Flexible polar region coating composition, coating material as well as preparation method and application of flexible polar region coating material

SER modified resin prepared by reacting bisphenol A type epoxy resin in the coating with 3-isocyanate propyltrimethoxysilane pre-addition and terminal hydroxyl polydimethylsilane addition, combined with polyamide resin, The formation of flexible polar coatings with excellent low temperature performance solves the problem that existing coatings lose toughness in extremely low temperature environments, achieves high adhesion and cold and heat resistance, and significantly improves the corrosion protection effect of the steel structure surface.

CN118879201AActive Publication Date: 2024-11-01XINHE NEW MATERIALS CO LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410958276.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-01
Estimated Expiration
2044-07-17

AI Technical Summary

Technical Problem

Existing paints lose toughness in extremely low temperature environments, causing the coating on the surface of steel substrate to crack or fall off, and cannot take into account both toughness and environmental resistance.

Method used

The Sil-EP modified resin was prepared by pre-addition reaction of bisphenol A type epoxy resin and 3-isocyanate propyltrimethoxysilane, and the SER modified resin was prepared by pre-addition reaction with terminal hydroxyl polydimethylsilane. , combined with a polyamide resin and a solvent, a flexible polar coating composition with excellent low temperature adhesion, impact resistance and cold and heat alternation resistance is formed.

Benefits of technology

Maintain 12MPa adhesion under -60℃, and passes the 10 Joule impact test, the flexibility reaches 1mm, and the adhesion of the paint film can reach more than 10MPa after 30 cycles after the cold and heat alternation between -60℃~80℃, and it is resistant to salt water There is no rust, cracking, or falling off for 2000 hours, which significantly improves the corrosion protection period of the steel structure surface coating in polar environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004949539140000101
    Figure BDA0004949539140000101
Patent Text Reader

Abstract

The invention discloses a flexible polar region coating composition, a coating material as well as a preparation method and application thereof. The flexible polar region coating composition comprises a first component and a second component, the first component comprises SER modified resin, pigment filler, an auxiliary agent and a solvent, the second component comprises polyamide resin and a solvent, the SER modified resin is Sil-EP modified resin prepared by performing a pre-addition reaction on bisphenol A type epoxy resin and 3-isocyanate propyl trimethoxy silane, and the Sil-EP modified resin is mixed with the polyamide resin to prepare the flexible polar region coating composition. And then carrying out addition reaction on the hydroxyl-terminated polydimethylsilane and the hydroxyl-terminated polydimethylsilane. The flexible polar region coating composition and the coating material provided by the invention have excellent adhesive force, flexibility and high and low temperature alternating resistance under the condition of polar region temperature (-60 DEG C), and can effectively prevent the phenomena of paint film damage and shedding caused by mechanical impact and cold and hot temperature change on the surface of a steel structure in a low-temperature environment; therefore, the anti-corrosion protection period of the steel structure surface coating material in the polar region environment is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a coating material, in particular to a flexible polar coating composition, a coating material and a preparation method and application thereof, belonging to the technical field of heavy-duty anti-corrosion coatings. Background Art

[0002] The Arctic region is extremely cold, especially in the polar regions within the Arctic Circle, where the lowest temperature in winter can reach minus 50 degrees Celsius or even lower. In this low-temperature natural environment, the coating on the surface of the steel substrate tends to lose its toughness. When the substrate is hit or deformed due to alternating hot and cold, the coating will crack or fall off due to loss of adhesion, thereby losing its anti-corrosion protection for the steel substrate. Therefore, the toughness of the coating in a low-temperature environment has always been an important research topic in the field of coatings. Usually when the temperature is below -20°C, conventional epoxy coatings will begin to have problems with poor adhesion and poor impact performance. On this issue, the industry usually adopts methods such as reducing the cross-linking density of the coating and adding toughening resins to improve the toughness of the coating, but this approach will also lead to a decrease in the environmental resistance of the paint film. In recent years, both domestic and foreign countries have increased their efforts to develop the Arctic region. For example, equipment has been developed for use in icebreaker hulls and high-cold areas, but they cannot achieve both toughness and environmental resistance, and the results are not ideal. Therefore, how to develop a flexible polar coating material with greater toughness and environmental resistance is of great significance for improving my country's infrastructure or development capabilities in the Arctic region. Summary of the invention

[0003] The main purpose of the present invention is to provide a flexible polar coating composition, a coating material and a preparation method thereof, so as to overcome the deficiencies in the prior art.

