Conductive adhesive with high interface bonding force and high modulus for ACF (anisotropic conductive film) and preparation method of conductive adhesive

By using butyl rubber and epoxy resin graphene to modify raw materials such as 2-hydroxyethyl methacrylate phosphate, combined with silica and graphene oxide, the lack of interface connection force and modulus in the prior art was solved. The problem has improved the overall performance and stability of ACF and is suitable for high-performance connections of modern electronic products.

CN118879209APending Publication Date: 2024-11-01NINGBO LIANSEN ELECTRONIC MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410977695.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

When the existing heterosqualitative conductive adhesives increase the interface connection force and modulus, they often sacrifice the crosslink density and resistance of the adhesive film, resulting in weakening of the interface binding force and reducing the resistance of the cured adhesive film, and in some applications, the interface is shown. Problems of insufficient binding force, insufficient modulus and poor tolerance testing.

Method used

The modified 2-hydroxyethyl methacrylate phosphate of butyl rubber and epoxy resin graphene are used as the main raw materials. Through the synergistic effect between various raw materials, the mechanical strength, interface connection force and comprehensive performance of ACF are improved. Silica and graphene oxide are introduced as fillers and conductive particles to improve the modulus and optical properties of the adhesive film.

Benefits of technology

It significantly improves the interface connection force and modulus of ACF, enhances the adhesion and stability of conductive adhesives, ensures structural integrity and electrical performance stability in harsh environments, and miniaturizes and lightens the electronic products and High performance is supported.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention belongs to the technical field of anisotropic conductive adhesives, and relates to a conductive adhesive with high interface bonding force and high modulus for ACF and a preparation method of the conductive adhesive. The conductive adhesive is processed from the following raw materials in parts by weight: 10-20 parts of butyl rubber, 20-30 parts of epoxy resin graphene modified 2-hydroxyethyl methacrylate phosphate, 1-10 parts of conductive particles, 30-70 parts of filler, 20-40 parts of a solvent and 1-10 parts of an initiator. The epoxy resin graphene modified 2-hydroxyethyl methacrylate phosphate is added into the raw materials of the conductive adhesive, so that the key performance of an ACF product is improved, and the mechanical strength and modulus of an adhesive film are increased due to introduction of epoxy resin; due to the introduction of the graphene oxide, the interface connection force is obviously improved; 2-hydroxyethyl methacrylate phosphate is used as a functional monomer and assists in enhancing the comprehensive performance of the ACF product through the combined action of the 2-hydroxyethyl methacrylate phosphate, the graphene oxide and the epoxy resin.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of anisotropic conductive adhesives, and relates to a conductive adhesive for ACF with high interface connection force and high modulus, and a preparation method thereof. Background Art

[0002] ACF (Anisotropic Conductive Film) is a special material used for precision electronic component connection. It is characterized by being conductive in a specific direction (usually the Z axis, which is perpendicular to the film surface), while being insulated in the lateral direction (XY axis). This film is composed of metal particles (commonly gold, nickel, copper, etc.) evenly dispersed in a resin or polymer matrix. When subjected to appropriate external force and temperature, the metal particles can form a conductive channel to ensure the smooth transmission of electronic signals and current.

[0003] In the electronics industry, ACF is widely used in LCD, OLED display screens and flat panel displays, touch screens, and semiconductor packaging technologies, especially at the connection between the liquid crystal panel and the driver IC or flexible printed circuit board (FPC), providing reliable and stable electrical connection to meet the requirements of electronic products for miniaturization and thinness.

[0004] In order to improve the performance of ACF, anisotropic conductive adhesives on the market usually add polyurethane-acrylate to enhance the interface bonding strength, and silicon dioxide to increase the modulus of the material, but this process may sacrifice the cross-linking density of the adhesive film, resulting in weakened interface bonding and reduced resistance of the cured adhesive film. Another common improvement method is to enhance the bonding strength and resin skeleton strength of ACF by adding acrylate resin. However, the adhesive film prepared by this method may show problems such as insufficient interface bonding strength, insufficient modulus and poor resistance test in some applications. Summary of the invention

[0005] The present invention aims at the problems existing in the ACF in the prior art and provides a conductive adhesive for ACF with high interface connection force and high modulus and a preparation method thereof.

[0006] One object of the present invention is achieved by the following technical solutions:

[0007] A conductive adhesive for ACF with high interface connection force and high modulus is processed from the following raw materials in parts by weight: 10 to 20 parts of butyl rubber, 20 to 30 parts of epoxy resin graphene modified 2-hydroxyethyl methacrylate phosphate, 1 to 10 parts of conductive particles, 30 to 70 parts of fillers, 20 to 40 parts of solvents, and 1 to 10 parts of initiators.

