapsule technology uses phase polymerization, in-situ polymerization and interfacial polymerization technology to wrap the modifier with a polymer material to form a composite modifier with a coating structure, which can prevent the influence of the external environment, and the microcapsules have a smaller size and a larger specific surface area, which can be more compatible with the matrix material, and due to the protective effect of the wall material on the core material, the core material loss can be reduced, further improving the performance;
[0012] The present invention adds polydopamine microcapsules with polydopamine as shell material and polyalkyl organic metal salt as core material; wherein dopamine (DA) is a synthetic mussel adhesive protein, which is easily oxidized and spontaneously polymerized to generate polydopamine (PDA) under alkaline conditions (pH value greater than 7.5), and the PDA can achieve a strong adhesion deposition effect by forming hydrogen bonds, metal ligands and quinone charge transfer complexes without any complex instruments or harsh reaction conditions; and the polyalkyl organic metal salt has a non-polar long-chain structure and an excellent hydrophobic effect. After the coating is damaged, the polyalkyl organic metal salt hidden in the PDA escapes under high temperature conditions, thereby enabling the coating to have a self-repairing function.
[0013] In summary, the present invention uses the above two materials in combination, so that the obtained self-repairing and easy-to-clean coating material has excellent bonding properties with the stainless steel substrate, and the coating formed after curing has high hardness, excellent hydrophobicity, scratch resistance, antibacterial and self-repairing properties, which can effectively protect the stainless steel substrate and improve the performance and service life of kitchen appliances.
[0014] Preferably, the self-repairing easy-to-clean coating material comprises the following components in parts by weight:
[0015] 5 to 10 parts by weight of catechin-modified perfluoropolyether siloxane;
[0016] 10-20 parts by weight of polydopamine microcapsules;
[0017] Fluorinated solvent A 60-70 parts by weight
[0018] Wherein, the amount of the catechin-modified perfluoropolyether siloxane can be 5 parts by weight, 5.5 parts by weight, 6 parts by weight, 6.5 parts by weight, 7 parts by weight, 7.5 parts by weight, 8 parts by weight, 8.5 parts by weight, 9 parts by weight, 9.5 parts by weight or 10 parts by weight, etc.
[0019] The amount of the polydopamine microcapsules can be 10 parts by weight, 11 parts by weight, 12 parts by weight, 13 parts by weight, 14 parts by weight, 15 parts by weight, 16 parts by weight, 17 parts by weight, 18 parts by weight, 19 parts by weight or 20 parts by weight, etc.
[0020] The amount of the fluorinated solvent A can be 60 parts by weight, 61 parts by weight, 62 parts by weight, 63 parts by weight, 64 parts by weight, 65 parts by weight, 66 parts by weight, 67 parts by weight, 68 parts by weight, 69 parts by weight or 70 parts by weight.
[0021] Preferably, the raw materials for preparing the catechin-modified perfluoropolyether siloxane include the following components in parts by weight:
[0022]
[0023] The content of the perfluoropolyether acyl fluoride may be 180 parts by weight, 185 parts by weight, 190 parts by weight, 195 parts by weight, 200 parts by weight, 205 parts by weight, 210 parts by weight, 215 parts by weight or 220 parts by weight.
[0024] The content of the anhydrous ethanol can be 10 parts by weight, 11 parts by weight, 12 parts by weight, 13 parts by weight, 14 parts by weight, 15 parts by weight, 16 parts by weight, 17 parts by weight, 18 parts by weight, 19 parts by weight, 20 parts by weight, 22 parts by weight, 24 parts by weight, 26 parts by weight, 28 parts by weight or 30 parts by weight, etc.
[0025] The amount of the silane coupling agent can be 10 parts by weight, 11 parts by weight, 12 parts by weight, 13 parts by weight, 14 parts by weight, 15 parts by weight, 16 parts by weight, 17 parts by weight, 18 parts by weight, 19 parts by weight or 20 parts by weight, etc.
[0026] The content of the catechins may be 20 parts by weight, 21 parts by weight, 22 parts by weight, 23 parts by weight, 24 parts by weight, 25 parts by weight, 26 parts by weight, 27 parts by weight, 28 parts by weight, 29 parts by weight or 30 parts by weight.
[0027] Preferably, the silane coupling agent includes any one of γ-aminopropyldiethoxysilane, γ-glycidyloxypropyltrimethoxysilane or γ-(methacryloyloxy)propyltrimethoxysilane, or a combination of at least two thereof.