[0004] Another object of the present invention is to provide applications of the flexible polar coating composition and coating material.

[0005] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes:

[0006] The embodiment of the present invention provides a flexible polar coating composition, comprising: a first component and a second component, wherein the first component comprises a SER modified resin, a pigment, a filler, an additive and a solvent, and the second component comprises a polyamide resin and a solvent;

[0007] The SER modified resin is prepared by firstly subjecting bisphenol A epoxy resin to a pre-addition reaction with 3-isocyanate propyltrimethoxysilane to obtain Sil-EP modified resin, and then subjecting the Sil-EP modified resin to an addition reaction with terminal hydroxyl polydimethylsilane to obtain the SER modified resin.

[0008] In some embodiments, the first component includes the following components calculated in parts by weight: 45-55 parts of SER modified resin, 20-30 parts of pigments and fillers, 1-2 parts of additives, and 20-25 parts of solvents.

[0009] In some embodiments, the second component includes the following components calculated in parts by weight: 15 to 25 parts of a polyamide resin and 75 to 85 parts of a solvent.

[0010] The embodiment of the present invention also provides a method for preparing the aforementioned flexible polar coating composition, which comprises:

[0011] Firstly, bisphenol A epoxy resin and 3-isocyanate propyltrimethoxysilane are subjected to a pre-addition reaction to obtain Sil-EP modified resin, and then the Sil-EP modified resin is subjected to an addition reaction with terminal hydroxyl polydimethylsilane to obtain SER modified resin;

[0012] The SER modified resin, pigments, fillers, additives and solvent are mixed uniformly to obtain a first component;

[0013] The polyamide resin and the solvent are mixed uniformly to obtain a second component;

[0014] The first component and the second component are mixed evenly to prepare the flexible polar coating composition.

[0015] The embodiment of the present invention further provides a flexible polar coating material, which is formed from the aforementioned flexible polar coating composition.

[0016] The embodiments of the present invention also provide the use of the aforementioned flexible polar coating composition or flexible polar coating material in steel coating protection in polar environments.

[0017] Correspondingly, an embodiment of the present invention further provides a method for protecting the surface of a steel substrate in a polar environment, which comprises: coating the flexible polar coating composition on the surface of the steel substrate to form a protective coating.

[0018] Compared with the prior art, the beneficial effects of the present invention include:

[0019] The flexible polar coating composition and coating material provided by the present invention have excellent low-temperature adhesion, low-temperature impact resistance, low-temperature flexibility, resistance to hot and cold cycles, and resistance to salt water due to the aforementioned raw material component design. For example, the coating material is tested for adhesion, impact resistance, and flexibility at -60°C, and the adhesion can still reach 12MPa, and can pass the 10 Joule impact test, and the flexibility can reach 1mm; after 30 cycles under -60°C to 80°C hot and cold cycles, the paint film is good, the adhesion can reach more than 10MPa, and the salt water resistance is tested for 2000h after hot and cold cycles, and the paint film has no rust, cracking, or falling off. The coating material is applied to the surface of the steel structure, which can effectively prevent the paint film from being damaged and falling off due to mechanical impact and hot and cold temperature changes on the surface of the steel structure in a low-temperature environment, thereby increasing the anti-corrosion protection period of the coating material on the surface of the steel structure in the polar environment, and it is easy to prepare and suitable for large-scale production and application. DETAILED DESCRIPTION

[0020] In view of the above-mentioned problems existing in the prior art, the inventors of the present invention have conducted extensive and in-depth research and provided a flexible polar coating composition and coating material designed with specific raw material components, which have excellent low-temperature adhesion, low-temperature impact resistance, low-temperature flexibility, resistance to hot and cold cycles, and resistance to salt water.

[0021] The technical solution, its implementation process and principle will be further explained as follows.

[0022] As one aspect of the technical solution of the present invention, a flexible polar coating composition involves a first component and a second component, wherein the first component includes a Silane-Epoxy-Rubber modified resin (hereinafter referred to as SER modified resin), pigments, fillers, additives and solvents, and the second component includes a polyamide resin and a solvent.

[0023] In some embodiments, the SER modified resin is prepared by first subjecting bisphenol A epoxy resin to a pre-addition reaction with 3-isocyanate propyltrimethoxysilane to obtain Silane-Epoxy resin (abbreviated as Sil-EP modified resin), and then subjecting the Sil-EP modified resin to an addition reaction with terminal hydroxyl polydimethylsilane to obtain the obtained resin.