[0008] The present invention adopts butyl rubber as a partial skeleton, which has excellent air tightness, chemical stability and good electrical insulation, helps to form the basic structure of ACF, and provides necessary flexibility and elasticity, while ensuring that ACF has sufficient insulation in the non-conductive direction; the use of epoxy resin graphene modified 2-hydroxyethyl methacrylate phosphate can improve the comprehensive performance of ACF.

[0009] Preferably, the epoxy resin graphene modified 2-hydroxyethyl methacrylate phosphate is processed from the following raw materials in parts by weight: 20 to 30 parts of epoxy resin graphene intermediate, 10 to 30 parts of 2-hydroxyethyl methacrylate phosphate, and 0.1 to 1 part of initiator.

[0010] Preferably, the epoxy resin graphene intermediate is processed from the following raw materials in parts by weight: 60-75 parts of epoxy resin, 2-10 parts of graphene oxide, 0.1-1 part of triethylamine, and 20-60 parts of ethyl acetate.

[0011] The present invention introduces epoxy resin graphene modified 2-hydroxyethyl methacrylate phosphate into the raw materials of anisotropic conductive adhesive, and aims to improve the key performance of ACF through the synergistic effect of multiple raw materials, wherein the introduction of epoxy resin increases the mechanical strength and modulus of the adhesive film; the introduction of graphene oxide significantly improves the interface connection force; 2-hydroxyethyl methacrylate phosphate is used as a functional monomer.

[0012] Preferably, the epoxy resin is bisphenol A epoxy resin.

[0013] Preferably, the graphene oxide is carboxylated graphene oxide.

[0014] Preferably, the preparation method of the epoxy resin graphene intermediate comprises the following steps: adding epoxy resin, graphene oxide, triethylamine and ethyl acetate into a reaction kettle, heating the reaction kettle to react, and cooling the reaction kettle to obtain the epoxy graphene intermediate.

[0015] In the preparation method of the epoxy resin graphene intermediate, preferably, the reaction temperature is 60 to 90° C. and the reaction time is 1 to 5 hours.

[0016] Preferably, the preparation method of the epoxy resin graphene modified 2-hydroxyethyl methacrylate phosphate comprises the following steps: adding an epoxy resin graphene intermediate, 2-hydroxyethyl methacrylate phosphate, and an initiator into a reaction kettle, heating the reaction kettle, and cooling the reaction kettle to obtain epoxy resin graphene modified 2-hydroxyethyl methacrylate phosphate.

[0017] In the preparation method of the epoxy resin graphene modified 2-hydroxyethyl methacrylate phosphate, preferably, the reaction temperature is 95 to 120° C. and the reaction time is 6 to 10 hours.

[0018] Preferably, the conductive particles are one or more of metal nickel balls, gold balls, nickel / gold balls, and resin microspheres with nickel and / or gold layers on their surfaces.

[0019] Preferably, the resin microspheres are one or more of polystyrene (PS) microspheres, polyaniline (PANI) microspheres, polymethyl methacrylate (PMMA) microspheres, polyacrylamide (PMA) microspheres, polyvinyl alcohol (PVA) microspheres, and polycaprolactone (PCL) microspheres.

[0020] Preferably, the filler includes one or more of silicon dioxide, titanium dioxide, aluminum oxide, iron oxide, silicate, and carbon black, and more preferably silicon dioxide and / or titanium dioxide.

[0021] Silica and / or titanium dioxide are used as fillers in anisotropic conductive adhesives. Silica can effectively increase the modulus of ACF, that is, the ability of the material to resist deformation, which helps to enhance the stability and structural integrity of ACF when subjected to external forces, especially in application scenarios that require high mechanical strength. Titanium dioxide has a high refractive index and white color. Adding it in an appropriate amount can improve the optical properties of the film, especially whiteness and opacity, which is very important for certain applications that require high visual effects.

[0022] Preferably, the solvent includes one or more of toluene, methanol, ethanol, tetrahydrofuran, acetonitrile, N,N-dimethylformamide, and dimethyl sulfoxide, and more preferably toluene.

[0023] Preferably, the initiator is an organic peroxidation initiator.

[0024] More preferably, the organic peroxidation initiator comprises one or more of dibenzoyl peroxide, benzoyl peroxide, tert-butyl benzoyl peroxide, and methyl ethyl ketone peroxide, preferably dibenzoyl peroxide (BPO).

