Protective film and preparation method thereof, curved screen assembly and electronic equipment
By using a hardened layer composed of polyurethane acrylate resin and hyperbranched acrylic resin on electronic devices such as curved screen mobile phones, combined with the base layer and the shaping layer, the problem of poor wear resistance of the existing protective film is solved, and high hardness and resistance are achieved Scratch, extending service life.
Patent Information
- Application Number
- CN202411110545.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-01
AI Technical Summary
The protective films of existing curved screen mobile phones and other electronic devices have poor wear resistance, are easy to scratch, have short service life, and affect user experience.
Using a hardened layer composed of polyurethane acrylate resin and hyperbranched acrylic resin, combined with the base layer and the shaping layer, the mass ratio of polyurethane acrylate resin to hyperbranched acrylic resin in the hardened layer is between 1 and 4, forming a high hardness. and scratch-resistant atmosphere.
It significantly improves the wear and scratch resistance of the protective film, extends the service life, is suitable for curved screen applications that are not easy to crack, and reduces construction viscosity and energy consumption.
Smart Images

Figure CN118879216A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of electronics, and in particular to a protective film and a preparation method thereof, a curved screen assembly and an electronic device. Background Art
[0002] With the development of the form of electronic devices such as mobile phones, in order to pursue a large viewing area, thin body, and exquisite appearance, more and more mobile phones and other electronic devices are designed with 3D curved screen covers, with curved surfaces on the left and right long sides, and four curved surfaces with equal depth on four sides, etc. The protective film of curved screen mobile phones and other electronic devices in the related art has poor wear resistance, is easy to scratch, has a short service life, and long-term use will seriously affect the user experience. Summary of the invention
[0003] The embodiment of the present application provides a protective film having good wear resistance.
[0004] In a first aspect, an embodiment of the present application provides a protective film, comprising:
[0005] substrate layer;
[0006] a hardening layer, the hardening layer being disposed on one side of the substrate layer, the hardening layer comprising a polyurethane acrylate resin and a hyperbranched acrylic resin, wherein a mass ratio of the polyurethane acrylate resin to the hyperbranched acrylic resin in the hardening layer is in a range of 1 to 4; and
[0007] A shaping layer is arranged on a side of the substrate layer away from the hardening layer.
[0008] In a second aspect, the present application also provides a method for preparing a protective film, which comprises:
[0009] providing a substrate layer;
[0010] forming a hardening layer on one side of the substrate layer, the hardening layer comprising a polyurethane acrylate prepolymer and a hyperbranched acrylic resin, wherein the mass ratio of the polyurethane acrylate prepolymer to the hyperbranched acrylic resin in the hardening layer is in a range of 1 to 4; and
[0011] A shaping layer is formed on a side of the substrate layer facing away from the hardening layer.
[0012] In a third aspect, the embodiment of the present application further provides a curved screen assembly, which includes:
[0013] A curved screen, the curved screen having a display surface; and
[0014] The protective film described in the embodiment of the present application is arranged on the display surface, between the shaping layer, the substrate layer and the curved screen.
[0015] In a fourth aspect, an embodiment of the present application further provides an electronic device, comprising:
[0016] The curved screen assembly described in the embodiment of the present application; and
[0017] A processor is electrically connected to the curved screen assembly and is used to control the curved screen assembly to display.
[0018] The protective film of the embodiment of the present application comprises a substrate layer, a hardening layer and a shaping layer which are stacked in sequence, the hardening layer comprises a polyurethane acrylate resin and a hyperbranched acrylic resin, and in the hardening layer, the mass ratio of the polyurethane acrylate resin to the hyperbranched acrylic resin is in a range of 1 to 4. The polyurethane acrylate is the main molecular structure, providing the main mechanical properties and molecular chain structure, and the hyperbranched acrylic resin plays a toughening and strengthening role. Through the coordination of the polyurethane acrylate resin and the hyperbranched acrylic resin, the hardening layer has higher hardness and rigidity, higher wear resistance and scratch resistance, and better toughness. When applied to a curved screen, it can be bent better and is not prone to cracking. In addition, hyperbranched acrylic resin has the characteristics of good fluidity, low viscosity, not easy to crystallize, good film-forming properties, etc., and has good solubility and good weather resistance. The application of hyperbranched acrylic resin in polyurethane acrylate resin system can effectively increase the double bond content of the system, thereby effectively improving the rate of light curing (such as ultraviolet light curing, referred to as UV curing) and the mechanical properties of the hardened layer; furthermore, at the same solid content, hyperbranched acrylic resin can significantly reduce the viscosity of the system, which is beneficial to the construction of the hardened layer and saves energy. Furthermore, hyperbranched acrylic resin has more side chains, which can better form a cross-linked network structure in the hardened layer, increase the cross-linking degree of the hardened layer, and make the hardened layer have better toughness and wear resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0020] Figure 1 It is a schematic diagram of the planar structure of a protective film according to an embodiment of the present application.