[0024] In some embodiments, the bisphenol A epoxy resin used in the preparation of the SER modified resin has a weight average molecular weight of 900-1120 and an epoxy equivalent of 450-560.

[0025] In some embodiments, the weight average molecular weight of 3-isocyanatepropyltrimethoxysilane used in the preparation of the SER modified resin is 200-230, and the NCO equivalent is 200-230.

[0026] In some embodiments, the mass ratio of the bisphenol A epoxy resin to 3-isocyanatepropyltrimethoxysilane is 3.0-3.3:1.

[0027] In some embodiments, the weight average molecular weight of the hydroxy-terminated polydimethylsilane is 41,000 to 52,000, and the viscosity is 3,500 to 4,500 CPS.

[0028] In some embodiments, the mass ratio of the Sil-EP modified resin to the hydroxy-terminated polydimethylsilane is 1:12.5-13.4.

[0029] In some preferred embodiments, the SER modified resin is prepared by pre-addition reaction of bisphenol A epoxy resin and 3-isocyanate propyltrimethoxysilane in a mass ratio of 3.0 to 3.3:1, and then reacting the product with terminal hydroxyl polydimethylsilane in a mass ratio of 1:12.5 to 13.4.

[0030] In some more preferred embodiments, the SER modified resin is prepared by pre-addition reaction of bisphenol A epoxy resin with a weight average molecular weight of 900-1120 and an epoxy equivalent of 450-560 with 3-isocyanate propyltrimethoxysilane with a weight average molecular weight of 200-230 and an NCO equivalent of 200-230 in a mass ratio of 3.0-3.3:1 to obtain Silane-Epoxy resin (Sil-EP modified resin), and then the Sil-EP modified resin is added with terminal hydroxyl polydimethylsilane with a weight average molecular weight of 41000-52000 and a viscosity of 3500-4500 CPS in a mass ratio of 1:12.5-13.4.

[0031] In some embodiments, the first component includes the following components calculated in parts by weight: 45-55 parts of SER modified resin, 20-30 parts of pigments and fillers, 1-2 parts of additives, and 20-25 parts of solvents.

[0032] In some embodiments, the second component includes the following components calculated in parts by weight: 15 to 25 parts of a polyamide resin and 75 to 85 parts of a solvent.

[0033] In some embodiments, the mass ratio of the first component to the second component is 10.2-12.8:1.

[0034] In some embodiments, the active hydrogen equivalent of the polyamide resin is 275-285.

[0035] Furthermore, the pigments and fillers include any one or more combinations of titanium dioxide, black iron oxide, red iron oxide, talcum powder and silica powder, but are not limited thereto.

[0036] Furthermore, the auxiliary agent includes any one or more combinations of defoaming agents, leveling agents, and rheological additives, but is not limited thereto.

[0037] Further, the solvent includes any one or more combinations of xylene, propylene glycol methyl ether (PM), methyl isobutyl ketone (MIBK), acetone, n-butanol and acetylacetone, etc., but is not limited thereto.

[0038] As another aspect of the technical solution of the present invention, a method for preparing a flexible polar coating composition involves:

[0039] Firstly, bisphenol A epoxy resin and 3-isocyanate propyltrimethoxysilane are subjected to a pre-addition reaction to obtain Sil-EP modified resin, and then the Sil-EP modified resin is subjected to an addition reaction with terminal hydroxyl polydimethylsilane to obtain SER modified resin;

[0040] The SER modified resin, pigments, fillers, additives and solvent are mixed uniformly to obtain a first component;

[0041] The polyamide resin and the solvent are mixed uniformly to obtain a second component;

[0042] The first component and the second component are mixed evenly to prepare the flexible polar coating composition.

[0043] In some embodiments, the preparation process of the SER modified resin includes:

[0044] Add bisphenol A epoxy resin to a mixed solvent containing xylene and butanol, and heat to 55-65° C. to fully dissolve, then add 3-isocyanate propyl trimethoxy silane in batches until the mass ratio of bisphenol A epoxy resin to 3-isocyanate propyl trimethoxy silane is 3.0-3.3:1, and then perform a pre-addition reaction at 55-65° C. for 2-2.5 hours under stirring conditions to obtain a Sil-EP modified resin;

[0045] The terminal hydroxyl polydimethylsilane is added in batches under stirring until the mass ratio of the Sil-EP modified resin to the terminal hydroxyl polydimethylsilane is 1:12.5-13.4, and then the addition reaction is carried out at 55-65° C. under stirring for 1-1.5 hours to obtain the SER modified resin.