[0025] Preferably, the solid content of the conductive adhesive for ACF with high interface connection strength and high modulus is 30-60wt%.

[0026] The second object of the present invention is achieved by the following technical solutions:

[0027] A method for preparing a conductive adhesive for ACF with high interface connection force and high modulus comprises the following steps: weighing a solvent into a container, adding butyl rubber and epoxy resin graphene-modified 2-hydroxyethyl methacrylate phosphate, heating to 30-60°C to dissolve the adhesive in the solvent, adding a filler and stirring evenly, then adding conductive particles, and finally adding an initiator, placing the mixture in a defoaming mixer and dispersing the mixture evenly, thereby obtaining a conductive adhesive for ACF with high interface connection force and high modulus.

[0028] The third object of the present invention is achieved by the following technical solutions:

[0029] A high-interface connection force and high-modulus ACF is obtained by coating and drying the above-mentioned conductive adhesive for high-interface connection force and high-modulus ACF.

[0030] Compared with the prior art, the present invention has the following beneficial effects:

[0031] 1. The present invention provides a conductive adhesive for ACF with high interface connection strength and high modulus, which aims to improve the key performance of ACF products by adding epoxy resin graphene modified 2-hydroxyethyl methacrylate phosphate, wherein the introduction of epoxy resin increases the mechanical strength and modulus of the adhesive film; the introduction of graphene oxide significantly improves the interface connection strength; 2-hydroxyethyl methacrylate phosphate, as a functional monomer, helps to enhance the comprehensive performance of ACF products through the combined action of graphene oxide and epoxy resin.

[0032] 2. The present invention first synthesizes the epoxy resin graphene intermediate, and then further modifies the 2-hydroxyethyl methacrylate phosphate, so that it can be evenly distributed in the conductive adhesive, thereby enhancing the adhesion between the conductive adhesive and different substrates, especially in the connection of electronic components, and can provide more reliable electrical and mechanical connections; and the ACF exhibits stronger strength and stability after curing, which means that even in harsh environments, the ACF can maintain its structural integrity and the stability of its electrical properties, providing strong support for the miniaturization, lightweight and high performance of modern electronic products.

[0033] 3. In the epoxy resin graphene intermediate provided by the present invention, carboxylated graphene oxide is used as the graphene source in order to enhance the compatibility and reactivity with the epoxy resin. The carboxyl functional group of the carboxylated graphene oxide can undergo a ring-opening cross-linking reaction with the epoxy group of the epoxy resin to generate a stable epoxy graphene intermediate, which not only retains the excellent physical properties of graphene oxide, but also gives the conductive adhesive unique chemical properties. DETAILED DESCRIPTION

[0034] The technical solution of the present invention is further described below in conjunction with specific embodiments. It should be understood that the specific embodiments described herein are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined by the claims attached to this application.

[0035] The sources of raw materials in the following examples and comparative examples are as follows:

[0036] Conductive particles: Sekisui Chemical NIEYB4B-00475-S;

[0037] 2-Hydroxyethyl Methacrylate Phosphate: MERCK, 695890

[0038] Bisphenol A epoxy resin: Dow Chemical DER331;

[0039] Carboxylated graphene oxide: Xianfeng Nanotechnology Co., Ltd., carboxylated graphene oxide powder.

[0040] Example 1

[0041] The conductive adhesive for ACF with high interface connection strength and high modulus in this embodiment is made from the following raw materials in parts by weight: 15 parts of butyl rubber, 25 parts of epoxy resin graphene modified 2-hydroxyethyl methacrylate phosphate, 5 parts of conductive particles, 10 parts of silicon dioxide, 20 parts of titanium dioxide, 20 parts of toluene, and 3 parts of BPO.

[0042] The preparation method of the above-mentioned conductive adhesive with high interface connection force and high modulus for ACF comprises the following steps: weighing a solvent into a container, adding butyl rubber and epoxy resin graphene-modified 2-hydroxyethyl methacrylate phosphate, heating to 50°C to dissolve it in the solvent, adding filler and stirring evenly, then adding conductive particles, and finally adding an initiator, putting it into a defoaming mixer and dispersing it evenly to obtain a conductive adhesive with high interface connection force and high modulus for ACF.

[0043] The epoxy resin graphene modified 2-hydroxyethyl methacrylate phosphate of this embodiment is processed from the following raw materials in parts by weight: 20 parts of epoxy resin graphene intermediate, 30 parts of 2-hydroxyethyl methacrylate phosphate, and 0.5 parts of BPO.