[0021] Figure 2 The protective film of one embodiment of the present application is Figure 1 Schematic diagram of the structure in the AA direction.
[0022] Figure 3 The protective film of another embodiment of the present application is Figure 1Schematic diagram of the structure in the AA direction.
[0023] Figure 4 It is a schematic flow chart of a method for preparing a protective film according to an embodiment of the present application.
[0024] Figure 5 It is a schematic flow chart of a method for preparing a protective film according to another embodiment of the present application.
[0025] Figure 6 It is a schematic structural diagram of a curved screen assembly according to an embodiment of the present application.
[0026] Figure 7 It is a schematic diagram of the exploded structure of the curved screen assembly according to an embodiment of the present application.
[0027] Figure 8 It is a side view structural schematic diagram of a curved screen assembly according to an embodiment of the present application.
[0028] Fig. 9 It is a schematic diagram of the structure of an electronic device according to an embodiment of the present application.
[0029] Fig.10 It is a schematic diagram of a partial exploded structure of an electronic device according to an embodiment of the present application.
[0030] Fig.11 It is a side view of an electronic device according to an embodiment of the present application.
[0031] Fig.12 It is a circuit block diagram of an electronic device according to an embodiment of the present application.
[0032] Description of reference numerals:
[0033] 100-protective film, 10-base material layer, 20-hardening layer, 30-shaping layer, 40-adhesive layer, 200-curved screen assembly, 210-curved screen, 211-display surface, 300-electronic device, 310-processor, 320-memory, 330-housing, 340-middle frame, 350-camera module. DETAILED DESCRIPTION
[0034] In order to enable those skilled in the art to better understand the solution of the present application, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0035] The terms "first", "second", etc. in the specification and claims of this application and the above-mentioned drawings are used to distinguish different objects, rather than to describe a specific order. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device that includes a series of steps or units is not limited to the listed steps or units, but optionally includes steps or units that are not listed, or optionally includes other steps or units inherent to these processes, methods, products or devices.
[0036] The technical solutions in the embodiments of the present application will be described below in conjunction with the accompanying drawings.
[0037] It should be noted that, for the convenience of explanation, in the embodiments of the present application, the same figure marks represent the same components, and for the sake of brevity, detailed descriptions of the same components are omitted in different embodiments.
[0038] With the development of the form of electronic devices such as mobile phones, in order to pursue a large viewing area, thin body, and exquisite appearance, more and more mobile phones and other electronic devices are designed with 3D curved screen covers, with curved surfaces on the left and right long sides, and four curved surfaces with equal depth on four sides, etc. The protective film of curved screen mobile phones and other electronic devices in the related art has poor wear resistance, is easy to scratch, has a short service life, and long-term use will seriously affect the user experience.
[0039] Figure 1 Schematic diagram of the planar structure of a protective film 100 according to an embodiment of the present application. Figure 2 The protective film 100 of one embodiment of the present application is Figure 1 Schematic diagram of the structure in the AA direction.
[0040] See also Figure 1 and Figure 2 The embodiment of the present application provides a protective film 100, which includes: a substrate layer 10, a hardening layer 20 and a shaping layer 30, wherein the hardening layer 20 is arranged on one side of the substrate layer 10, and the hardening layer 20 includes a polyurethane acrylate resin and a hyperbranched acrylic resin. In the hardening layer 20, the mass ratio of the polyurethane acrylate resin to the hyperbranched acrylic resin ranges from 1 to 4; the shaping layer 30 is arranged on the side of the substrate layer 10 away from the hardening layer 20.
[0041] The protective film 100 of the embodiment of the present application is applied to electronic devices, as a protective film 100 for a 3D curved screen of an electronic device, and is used to protect the curved screen. Optionally, the electronic device may include but is not limited to portable electronic devices such as mobile phones, tablet computers, laptop computers, desktop computers, smart bracelets, smart watches, e-readers, game consoles, etc. Optionally, the curved screen may be curved on two relatively long sides, or on two relatively short sides, or on all four sides.
[0042] In the embodiments of the present application, when a numerical value range from a to b is involved, unless otherwise specified, it means that the numerical value can be any numerical value between a and b, including the endpoint numerical value a and the endpoint numerical value b.