[0046] The bisphenol A epoxy resin, 3-isocyanate propyltrimethoxysilane and hydroxy-terminated polydimethylsilane used in the process of preparing the SER modified resin are as defined above and will not be described in detail here.

[0047] In some more specific embodiments, during the preparation of the SER modified resin, epoxy is excessive, and in order to ensure the stable distribution of the coupling agent in the epoxy structure, the mass ratio of bisphenol A epoxy resin to 3-isocyanatepropyltrimethoxysilane is set to 3.0-3.3:1.

[0048] Furthermore, the present invention sets the mass ratio of Sil-EP modified resin to terminal hydroxyl polydimethylsilane to 1:12.5-13.4, which can prevent the terminal hydroxyl polydimethylsilane from self-polymerization, and uses the Sil-EP modified resin to sandwich the terminal hydroxyl polydimethylsilane in the middle to eliminate the silanol group on the terminal hydroxyl polydimethylsilane, thereby ensuring its stability.

[0049] The present invention introduces the silane structure into the epoxy structure by reacting the hydroxyl group in the epoxy structure with a silane coupling agent (3-isocyanate propyltrimethoxysilane) having an NCO group without destroying the epoxy group, and then connects the terminal hydroxyl polydimethylsilane having silanol groups at both ends into the structure by cross-linking with the silyl alkoxy group.

[0050] As one of the more specific embodiments, the method for preparing the flexible polar coating composition may include the following steps:

[0051] A mixed solvent of xylene and butanol is added to a reaction kettle, and bisphenol A epoxy resin is added under low-speed stirring, and the temperature is raised to 55-65° C., and the epoxy resin is stirred at a low speed until it is fully dissolved, and then 3-isocyanate propyl trimethoxy silane is added in batches until the mass ratio of bisphenol A epoxy resin to 3-isocyanate propyl trimethoxy silane is 3.0-3.3:1, and then a pre-addition reaction is carried out at 55-65° C. for 2-2.5 hours under stirring conditions to obtain a pre-addition resin, and then a stirring state is maintained, and terminal hydroxyl polydimethyl silane is added in batches until the mass ratio of the pre-addition resin to the terminal hydroxyl polydimethyl silane is 1:12.5-13.4, and then the reaction is carried out at 55-65° C. for 1-1.5 hours under stirring conditions, and the SER modified resin is obtained after cooling to room temperature;

[0052] The SER modified resin is mixed evenly with pigments, fillers, additives and solvents to obtain a first component;

[0053] The polyamide resin and the solvent are mixed uniformly to obtain a second component.

[0054] Exemplarily, a mixed solvent of xylene and butanol can be added to a reactor, and an agitator is turned on to stir at a speed of 300-500 r / min, followed by adding bisphenol A epoxy resin and heating to 55-65° C., and then slowly adding 3-isocyanate propyl trimethoxy silane dropwise to the bisphenol A epoxy resin solution at a mass ratio of 3.0-3.3:1 of bisphenol A epoxy resin and 3-isocyanate propyl trimethoxy silane under stirring conditions, and continuing to stir and control the temperature to 55-65° C. for a pre-addition reaction for 2-2.5 hours to obtain a pre-addition resin (Sil-EP modified resin), and then maintaining stirring, slowly adding terminal hydroxyl polydimethyl silane to the Sil-EP modified resin at a mass ratio of 1:12.5-13.4 of the pre-addition resin and terminal hydroxyl polydimethyl silane, and then reacting at 55-65° C. for 1-1.5 hours under stirring conditions to obtain a SER modified resin.

[0055] The mechanism of preparing the SER modified resin of the present invention is: using bisphenol A epoxy resin and 3-isocyanate propyl trimethoxy silane to react, the bisphenol A epoxy resin has an epoxy equivalent of 450-560, contains no less than 2 hydroxyl groups in the molecular structure, and can react with the NCO group in the 3-isocyanate propyl trimethoxy silane, thereby introducing the propyl trimethoxy silane into the epoxy resin structure without consuming the epoxy group to form the Sil-EP modified resin. Subsequently, through the condensation reaction between the silanol group and the silyl alkoxy group, the silanol groups at both ends of the terminal hydroxyl polydimethylsilane are reacted with the Sil-EP modified resin, so that it is connected to the Sil-EP modified resin structure to generate the SER modified resin.