[0044] The preparation method of the above-mentioned epoxy resin graphene modified 2-hydroxyethyl methacrylate phosphate comprises the following steps: adding an epoxy resin graphene intermediate, 2-hydroxyethyl methacrylate phosphate, and an initiator into a reaction kettle, heating to 100° C. to react for 6 hours, and cooling and discharging to obtain epoxy resin graphene modified 2-hydroxyethyl methacrylate phosphate.

[0045] The epoxy resin graphene intermediate of this embodiment is processed from the following raw materials in parts by weight: 65 parts of bisphenol A epoxy resin, 5 parts of carboxylated graphene oxide, 0.2 parts of triethylamine, and 40 parts of ethyl acetate.

[0046] The preparation method of the epoxy resin graphene intermediate comprises the following steps: adding bisphenol A epoxy resin, carboxylated graphene oxide, triethylamine and ethyl acetate into a reaction kettle, heating to 80° C. for reaction for 3 hours, and cooling and discharging to obtain the epoxy graphene intermediate.

[0047] Example 2

[0048] The only difference between this embodiment and embodiment 1 is that the conductive adhesive for ACF with high interface connection force and high modulus in this embodiment is processed from the following raw materials in parts by weight: 10 parts of butyl rubber, 45 parts of epoxy resin graphene modified 2-hydroxyethyl methacrylate phosphate, 7 parts of conductive particles, 30 parts of silicon dioxide, 40 parts of titanium dioxide, 30 parts of toluene, and 5 parts of BPO.

[0049] The epoxy resin graphene modified 2-hydroxyethyl methacrylate phosphate of this embodiment is processed from the following raw materials in parts by weight: 30 parts of epoxy resin graphene intermediate, 20 parts of 2-hydroxyethyl methacrylate phosphate, and 0.7 parts of BPO.

[0050] The rest is the same as in Example 1.

[0051] Example 3

[0052] The only difference between this embodiment and embodiment 1 is that the conductive adhesive for ACF with high interface connection force and high modulus in this embodiment is processed from the following raw materials in parts by weight: 13 parts of butyl rubber, 35 parts of epoxy resin graphene modified 2-hydroxyethyl methacrylate phosphate, 6 parts of conductive particles, 20 parts of silicon dioxide, 30 parts of titanium dioxide, 25 parts of toluene, and 4 parts of BPO.

[0053] The epoxy resin graphene modified 2-hydroxyethyl methacrylate phosphate of this embodiment is processed from the following raw materials in parts by weight: 25 parts of epoxy resin graphene intermediate, 25 parts of 2-hydroxyethyl methacrylate phosphate, and 0.6 parts of BPO.

[0054] The rest is the same as in Example 1.

[0055] Comparative Example 1

[0056] The difference between this comparative example and Example 1 is that the epoxy resin graphene modified 2-hydroxyethyl methacrylate phosphate in the conductive adhesive raw material of this comparative example is 10 parts, and the rest is the same as Example 1.

[0057] Comparative Example 2

[0058] The difference between this comparative example and Example 1 is that the epoxy resin graphene modified 2-hydroxyethyl methacrylate phosphate in the conductive adhesive raw material of this comparative example is 5 parts, and the rest is the same as Example 1.

[0059] Comparative Example 3

[0060] The difference between this comparative example and Example 1 is that epoxy resin graphene-modified 2-hydroxyethyl methacrylate phosphate is not added to the conductive adhesive raw material of this comparative example, and the rest is the same as Example 1.

[0061] Comparative Example 4

[0062] The difference between this comparative example and Example 1 is that the epoxy resin graphene modified 2-hydroxyethyl methacrylate phosphate in this comparative example is processed from the following raw materials in parts by weight: 5 parts of epoxy resin graphene intermediate, 40 parts of 2-hydroxyethyl methacrylate phosphate, and 0.5 parts of BPO. The rest is the same as Example 1.

[0063] Comparative Example 5

[0064] The difference between this comparative example and Example 1 is that this comparative example does not use epoxy resin graphene intermediate to modify 2-hydroxyethyl methacrylate phosphate, and the rest is the same as Example 1.

[0065] The conductive adhesive of this comparative example is processed from the following raw materials in parts by weight: 15 parts of butyl rubber, 20 parts of 2-hydroxyethyl methacrylate phosphate, 5 parts of conductive particles, 10 parts of silicon dioxide, 20 parts of titanium dioxide, 20 parts of toluene, and 3 parts of BPO.