[0043] It should be noted that, unless otherwise specified, the “content”, “fraction”, etc. in this application refer to mass content and mass fraction.
[0044] It can be understood that the shaping layer 30, the substrate layer 10 and the hardening layer 20 are stacked in sequence. When the protective film 100 is applied to a curved screen, the shaping layer 30 is closer to the display surface of the curved screen than the hardening layer 20. In other words, the hardening layer 20 is closer to the contact surface, that is, the outer surface, than the substrate layer 10.
[0045] It should be noted that the urethane acrylate resin is formed by curing a urethane acrylate prepolymer or oligomer. The hardened layer 20 is formed by curing a hardening liquid (at least one of thermal curing and photocuring).
[0046] Specifically, in the hardened layer 20, the mass ratio of the polyurethane acrylate resin to the hyperbranched acrylic resin can be, but is not limited to, 1, 1.3, 1.5, 1.8, 2, 2.3, 2.5, 2.8, 3, 3.2, 3.5, 3.8, 4, etc. Polyurethane acrylate is the main molecular structure, providing the main mechanical properties and molecular chain structure, and the hyperbranched acrylic resin plays a toughening and strengthening role. When the mass ratio of polyurethane acrylate to hyperbranched acrylic resin is too small, that is, the content of polyurethane acrylate is too low, the overall hardness and rigidity of the hardened layer 20 are poor, and the wear resistance and scratch resistance are poor; when the mass ratio of polyurethane acrylate to hyperbranched acrylic resin is too large, that is, the content of hyperbranched acrylic resin is too low, the content of polyurethane acrylate is too much, the flexibility of the hardened layer 20 is reduced, it is difficult to achieve curved bending, and when applied to a curved screen, it is easy to crack during the bending process. When the mass ratio of the polyurethane acrylate resin to the hyperbranched acrylic resin in the hardened layer 20 is in the range of 1 to 4, the hardened layer 20 can have higher hardness and rigidity, higher wear resistance and scratch resistance, and better toughness. When applied to a curved screen, it can be bent better and is less likely to crack.
[0047] In some embodiments, the hardened layer comprises, by mass fraction, 40% to 75% of polyurethane acrylate resin and 10% to 40% of hyperbranched acrylic resin.
[0048] Specifically, the mass fraction of the polyurethane acrylic resin in the hardening layer 20 may be, but is not limited to, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, etc. If the content of polyurethane acrylic resin is too low, the overall hardness and rigidity of the hardening layer 20 are poor, and the wear resistance and scratch resistance are poor; if the content of polyurethane acrylic resin is too high, the flexibility of the hardening layer 20 is reduced, and it is difficult to achieve curved bending, and when applied to a curved screen, it is easy to crack during the bending process.
[0049] Specifically, the mass fraction of the hyperbranched acrylic resin in the hardened layer 20 may be, but is not limited to, 10%, 15%, 20%, 25%, 30%, 35%, 40%, etc. If the hyperbranched acrylic resin in the hardened layer 20 is too low, the toughness of the hardened layer 20 is reduced, and it is difficult to achieve curved bending, and when applied to a curved screen, cracking is likely to occur during the bending process; if the hyperbranched acrylic resin in the hardened layer 20 is too high, the overall hardness and rigidity of the hardened layer 20 are poor, and the wear resistance and scratch resistance are poor.
[0050] The protective film 100 of the embodiment of the present application includes a substrate layer 10, a hardening layer 20 and a shaping layer 30 which are stacked in sequence. The hardening layer 20 includes a polyurethane acrylate resin and a hyperbranched acrylic resin. In the hardening layer 20, the mass ratio of the polyurethane acrylate resin to the hyperbranched acrylic resin is in a range of 1 to 4. The polyurethane acrylate is the main molecular structure, providing the main mechanical properties and molecular chain structure, and the hyperbranched acrylic resin plays a toughening and strengthening role. Through the coordination of the polyurethane acrylate resin and the hyperbranched acrylic resin, the hardening layer 20 has high hardness and rigidity, high wear resistance and scratch resistance, and good toughness. When applied to a curved screen, it can be better bent and is not prone to cracking. In addition, the hyperbranched acrylic resin has the characteristics of good fluidity, low viscosity, not easy to crystallize, good film-forming properties, etc., and has good solubility and good weather resistance. The application of hyperbranched acrylic resin in the polyurethane acrylate resin system can effectively increase the double bond content of the system, thereby effectively improving the rate of light curing (such as ultraviolet light curing, referred to as UV curing) and the mechanical properties of the hardened layer 20; furthermore, at the same solid content, the hyperbranched acrylic resin can significantly reduce the viscosity of the system, which is beneficial to the construction of the hardened layer 20 and saves energy. Furthermore, the hyperbranched acrylic resin has more side chains, which can better form a cross-linked network structure in the hardened layer 20, increase the cross-linking degree of the hardened layer 20, and make the hardened layer 20 have better toughness and wear resistance.