[0056] The characteristics of this resin structure are: while retaining the toughness of terminal hydroxyl polydimethylsilane, by eliminating the silanol group, its storage stability is improved to prevent the adhesion of the coating from being affected by excessive polymerization. At the same time, the structure contains epoxy groups, which can further react with polyamide resin to form a three-dimensional network coating structure to ensure the environmental resistance of the coating. In addition, some silyl alkoxy groups are left in the structure. After the epoxy and active hydrogen are cross-linked to form a film, this part of the silyl alkoxy group will continue to slowly hydrolyze to produce silanol groups, and further cross-link with the hydroxyl groups on the metal substrate to improve the adhesion of the coating. The long-chain silane in the SER resin structure can give the coating film good elongation and tensile strength, and the structure is insensitive to temperature changes and will not cause the coating film to become more brittle with the rapid decrease in temperature. Therefore, it has excellent low-temperature toughness. The coating material formed by it can still ensure good flexibility in a low-temperature environment, so that the paint film will not crack or fall off due to brittleness.

[0057] In some embodiments, the preparation method specifically includes: mixing the SER modified resin with the pigment, filler, additive and a portion of the solvent in sequence, dispersing at a speed of 2000-3000 r / min for 25-30 minutes, and then adjusting the viscosity of the obtained mixture to 120-130 KU with another portion of the solvent to obtain the first component.

[0058] In some embodiments, the preparation method specifically comprises: uniformly mixing the polyamide resin and the solvent under a low-speed stirring condition of 300 to 500 r / min to obtain the second component. The second component of the present invention is an amine component, which is responsible for cross-linking with the epoxy in the first component.

[0059] In one embodiment, the preparation method further comprises: uniformly mixing the first component and the second component at a mass ratio of 10.2 to 12.8: 1. The SER modified resin structure prepared by the present invention can increase the elongation of the coating film, thereby improving the adaptability of the coating film under hot and cold alternating conditions; and the normal cross-linking of epoxy and amine can ensure the basic shielding performance and seawater resistance and chemical resistance of the coating film.

[0060] Another aspect of an embodiment of the present invention further provides a flexible polar coating material, which is formed by the aforementioned flexible polar coating composition (also referred to as a coating composition for forming a flexible polar coating material).

[0061] Furthermore, the dry film thickness of the flexible polar coating material is within 200 μm.

[0062] Another aspect of the embodiments of the present invention further provides the use of the aforementioned flexible polar coating composition or flexible polar coating material in the field of surface protection of steel substrates in polar environments.

[0063] For example, one embodiment of the present invention provides a method for protecting the surface of a steel substrate in a polar environment, which comprises: applying the composition for forming a flexible polar coating material to the surface of a steel substrate to form a protective coating.

[0064] Correspondingly, another aspect of an embodiment of the present invention further provides a method for protecting the surface of a steel substrate in a polar environment, which comprises: applying the flexible polar coating composition to the surface of the steel substrate to form a protective coating.

[0065] In summary, the flexible polar coating material provided by the present invention has excellent low-temperature adhesion, low-temperature impact resistance, low-temperature flexibility, resistance to hot and cold cycles, and resistance to salt water. For example, the coating material is tested for adhesion, impact resistance, and flexibility at -60°C, and the adhesion can still reach 12MPa, and can pass the 10 Joule impact test, and the flexibility can reach 1mm; after 30 cycles under -60°C to 80°C hot and cold cycles, the paint film is good, the adhesion can reach more than 10MPa, and the salt water resistance is tested for 2000h after hot and cold cycles, and the paint film has no rust, cracking, or falling off. Applying the coating composition to the surface of the steel structure can effectively prevent the paint film from being damaged or falling off due to mechanical impact and hot and cold temperature changes on the surface of the steel structure in a low-temperature environment, thereby increasing the anti-corrosion protection period of the coating material on the surface of the steel structure in the polar environment, and it is easy to prepare and suitable for large-scale production and application.

[0066] The technical scheme of the present invention is further described below in conjunction with several embodiments, but the present invention is not limited to the scope of the embodiments. The reagents and raw materials used in the following examples are all commercially available, and the test methods for which specific conditions are not specified are usually carried out under conventional conditions or under conditions recommended by the manufacturers. In addition, in the following examples, low-speed stirring refers to a rotation speed of 500 r / min or less, 500-2000 r / min is medium-speed stirring, and high-speed stirring refers to a rotation speed of 2000 r / min or more. High-speed dispersion refers to a rotation speed of 2000-3000 r / min.