[0028] Preferably, the catechin compound includes any one of catechin, epicatechin, gallocatechin or catechin gallate, or a combination of at least two thereof.
[0029] Preferably, the catechin-modified perfluoropolyether siloxane is prepared by the following method, which comprises the following steps:
[0030] (A1) reacting perfluoropolyether acyl fluoride and anhydrous ethanol in a fluorine solvent B, followed by cooling, washing, drying, filtering and distilling to obtain perfluoropolyether methyl ester;
[0031] (A2) reacting perfluoropolyether methyl ester and a silane coupling agent, adding anhydrous ethanol and a fluorinated solvent C to mix, standing to separate the liquids, and removing the lower layer of liquid for vacuum distillation to obtain perfluoropolyether siloxane;
[0032] (A3) Mixing perfluoropolyether siloxane and a catechin compound in a fluorinated solvent D to obtain the catechin-modified perfluoropolyether siloxane.
[0033] Preferably, the reaction in step (A1) comprises two stages, stage 1 is to react at room temperature for 1 to 2 h (e.g., 1 h, 1.2 h, 1.4 h, 1.6 h, 1.8 h or 2 h, etc.), and stage 2 is to heat the reaction to 50 to 70 ° C (e.g., 50 ° C, 52 ° C, 54 ° C, 56 ° C, 58 ° C, 60 ° C, 62 ° C, 64 ° C, 66 ° C, 68 ° C or 70 ° C, etc.) for 1 to 2 h (e.g., 1 h, 1.2 h, 1.4 h, 1.6 h, 1.8 h or 2 h, etc.).
[0034] Preferably, the reaction temperature in step (A2) is 50-70°C, for example, 50°C, 52°C, 54°C, 56°C, 58°C, 60°C, 62°C, 64°C, 66°C, 68°C or 70°C, etc.
[0035] Preferably, the reaction time of step (A2) is 2 to 4 h, for example, 2 h, 2.2 h, 2.4 h, 2.6 h, 2.8 h, 3 h, 3.2 h, 3.4 h, 3.6 h, 3.8 h or 4 h.
[0036] Preferably, the reaction in step (A2) is carried out under nitrogen protection.
[0037] Preferably, the mixing temperature in step (A3) is 30-35°C, for example, 30°C, 31°C, 32°C, 33°C, 34°C or 35°C.
[0038] Preferably, the mixing time in step (A3) is 20 to 40 min, for example, 20 min, 24 min, 26 min, 28 min, 30 min, 32 min, 34 min, 36 min, 38 min or 40 min.
[0039] Preferably, the raw materials for preparing the polydopamine microcapsules include the following components in parts by weight:
[0040] 100 parts by weight of polyalkyl organic metal salt;
[0041] Dopamine 70-90 parts by weight.
[0042] Wherein, the content of dopamine can be 70 parts by weight, 72 parts by weight, 74 parts by weight, 76 parts by weight, 78 parts by weight, 80 parts by weight, 82 parts by weight, 84 parts by weight, 86 parts by weight, 88 parts by weight or 90 parts by weight, etc.
[0043] Preferably, the polyalkyl organic metal salt includes any one of sodium octane sulfonate and sodium dodecyl sulfonate, sodium dodecyl sulfonate, sodium polystyrene sulfonate or polydiallyldimethylammonium chloride, or a combination of at least two thereof.
[0044] Preferably, the preparation method of the polydopamine microcapsules comprises: dissolving a polyalkyl organic metal salt in a buffer solution, adding dopamine and mixing, to obtain the polydopamine microcapsules.
[0045] Preferably, the buffer comprises Tris-HCl buffer.
[0046] Preferably, the pH value of the buffer solution is 8-9, such as 8, 8.2, 8.4, 8.6, 8.8 or 9.
[0047] Preferably, the mixing temperature is 40-60°C, for example, 40°C, 42°C, 44°C, 46°C, 48°C, 50°C, 52°C, 54°C, 56°C, 58°C or 60°C, etc.
[0048] Preferably, the mixing time is 20 to 30 hours, for example, 20 hours, 22 hours, 24 hours, 26 hours, 28 hours or 30 hours.
[0049] Preferably, the fluorine solvent A, fluorine solvent B, fluorine solvent C and fluorine solvent D each independently include any one of perfluorohexane, perfluorocyclohexane, perfluoromethylcyclohexane, perfluorotoluene or perfluoroheptane, or a combination of at least two thereof.