[0051] Optionally, the thickness of the protective film 100 ranges from 100 μm to 120 μm. Specifically, the thickness of the protective film 100 may be, but is not limited to, 100 μm, 102 μm, 104 μm, 106 μm, 108 μm, 110 μm, 112 μm, 114 μm, 116 μm, 118 μm, 120 μm, etc. If the thickness of the protective film 100 is too thin, the strength of the protective film 100 is insufficient, and when applied to a curved screen assembly, the protective force of the curved screen is reduced; if the thickness of the protective film 100 is too thick, the rigidity of the protective film 100 is too high, and when the protective film 100 is attached to the curved screen, it is easy to warp.
[0052] Furthermore, the thickness of the protective film 100 ranges from 105 μm to 110 μm. Specifically, the thickness of the protective film 100 may be, but is not limited to, 105 μm, 106 μm, 107 μm, 108 μm, 109 μm, 110 μm, etc. In this way, the protective film 100 can have better protection and better fit with the curved screen, making it less prone to warping.
[0053] Optionally, the thickness of the substrate layer 10 ranges from 18 μm to 40 μm. Specifically, the thickness of the substrate layer 10 may be, but is not limited to, 18 μm, 19 μm, 20 μm, 21 μm, 22 μm, 23 μm, 24 μm, 25 μm, 28 μm, 30 μm, 33 μm, 35 μm, 38 μm, 40 μm, etc. If the thickness of the substrate layer 10 is too thin, the coating difficulty will be increased when the substrate layer 10 is prepared by coating, and the hardness is not enough, which reduces the wear resistance of the protective film 100. In addition, the stiffness of the substrate layer 10 is not enough, which makes the protective film 100 prone to wrinkles, orange peel and other poor appearance phenomena; if the thickness of the substrate layer 10 is too thick, the rebound force of the protective film 100 during shaping is too large, which makes the protective film 100 not fit the edge of the curved screen well and prone to warping.
[0054] Furthermore, the thickness of the substrate layer 10 is in the range of 18 μm to 25 μm. In this way, the substrate layer 10 has good coating performance during preparation, high strength and hardness, and low rebound force, which can well support the hardening layer 20. When applied to a curved screen, the protective film 100 has good adhesion to the curved screen and is not prone to warping.
[0055] In some embodiments, the substrate layer 10 is isotropic, and the substrate layer 10 includes at least one of thermoplastic elastomers such as thermoplastic polyurethane and silicone rubber.
[0056] It can be understood that the substrate layer 10 is non-polarized.
[0057] In the related art, the substrate is usually made of polyethylene terephthalate (PET) and the like. The substrate is usually prepared by biaxial stretching. During the stretching process, the molecular chains will be oriented, which makes the substrate of the related art anisotropic and has high mechanical strength. When it is applied to the protective film of the curved screen and is formed, the forming layer will shrink in volume toward the substrate layer after photocuring. The modulus of the substrate layer is large, which will produce greater stress and rebound force, so that warping, bubbles, wrinkles, etc. are likely to occur at the edge of the curved screen, making it difficult to fully fit the curved screen.
[0058] The substrate layer 10 of the embodiment of the present application is isotropic, and thermoplastic polyurethane and silicone rubber have a lower elastic modulus than substrates such as PET, are soft and easy to deform, and have extremely low rebound force. Therefore, when applied to a curved screen, the substrate layer 10 can easily deform together with the shaping layer when the protective film 100 is formed, so that it can better fit the structure of the curved screen, and is not prone to rebound or warping after fitting, thereby better protecting the curved screen.
[0059] In some embodiments, the elastic modulus of the substrate layer 10 ranges from 1.5 GPa to 4 GPa. Specifically, the elastic modulus of the substrate layer 10 may be, but is not limited to, 1.5 GPa, 1.8 GPa, 2.0 GPa, 2.3 GPa, 2.5 GPa, 2.8 GPa, 3.0 GPa, 3.3 GPa, 3.5 GPa, 3.8 GPa, 4.0 GPa, etc. If the elastic modulus of the substrate layer 10 is too low, the hardness of the substrate layer 10 is insufficient, which reduces the hardness and wear resistance of the protective film 100. In addition, the stiffness of the substrate layer 10 is insufficient, which makes the protective film 100 prone to wrinkles, orange peel and other poor appearance phenomena; if the elastic modulus of the substrate layer 10 is too high, the rebound force of the protective film 100 during shaping is too large, which makes the protective film 100 not fit the edge of the curved screen well and prone to warping.