[0067] Example 1

[0068] A method for preparing a coating composition for forming a flexible polar coating material comprises the following steps:

[0069] (1) Add 1000 g of a mixed solvent of xylene and butanol into a reactor, add 300 g of bisphenol A epoxy resin under low-speed stirring, and heat to 55°C. Stir at a low speed until the epoxy resin is fully dissolved, then add 100 g of 3-isocyanatepropyltrimethoxysilane in batches, and carry out addition reaction at 55°C under low-speed stirring for 2.5 h to obtain Sil-EP modified resin. Then, keep stirring, add 5000 g of terminal hydroxyl polydimethylsilane in batches, and then react at 55°C under stirring for 1.5 h, and then cool to room temperature to obtain a SER modified resin solution.

[0070] (2) 4500 g of SER modified resin solution was mixed with 2300 g of titanium dioxide, 100 g of defoamer, 100 g of rheological additive, and 2700 g of a mixed solvent of xylene and n-butanol in sequence, and dispersed at high speed for about 30 min. Thereafter, the viscosity of the mixture was adjusted to about 120 KU with 300 g of a mixed solvent of xylene and butanol to obtain a first component.

[0071] (3) Add 1500 g of polyamide resin and 8500 g of xylene into a reaction kettle, stir and disperse at medium speed for 10 minutes to obtain a second component.

[0072] (4) The first component and the second component are uniformly mixed at a mass ratio of about 10.2:1 to obtain a coating composition for forming a flexible polar coating material.

[0073] Example 2

[0074] A method for preparing a coating composition for forming a flexible polar coating material comprises the following steps:

[0075] (1) Add 1000 g of a mixed solvent of xylene and butanol into a reaction kettle, add 330 g of bisphenol A epoxy resin under low-speed stirring, and heat to 65°C. Stir at a low speed until the epoxy resin is fully dissolved, then add 100 g of 3-isocyanatepropyltrimethoxysilane in batches, and carry out addition reaction at 65°C under low-speed stirring for 2 h to obtain Sil-EP modified resin. Then, keep stirring, add 5762 g of terminal hydroxyl polydimethylsilane in batches, and then react at 65°C for 1 h under stirring, and then cool to room temperature to obtain a SER modified resin solution.

[0076] (2) 5500 g of SER modified resin solution was mixed with 2500 g of titanium dioxide, 100 g of defoamer, 100 g of rheological additive, and 1500 g of a mixed solvent of xylene and n-butanol in sequence, and dispersed at high speed for about 30 min. Thereafter, the viscosity of the mixture was adjusted to about 120 KU with 300 g of a mixed solvent of xylene and butanol to obtain a first component.

[0077] (3) Add 2500 g of polyamide resin and 7500 g of xylene into a reaction kettle, stir and disperse at medium speed for 10 minutes to obtain a second component.

[0078] (4) The first component and the second component are uniformly mixed at a mass ratio of about 12.8:1 to obtain a coating composition for forming a flexible polar coating material.

[0079] Example 3

[0080] A method for preparing a coating composition for forming a flexible polar coating material comprises the following steps:

[0081] (1) Add 1000 g of a mixed solvent of xylene and butanol into a reactor, add 320 g of bisphenol A epoxy resin under low-speed stirring, and heat to 55° C., stir at low speed until the epoxy resin is fully dissolved, then add 100 g of 3-isocyanatepropyltrimethoxysilane in batches, and carry out addition reaction at 55° C. under low-speed stirring for 2.5 h to obtain Sil-EP modified resin, then keep stirring, add 4290 g of terminal hydroxyl polydimethylsilane in batches, and then react at 55° C. under stirring for 1.5 h, and then cool to room temperature to obtain a SER modified resin solution.

[0082] (2) 5000 g of SER modified resin solution was mixed with 2300 g of titanium dioxide, 100 g of defoamer, 100 g of rheological additive, and 2200 g of a mixed solvent of xylene and n-butanol in sequence, and dispersed at high speed for about 30 min. Thereafter, the viscosity of the mixture was adjusted to about 120 KU with 300 g of a mixed solvent of xylene and butanol to obtain a first component.

[0083] (3) Add 2000 g of polyamide resin and 8000 g of xylene into a reaction kettle, stir and disperse at medium speed for 10 minutes to obtain a second component.

[0084] (4) The first component and the second component are uniformly mixed at a mass ratio of about 11.5:1 to obtain a coating composition for forming a flexible polar coating material.

[0085] Example 4

[0086] The present embodiment is different from the embodiment 1 in that 2300 g of titanium dioxide in the embodiment 1 is replaced by 300 g of red iron oxide, 500 g of talc and 1500 g of silica powder.