[0050] In a second aspect, the present invention provides a method for preparing the self-repairing and easy-to-clean coating material as described in the first aspect, the preparation method comprising: uniformly mixing catechin-modified perfluoropolyether siloxane, polydopamine microcapsules and fluorine solvent A to obtain the self-repairing and easy-to-clean coating material.
[0051] In a third aspect, the present invention provides a method for using the self-repairing, easy-to-clean coating material as described in the first aspect, the method comprising: coating the self-repairing, easy-to-clean coating material on the surface of a stainless steel plate, and forming a self-repairing, easy-to-clean coating on the stainless steel plate after drying and curing.
[0052] Preferably, the drying temperature is 20-40°C, for example, 20°C, 22°C, 24°C, 26°C, 28°C, 30°C, 32°C, 34°C, 36°C, 38°C or 40°C.
[0053] Preferably, the drying time is 5 to 10 min, for example, 5 min, 6 min, 7 min, 8 min, 9 min or 10 min.
[0054] Preferably, the curing temperature is 120-140°C, for example, 120°C, 124°C, 128°C, 132°C, 135°C, 138°C or 140°C.
[0055] Preferably, the curing time is 40 to 60 min, for example, 40 min, 42 min, 44 min, 46 min, 48 min, 50 min, 52 min, 54 min, 56 min, 58 min or 60 min.
[0056] In a fourth aspect, the present invention provides a use of the self-repairing and easy-to-clean coating material as described in the first aspect in a kitchen appliance product.
[0057] Compared with the prior art, the present invention has the following beneficial effects:
[0058] The self-repairing and easy-to-clean coating material provided by the present invention comprises catechin-modified perfluoropolyether siloxane, polydopamine microcapsules and fluorine solvent A, and the shell material of the polydopamine microcapsules comprises polydopamine, and the core material comprises a polyalkyl organic metal salt; by selecting the catechin-modified perfluoropolyether siloxane as the matrix and adding the polydopamine microcapsules, the obtained self-repairing and easy-to-clean coating material has good bonding properties with the stainless steel substrate, and the coating has high hardness, excellent hydrophobicity, self-repairing and antibacterial properties. After being coated on the surface of the stainless steel substrate, the stainless steel substrate can be effectively protected, thereby effectively improving the performance and service life of kitchen appliances. DETAILED DESCRIPTION
[0059] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0060] Preparation Example 1-1
[0061] A polydopamine microcapsule, the preparation method of which comprises: adding 100 parts by weight of sodium dodecyl sulfate into 60 mL of tris(hydroxymethylaminomethane) hydrochloride solution with a pH of 8, subjecting the solution to ultrasonic treatment for 20 minutes to form a white emulsion, then adding 80 parts by weight of dopamine hydrochloride, stirring the mixture at 50°C for 24 hours to obtain a polydopamine microcapsule solution.
[0062] Preparation Example 1-2
[0063] A polydopamine microcapsule, the preparation method of which comprises: adding 100 parts by weight of sodium dodecyl sulfate into 60 mL of tris(hydroxymethylaminomethane) hydrochloride solution with a pH of 8, subjecting the solution to ultrasonic treatment for 20 minutes to form a white emulsion, then adding 75 parts by weight of dopamine hydrochloride, stirring the mixture at 50°C for 24 hours to obtain a polydopamine microcapsule solution.
[0064] Preparation Example 1-3
[0065] A polydopamine microcapsule, the preparation method of which comprises: adding 100 parts by weight of sodium dodecyl sulfate into 60 mL of tris(hydroxymethylaminomethane) hydrochloride solution with a pH of 8, subjecting the solution to ultrasonic treatment for 20 minutes to form a white emulsion, then adding 85 parts by weight of dopamine hydrochloride, stirring the mixture at 50°C for 24 hours to obtain a polydopamine microcapsule solution.
[0066] Preparation Example 1-4
[0067] A polydopamine microcapsule, the preparation method of which comprises: adding 100 parts by weight of sodium dodecyl sulfate into 60 mL of tris(hydroxymethylaminomethane) hydrochloride solution with a pH of 8, subjecting the solution to ultrasonic treatment for 20 minutes to form a white emulsion, then adding 60 parts by weight of dopamine hydrochloride, stirring the mixture at 50°C for 24 hours to obtain a polydopamine microcapsule solution.