[0066] Comparative Example 6

[0067] The difference between this comparative example and Example 1 is that epoxy resin modified 2-hydroxyethyl methacrylate phosphate is used in the conductive adhesive raw material of this comparative example instead of epoxy resin graphene intermediate modified 2-hydroxyethyl methacrylate phosphate, and the rest is the same as Example 1.

[0068] The epoxy resin modified 2-hydroxyethyl methacrylate phosphate of this comparative example is processed from the following raw materials in parts by weight: 20 parts of bisphenol A epoxy resin, 30 parts of 2-hydroxyethyl methacrylate phosphate, and 0.5 parts of BPO.

[0069] Comparative Example 7

[0070] The difference between this comparative example and Example 1 is that graphene oxide modified 2-hydroxyethyl methacrylate phosphate is used in the conductive adhesive raw material of this comparative example instead of epoxy resin graphene intermediate modified 2-hydroxyethyl methacrylate phosphate, and the rest is the same as Example 1.

[0071] The graphene oxide modified 2-hydroxyethyl methacrylate phosphate in this comparative example is processed from the following raw materials in parts by weight: 20 parts of carboxylated graphene oxide, 30 parts of 2-hydroxyethyl methacrylate phosphate, and 0.5 parts of BPO.

[0072] The conductive adhesives prepared in Examples 1 to 3 and Comparative Examples 1 to 4 were coated on a coating machine and dried in an oven at 70° C. to obtain ACF, which was placed between two electronic components and cured using a Bonder device under the conditions of 3 MPa, 4 s, and 150° C. Then, initial modulus, interface adhesion, and on-resistance tests were performed, and the test methods were as follows.

[0073] Initial modulus determination method: Use a rheometer to test and use the equipment to analyze the modulus data at 30°C; use a peel strength tester to measure the adhesion at a peel angle of 90° and a peel speed of 50mm / min; use a Keithley resistance meter to measure the connection resistance of the conductive adhesive bonding product. The specific test results are shown in Table 1.

[0074] Table 1 Performance test data

[0075] Initial modulus MPa Interface adhesion gf / cm On-resistance Ω Example 1 0.65 1100 0.24 Example 2 0.57 1050 0.41 Example 3 0.82 1200 0.31 Comparative Example 1 0.10 760 1.20 Comparative Example 2 0.20 720 3.51 Comparative Example 3 0.12 800 0.61 Comparative Example 4 0.32 830 1.12 Comparative Example 5 0.18 700 1.52 Comparative Example 6 0.24 750 1.22 Comparative Example 7 0.30 980 1.38

[0076] As shown in Table 1, it can be seen from Examples 1 to 3 and Comparative Example 3 that the present invention significantly improves the interface connection force of the ACF product for the circuit board connection by adding epoxy resin graphene intermediate modified 2-hydroxyethyl methacrylate phosphate in the preparation of the conductive adhesive, ensuring a more stable electrical contact; at the same time, the ACF prepared using the conductive adhesive of the present invention exhibits a higher initial modulus, which means that it can maintain better structural integrity when subjected to external force, reducing connection problems caused by deformation; in addition, the ACF prepared using the conductive adhesive of the present invention has a lower on-resistance, which is crucial for improving the current transmission efficiency of electronic components.

[0077] It can be seen from Comparative Examples 1 to 2 that when too little epoxy resin graphene modified 2-hydroxyethyl methacrylate phosphate is used in the preparation of conductive adhesive, the initial modulus of the prepared ACF will be reduced and the mechanical strength will be weakened, resulting in easy deformation or breakage in practical applications; lower interfacial adhesion means that the ACF may become loose or fall off when connecting electronic components, reducing the reliability of the connection; high on-resistance will increase energy consumption and reduce the efficiency and performance of electronic equipment.

[0078] It can be seen from Comparative Examples 4 to 5 that when a small amount of epoxy resin graphene intermediate is used for modification / 2-hydroxyethyl methacrylate phosphate is not modified / 2-hydroxyethyl methacrylate phosphate is only modified with epoxy resin / 2-hydroxyethyl methacrylate phosphate is only modified with graphene oxide, the prepared ACF also faces the problems of low initial modulus, low interfacial adhesion and large on-resistance, which is far inferior to the embodiment.

[0079] The various aspects, embodiments, and features of the present invention should be considered to be illustrative in all aspects and not limiting of the present invention, the scope of which is defined solely by the claims. Other embodiments, modifications, and uses will be apparent to those skilled in the art without departing from the spirit and scope of the claimed invention.