[0087] Example 5

[0088] The present embodiment differs from the embodiment 2 in that 2500 g of titanium dioxide in the embodiment 2 is replaced by 500 g of black iron oxide, 500 g of talc and 1500 g of silica powder.

[0089] Comparative Example 1

[0090] The preparation method of a coating composition provided in this comparative example is basically the same as that of Example 1, except that the terminal hydroxyl polydimethylsilane in Example 1 is removed and the Sil-EP modified resin is used instead of the SER modified resin.

[0091] Comparative Example 2

[0092] The preparation method of a coating composition provided in this comparative example is basically the same as that of Example 1, except that the SER modified resin in Example 1 is replaced with conventional bisphenol A epoxy resin E-20.

[0093] Comparative Example 3

[0094] The preparation method of a coating composition provided in this comparative example is basically the same as that of Example 1, except that the mass ratio of the first component to the second component in Example 1 is replaced with 7:1.

[0095] Comparative Example 4

[0096] The preparation method of a coating composition provided in this control example is basically the same as that in Example 1, the only difference is that in the preparation process of the Sil-EP resin in Example 1, the mass ratio of bisphenol A epoxy resin to 3-isocyanatepropyltrimethoxysilane is replaced with 10:1.

[0097] Comparative Example 5

[0098] The preparation method of a coating composition provided in this comparative example is basically the same as that in Example 1, except that the amount of SER modified resin added in Example 1 is changed to 4000 g. If the PVC content is too low, dark bubbles are easily formed in the paint film during the construction process, which also affects the durability of the coating film.

[0099] Comparative Example 6

[0100] The preparation method of a coating composition provided in this comparative example is basically the same as that in Example 1, except that the amount of SER modified resin added in Example 1 is changed to 6000 g. The PVC content is too high, the anti-penetration ability / salt water resistance of the coating film is low, and the low-temperature toughness is low.

[0101] Comparative Example 7

[0102] The preparation method of a coating composition provided in this comparative example is basically the same as that in Example 1, the only difference is that in the preparation process of the Sil-EP resin in Example 1, the mass ratio of the Sil-EP modified resin to the terminal hydroxyl polydimethylsilane is 1:15. When the ratio is too large, the viscosity of the product is high, part of the silicone rubber self-polymerizes, affecting the final crosslinking density, and reducing the salt water resistance.

[0103] The coating compositions of Examples 1-5 and Comparative Examples 1-7 and commercially available conventional low-temperature resistant coatings were coated on the surface of sandblasted steel plates to form coatings of the same thickness, and the properties of these coatings were tested respectively, and the corresponding test results are shown in Table 1. The test results in Table 1 are the average values ​​of the test results of multiple batches of products.

[0104] Table 1 Performance test results of coating compositions of Examples 1-5 and Comparative Examples 1-7 and conventional low-temperature resistant coatings available on the market after forming coatings

[0105]

[0106] Referring to Table 1, it can be seen that the coating composition of Examples 1-5 can form a flexible polar coating material. The coating material is tested for adhesion, impact resistance, and flexibility at -60°C. The adhesion can still reach more than 11MPa, and can pass the 10 Joule impact test. The flexibility can reach 1mm. After 30 cycles under -60°C to 80°C hot and cold alternating conditions, the paint film is good, the adhesion can reach more than 10MPa, and after hot and cold alternating conditions, the paint film is tested for salt water resistance for 2000h, and there is no rust, cracking, or shedding. The comprehensive performance is far superior to conventional commercially available low-temperature resistant coatings.

[0107] In addition, the inventors of this case also conducted experiments with other raw materials and conditions listed in this specification with reference to the methods of Examples 1 to 5, and obtained similar results.

[0108] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A flexible polar coating composition, It is characterized in that include: A first component and a second component, wherein the first component comprises a SER modified resin, a pigment, a filler, an additive and a solvent, and the second component comprises a polyamide resin and a solvent; The SER modified resin is prepared by firstly subjecting bisphenol A epoxy resin to a pre-addition reaction with 3-isocyanate propyltrimethoxysilane to obtain Sil-EP modified resin, and then subjecting the Sil-EP modified resin to an addition reaction with terminal hydroxyl polydimethylsilane to obtain the SER modified resin.