[0068] Preparation Example 1-5
[0069] A polydopamine microcapsule, the preparation method of which comprises: adding 100 parts by weight of sodium dodecyl sulfate into 60 mL of tris(hydroxymethylaminomethane) hydrochloride solution with a pH of 8, subjecting the solution to ultrasonic treatment for 20 minutes to form a white emulsion, then adding 100 parts by weight of dopamine hydrochloride, stirring the mixture at 50°C for 24 hours to obtain a polydopamine microcapsule solution.
[0070] Preparation Example 2-1
[0071] A catechin-modified perfluoropolyether siloxane, the preparation method of which comprises the following steps:
[0072] (1) 200 parts by mass of perfluoropolyether acyl fluoride is dissolved in 400 parts by mass of perfluorohexane, 10 parts by mass of anhydrous ethanol is added dropwise, and the mixture is stirred at room temperature for 1.5 hours, and then the mixture is heated to 60° C. for 1.5 hours. After the reaction is completed, the mixture is cooled to room temperature, filtered, and the solvent is distilled off to obtain perfluoropolyether methyl ester;
[0073] (2) Then, 12 parts by weight of KH550 silane coupling agent was added to the perfluoropolyether methyl ester, and the mixture was reacted at 60° C. for 3 h under nitrogen protection, and then cooled to room temperature, 23 parts by weight of anhydrous ethanol and 167 parts by weight of perfluorohexane were added, and the mixture was allowed to stand for separation, the lower layer of liquid was taken out, and the solvent was evaporated under reduced pressure to obtain a colorless and transparent perfluoropolyether siloxane;
[0074] (3) Then, 20 parts by weight of catechin (290.27 g / mol) was added to 50 parts by weight of fluorohexane to obtain a mixed solvent, which was evenly stirred and added to the perfluoropolyether siloxane. The mixture was stirred at 30° C. for 30 min to obtain catechin-modified perfluoropolyether siloxane.
[0075] Comparative Preparation Example 2-1
[0076] A perfluoropolyether siloxane, the preparation method of which comprises the following steps:
[0077] (1) 200 parts by weight of perfluoropolyether acyl fluoride is dissolved in 400 parts by weight of perfluorohexane, 10 parts by weight of anhydrous ethanol is added dropwise, and the mixture is stirred and reacted at room temperature for 1.5 hours, and then the mixture is heated to 60° C. and reacted for 1.5 hours, and then cooled to room temperature, and the solvent is removed by filtration and distillation to obtain perfluoropolyether methyl ester;
[0078] (2) 12 parts by weight of KH550 silane coupling agent was added to perfluoropolyether methyl ester, and the mixture was reacted at 60° C. for 3 h under nitrogen protection. The mixture was then cooled to room temperature, and 23 parts by weight of anhydrous ethanol and 167 parts by weight of perfluorohexane were added. The mixture was allowed to stand for separation, and the lower layer of liquid was taken out. The solvent was evaporated under reduced pressure to obtain a colorless and transparent perfluoropolyether siloxane.
[0079] Examples 1 to 7 and Comparative Examples 1 to 3
[0080] Examples 1 to 7 and Comparative Examples 1 to 3 respectively provide a self-repairing easy-to-clean coating material, the components contained therein are shown in Table 1. In Table 1, the dosage units of each component are parts by weight;
[0081] Table 1
[0082]
[0083] The preparation method of the self-repairing easy-to-clean coating material provided in Examples 1 to 7 and Comparative Examples 1 to 3 includes: firstly mixing the fluorine solvent A and the perfluoropolyether siloxane, adding the polydopamine microcapsules and stirring them thoroughly for 1 minute to obtain the self-repairing easy-to-clean coating material.
[0084] Performance Test:
[0085] The stainless steel plate was ultrasonically cleaned with acetone, anhydrous ethanol and deionized water respectively, and dried at 100°C for standby use, the self-repairing easy-to-clean coating material was sprayed on the surface of the cleaned stainless steel plate, and then placed in an oven at room temperature for 5 minutes, and cured at 130°C for 40 minutes to form a self-repairing easy-to-clean coating on the surface of the stainless steel plate; the formed self-repairing easy-to-clean coating was tested in the following manner;
[0086] (1) Hardness: Tested in accordance with GB / T 6739;
[0087] (2) Water contact angle: The water contact angle of the coating surface was tested according to GB / T 24368-2009;
[0088] (3) Coating adhesion: Tested in accordance with the provisions of GB / T 9286;
[0089] (4) Wipe resistance: Wipe the coating of the specimen with a scouring pad with water at a force of 10 N. One round trip is counted as one time, and a total of 3000 wipes are made. After the test is completed, wipe the coating surface clean and test the water contact angle.