[0080] In the preparation method of the present invention, the order of each step is not limited to the order listed. For those skilled in the art, without creative work, the order of each step is also within the protection scope of the present invention. In addition, two or more steps or actions can be performed simultaneously.

[0081] Finally, it should be noted that the specific embodiments described herein are merely examples of the present invention, and are not intended to limit the implementation methods of the present invention. A person skilled in the art of the present invention may make various modifications or supplements to the specific embodiments described, or replace them in a similar manner. It is not necessary and impossible to provide all examples of all implementation methods here. However, these obvious changes or modifications derived from the essential spirit of the present invention still fall within the scope of protection of the present invention, and interpreting them as any additional limitation is contrary to the spirit of the present invention.

Claims

1. A conductive adhesive for ACF with high interface connection strength and high modulus, characterized in that: The conductive adhesive is processed from the following raw materials in parts by weight: 10 to 20 parts of butyl rubber, 20 to 30 parts of epoxy resin graphene modified 2-hydroxyethyl methacrylate phosphate, 1 to 10 parts of conductive particles, 30 to 70 parts of fillers, 20 to 40 parts of solvents, and 1 to 10 parts of initiators.

2. The conductive adhesive for ACF with high interface connection strength and high modulus according to claim 1, characterized in that: The epoxy resin graphene modified 2-hydroxyethyl methacrylate phosphate is processed from the following raw materials in parts by weight: 20 to 30 parts of epoxy resin graphene intermediate, 10 to 30 parts of 2-hydroxyethyl methacrylate phosphate, and 0.1 to 1 part of initiator.

3. The conductive adhesive for ACF with high interface connection strength and high modulus according to claim 2, characterized in that: The preparation method of epoxy resin graphene modified 2-hydroxyethyl methacrylate phosphate comprises the following steps: adding epoxy resin graphene intermediate, 2-hydroxyethyl methacrylate phosphate and initiator into a reaction kettle, heating up for reaction, cooling down and discharging to obtain epoxy resin graphene modified 2-hydroxyethyl methacrylate phosphate.

4. The conductive adhesive for ACF with high interface connection strength and high modulus according to claim 3, characterized in that: The reaction temperature is 95-120° C., and the reaction time is 6-10 hours.

5. The conductive adhesive for ACF with high interface connection strength and high modulus according to claim 2, characterized in that: The epoxy resin graphene intermediate is processed from the following raw materials in parts by weight: 60 to 75 parts of epoxy resin, 2 to 10 parts of graphene oxide, 0.1 to 1 part of triethylamine, and 20 to 60 parts of ethyl acetate.

6. The conductive adhesive for ACF with high interface connection strength and high modulus according to claim 5, characterized in that: The preparation method of the epoxy resin graphene intermediate comprises the following steps: adding epoxy resin, graphene oxide, triethylamine and ethyl acetate into a reaction kettle, heating the reaction kettle, and cooling the reaction kettle to obtain the epoxy graphene intermediate; The graphene oxide is carboxylated graphene oxide.

7. The conductive adhesive for ACF with high interface connection strength and high modulus according to claim 6, characterized in that: The reaction temperature is 60-90° C., and the reaction time is 1-5 hours.

8. The conductive adhesive for ACF with high interface connection strength and high modulus according to claim 1, characterized in that: The filler includes one or more of silicon dioxide, titanium dioxide, aluminum oxide, iron oxide, silicate, and carbon black; and / or, the solvent comprises one or more of toluene, methanol, ethanol, tetrahydrofuran, acetonitrile, N,N-dimethylformamide, and dimethyl sulfoxide; And / or, the initiator is an organic peroxidation initiator.

9. A method for preparing a conductive adhesive for ACF with high interface connection strength and high modulus as claimed in any one of claims 1 to 8, characterized in that: The preparation method comprises the following steps: weighing a solvent into a container, adding butyl rubber and epoxy resin graphene modified 2-hydroxyethyl methacrylate phosphate, heating to 30-60° C. to dissolve them in the solvent, adding filler and stirring evenly, then adding conductive particles, and finally adding an initiator, placing the mixture in a defoaming mixer and dispersing the mixture evenly, so as to obtain a conductive adhesive for ACF with high interface connection force and high modulus.

10. A high-interface connection strength and high-modulus ACF, which is obtained by coating and drying the conductive adhesive for ACF with high interface connection strength and high modulus as claimed in any one of claims 1 to 8.