2. The flexible polar coating composition according to claim 1, Features: The bisphenol A epoxy resin has a weight average molecular weight of 900 to 1120 and an epoxy equivalent of 450 to 560; and / or the 3-isocyanate propyltrimethoxysilane has a weight average molecular weight of 200 to 230 and an NCO equivalent of 200 to 230; And / or, the mass ratio of the bisphenol A epoxy resin to 3-isocyanate propyltrimethoxysilane is 3.0-3.3:1; And / or, the weight average molecular weight of the hydroxy-terminated polydimethylsilane is 41000-52000, and the viscosity is 3500-4500 CPS; And / or, the mass ratio of the Sil-EP modified resin to the hydroxy-terminated polydimethylsilane is 1:12.5-13.

4.

3. The flexible polar coating composition according to claim 1, It is characterized in that The first component includes the following components calculated in parts by weight: 45-55 parts of SER modified resin, 20-30 parts of pigments and fillers, 1-2 parts of additives and 20-25 parts of solvents.

4. The flexible polar coating composition according to claim 1, It is characterized in that The second component includes the following components calculated by weight: 15-25 parts of polyamide resin and 75-85 parts of solvent; And / or, the mass ratio of the first component to the second component is 10.2-12.8:

1.

5. The flexible polar coating composition according to claim 1, Features: The active hydrogen equivalent of the polyamide resin is 275-285; and / or, the pigment and filler include any one or more combinations of titanium dioxide, black iron oxide, red iron oxide, talcum powder and silica powder; and / or, the additive includes any one or more combinations of defoaming agent, leveling agent and rheological additive; and / or, the solvent includes any one or more combinations of xylene, propylene glycol methyl ether, methyl isobutyl ketone, acetone, n-butanol and acetylacetone.

6. A method for preparing the flexible polar coating composition according to any one of claims 1 to 5, It is characterized in that include: Firstly, bisphenol A epoxy resin and 3-isocyanate propyltrimethoxysilane are subjected to a pre-addition reaction to obtain Sil-EP modified resin, and then the Sil-EP modified resin is subjected to an addition reaction with terminal hydroxyl polydimethylsilane to obtain SER modified resin; The SER modified resin, pigments, fillers, additives and solvent are mixed uniformly to obtain a first component; The polyamide resin and the solvent are mixed uniformly to obtain a second component; The first component and the second component are mixed evenly to prepare the flexible polar coating composition.

7. The preparation method according to claim 6, It is characterized in that include: Add bisphenol A epoxy resin to a mixed solvent containing xylene and butanol, and heat to 55-65° C. to fully dissolve, then add 3-isocyanate propyl trimethoxy silane in batches until the mass ratio of bisphenol A epoxy resin to 3-isocyanate propyl trimethoxy silane is 3.0-3.3:1, and then perform a pre-addition reaction at 55-65° C. for 2-2.5 hours under stirring conditions to obtain a Sil-EP modified resin; Adding terminal hydroxyl polydimethylsilane in batches under stirring until the mass ratio of Sil-EP modified resin to terminal hydroxyl polydimethylsilane is 1:12.5-13.4, and then performing addition reaction at 55-65° C. under stirring for 1-1.5 hours to obtain the SER modified resin; And / or, the weight average molecular weight of the bisphenol A epoxy resin is 900-1120, and the epoxy equivalent is 450-560; And / or, the weight average molecular weight of the 3-isocyanate propyltrimethoxysilane is 200 to 230, and the NCO equivalent is 200 to 230; And / or, the weight average molecular weight of the hydroxy-terminated polydimethylsilane is 41000-52000, and the viscosity is 3500-500 CPS; And / or, the mass ratio of the first component to the second component is 10.2-12.8:

1.

8. A flexible polar coating material, It is characterized in that The flexible polar coating material is formed from the flexible polar coating composition according to any one of claims 1 to 5; Preferably, the dry film thickness of the flexible polar coating material is less than 200 μm.

9. Use of the flexible polar coating composition according to any one of claims 1 to 5 or the flexible polar coating material according to claim 8 in steel coating protection in polar environments.

10. A method for protecting the surface of a steel substrate in an arctic environment. It is characterized in that include: The flexible polar coating composition according to any one of claims 1 to 5 is applied to the surface of a steel substrate to form a protective coating.

Citation Information

Patent Citations

  • Epoxy-polysiloxane resin for paint and preparation method thereof

    CN102352043A

  • Silicon-modified waterborne epoxy resin emulsion and preparation method thereof

    CN112521830A

  • Epoxy resin composition and transparent composite material containing same and laminated board

    CN112759891A

  • Low-temperature-curing high-solid epoxy coating and preparation method thereof

    CN113045919A

  • A manufacturing method of a fatty acid and a silane coupling agent modified epoxy resin, and coating composition for ship containing the modified epoxy resin

    KR1020150070600A