[0090] (5) Self-healing performance: The coating that has undergone the wipe resistance test was placed in an environmental chamber at 120°C for 20 minutes, then the sample was taken out and cooled to room temperature, and the water contact angle of the surface coating was tested;
[0091] (6) Antibacterial properties: Tested in accordance with the provisions of GB 21551.2-2010, including the antibacterial rate of the material against Escherichia coli.
[0092] The self-repairing and easy-to-clean coating materials provided in Examples 1 to 7 and Comparative Examples 1 to 3 were tested according to the above test method. The test results are shown in Table 2:
[0093] Table 2
[0094]
[0095] From the data in Table 2, we can see that:
[0096] (1) The hardness of the coating formed by the self-repairing and easy-to-clean coating material provided in Examples 1 to 3 is 7H to 8H, the water contact angle is 120 to 123°, the coating adhesion can reach level 0, the water contact angle of the coating after wiping can still reach 82 to 85°, and the water contact angle of the coating after heat treatment can still reach 110 to 112°. The antibacterial rate against Escherichia coli can reach 99%, and it has high hardness, excellent anti-wiping properties, self-repairing properties and antibacterial properties.
[0097] (2) Compared with Example 1, the coating material provided in Comparative Example 1 does not contain polydopamine microcapsules, and the water contact angle of the formed coating after heat treatment is only 83°, which does not have self-healing properties.
[0098] (3) Compared with Example 1, the perfluoropolyether siloxane used in the coating material provided in Comparative Example 2 is not modified with catechins and does not have antibacterial properties, and the antibacterial rate against Escherichia coli is only 75%.
[0099] (4) Compared with Example 1, sodium dodecyl sulfate is directly added to the coating material provided in Comparative Example 3 without being made into microcapsules, resulting in the formed coating having a water contact angle of only 83° after heat treatment, and having no self-healing properties.
[0100] (5) Compared with Example 1, the amount of sodium dodecyl sulfate added to the polydopamine microcapsules used in the coating material provided in Example 4 is relatively too high, resulting in the hardness and water contact angle of the coating being too low, and the water contact angles after wiping and heat treatment are both low, and the self-healing property is poor; and the amount of sodium dodecyl sulfate added to the polydopamine microcapsules used in the coating material provided in Example 5 is relatively too low, which also results in the water contact angles of the coating after wiping and heat treatment are both low, and the self-healing property is poor.
[0101] (6) Compared with Example 1, the amount of polydopamine microcapsules added in the coating material provided in Example 6 is relatively too low, resulting in poor self-healing properties of the coating. The water contact angle of the coating decreases significantly after wiping and heat treatment. However, the amount of polydopamine microcapsules added in the coating material provided in Example 7 is relatively too high, resulting in the hardness and water contact angle of the coating being too low, the hydrophobicity being poor, and the self-healing properties being the same.
[0102] The applicant declares that the present invention illustrates a self-repairing and easy-to-clean coating material and its preparation method and application through the above embodiments, but the present invention is not limited to the above embodiments, that is, it does not mean that the present invention must rely on the above embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A self-repairing and easy-to-clean coating material, characterized in that: The self-repairing and easy-to-clean coating material comprises catechin-modified perfluoropolyether siloxane, polydopamine microcapsules and fluorine solvent A; The shell material of the polydopamine microcapsule comprises polydopamine, and the core material comprises polyalkyl organic metal salt.
2. The self-repairing and easy-to-clean coating material according to claim 1, characterized in that: The self-repairing easy-to-clean coating material comprises the following components in parts by weight: 5 to 10 parts by weight of catechin-modified perfluoropolyether siloxane; 10-20 parts by weight of polydopamine microcapsules; Fluorinated solvent A 60-70 parts by weight 3. The self-repairing and easy-to-clean coating material according to claim 1 or 2, characterized in that: The raw materials for preparing the catechin-modified perfluoropolyether siloxane include the following components in parts by weight: Preferably, the silane coupling agent includes any one of γ-aminopropyldiethoxysilane, γ-glycidyloxypropyltrimethoxysilane or γ-(methacryloyloxy)propyltrimethoxysilane or a combination of at least two thereof; Preferably, the catechin compound includes any one of catechin, epicatechin, gallocatechin or catechin gallate, or a combination of at least two thereof.
4. The self-repairing and easy-to-clean coating material according to claim 3, characterized in that: The catechin-modified perfluoropolyether siloxane is prepared by the following method, which comprises the following steps: (A1) reacting perfluoropolyether acyl fluoride and anhydrous ethanol in a fluorine solvent B, followed by cooling, washing, drying, filtering and distilling to obtain perfluoropolyether methyl ester; (A2) reacting perfluoropolyether methyl ester and a silane coupling agent, adding anhydrous ethanol and a fluorinated solvent C to mix, standing to separate the liquids, and removing the lower layer of liquid for vacuum distillation to obtain perfluoropolyether siloxane; (A3) mixing a perfluoropolyether siloxane and a catechin compound in a fluorinated solvent D to obtain the catechin-modified perfluoropolyether siloxane; Preferably, the reaction in step (A1) comprises two stages, stage 1 is a reaction at room temperature for 1 to 2 hours, and stage 2 is a reaction at a temperature of 50 to 70° C. for 1 to 2 hours; Preferably, the reaction temperature in step (A2) is 50-70°C and the reaction time is 2-4h; Preferably, the reaction in step (A2) is carried out under nitrogen protection; Preferably, the mixing temperature in step (A3) is 30-35° C. and the mixing time is 20-40 min.
5. The self-repairing and easy-to-clean coating material according to any one of claims 1 to 4, characterized in that: The raw materials for preparing the polydopamine microcapsules include the following components in parts by weight: 100 parts by weight of polyalkyl organic metal salt; 70-90 parts by weight of dopamine; Preferably, the polyalkyl organic metal salt includes any one of sodium octane sulfonate and sodium dodecyl sulfonate, sodium dodecyl sulfonate, sodium polystyrene sulfonate or polydiallyldimethylammonium chloride, or a combination of at least two thereof.
6. The self-repairing and easy-to-clean coating material according to claim 5, characterized in that: The preparation method of the polydopamine microcapsule comprises: dissolving a polyalkyl organic metal salt in a buffer solution, adding dopamine and mixing, thereby obtaining the polydopamine microcapsule; Preferably, the buffer comprises Tris hydrochloride buffer; Preferably, the pH value of the buffer is 8 to 9; Preferably, the mixing temperature is 40-60° C. and the mixing time is 20-30 hours.
7. The self-repairing and easy-to-clean coating material according to any one of claims 1 to 6, characterized in that: The fluorine solvent A, fluorine solvent B, fluorine solvent C and fluorine solvent D each independently include any one of perfluorohexane, perfluorocyclohexane, perfluoromethylcyclohexane, perfluorotoluene or perfluoroheptane, or a combination of at least two thereof.
8. A method for preparing the self-repairing and easy-to-clean coating material according to any one of claims 1 to 7, characterized in that: The preparation method comprises: uniformly mixing catechin-modified perfluoropolyether siloxane, polydopamine microcapsules and fluorine solvent A to obtain the self-repairing easy-to-clean coating material.
9. A method for using the self-repairing and easy-to-clean coating material according to any one of claims 1 to 7, characterized in that: The method of use comprises: coating the self-repairing easy-to-clean coating material on the surface of the stainless steel plate, and forming a self-repairing easy-to-clean coating on the stainless steel plate after drying and curing; Preferably, the drying temperature is 20-40°C and the drying time is 5-10 minutes; Preferably, the curing temperature is 120-140° C. and the curing time is 40-60 min.
10. Use of the self-repairing and easy-to-clean coating material according to any one of claims 1 to 7 in kitchen appliances.
Citation Information
Patent Citations
Self-clean material having self-repair function and preparation method thereof
CN105670565A
Self-cleaning coating material polymer and preparation method and application thereof
CN105778693A
Method for preparing high-hardness antifouling paint with excellent self-cleaning and insulating performances
CN109135566A
Perfluoropolyether siloxane compound and synthesis method and application thereof
CN109897176A
Surface treatment agent containing perfluoro(POLY)ether group-containing compound
CN110023450A
Cited By
Preparation process of automobile hub bearing blister tray
CN120792184A
Preparation process of automobile hub bearing blister tray
CN120792184B
Special easy-to-clean nano coating for photovoltaic glass
CN121406240A