[0060] Optionally, the tensile strength of the substrate layer 10 ranges from 40MPa to 100MPa. Specifically, the tensile strength of the substrate layer 10 may be, but is not limited to, 40MPa, 50MPa, 60MPa, 70MPa, 80MPa, 90MPa, 100MPa, etc. If the tensile strength of the substrate layer 10 is too low, the hardness of the substrate layer 10 is insufficient, which reduces the hardness and wear resistance of the protective film 100. In addition, the stiffness of the substrate layer 10 is insufficient, which makes the protective film 100 prone to wrinkles, orange peel and other poor appearance phenomena; if the tensile strength of the substrate layer 10 is too high, the rebound force of the protective film 100 during shaping is too large, which makes the protective film 100 not fit the edge of the curved screen well and prone to warping.
[0061] Optionally, the elongation at break of the substrate layer 10 ranges from 1% to 5%. Specifically, the elongation at break of the substrate layer 10 may be, but is not limited to, 1%, 1.5%, 2%, 3%, 4%, 5%, etc. If the elongation at break of the substrate layer 10 is too large, the hardness of the substrate layer 10 is insufficient, which reduces the hardness and wear resistance of the protective film 100. In addition, the stiffness of the substrate layer 10 is insufficient, which makes the protective film 100 prone to wrinkles, orange peel and other poor appearance phenomena; if the elongation at break of the substrate layer 10 is too small, the bending and stretching properties of the substrate layer 10 are insufficient, and the rebound force of the protective film 100 during shaping is too large, which makes the protective film 100 not fit the edge of the curved screen well and prone to warping.
[0062] Optionally, the thickness of the hardened layer 20 ranges from 1 μm to 5 μm. Specifically, the thickness of the hardened layer 20 may be, but is not limited to, 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, etc. If the thickness of the hardened layer 20 is too thin, the hardness and wear resistance of the hardened layer 20 are reduced, and the stiffness is reduced, so that the smoothness and feel of the protective film 100 are reduced; if the thickness of the hardened layer 20 is too thick, the hardness of the hardened layer 20 is too large, and the rebound force of the protective film 100 during shaping is too large, so that the protective film 100 is not sufficiently fitted to the edge of the curved screen, and warping is prone to occur.
[0063] In some embodiments, the number average molecular weight of the hyperbranched acrylic resin ranges from 5000 to 20000. Specifically, the number average molecular weight of the hyperbranched acrylic resin may be, but is not limited to, 5000, 8000, 10000, 12000, 14000, 16000, 18000, 20000, etc. If the number average molecular weight of the hyperbranched acrylic resin is too small, it is difficult to form a hyperbranched structure, and it is difficult to improve the toughness of the hardened layer 20 while making the hardening liquid have a lower viscosity; if the number average molecular weight of the hyperbranched acrylic resin is too large, the viscosity of the hardening liquid is increased, which is not conducive to the coating of the hardening liquid and reduces the processing performance of the hardened layer 20.
[0064] In some embodiments, the hyperbranched acrylic resin has the structural formula:
[0065]
[0066] Herein, m is an integer from 1 to 14, and n is an integer from 50 to 200.
[0067] It can be understood that the annular carbon structure of the hyperbranched acrylic resin can be a three-membered ring to a sixteen-membered ring. For example, when m is 1, the annular carbon structure is a three-membered ring, and the hyperbranched acrylic resin has three branches; when m is 3, the annular carbon structure is a five-membered ring, and the hyperbranched acrylic resin has five branches; when m is 8, the annular carbon structure is a ten-membered ring, and the hyperbranched acrylic resin has ten branches; when m is 14, the annular carbon structure is a sixteen-membered ring, and the hyperbranched acrylic resin has three branches; when m is 1, the annular carbon structure is a three-membered ring, and the hyperbranched acrylic resin has sixteen branches.
[0068] Specifically, the value of m can be, but is not limited to, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, etc. If m is too small, it is difficult to form a hyperbranched structure, and it is difficult to improve the toughness of the hardened layer 20 while making the hardening liquid have a lower viscosity; if m is too large, the preparation cost of the hyperbranched acrylic resin is increased, and it is even difficult to achieve.
[0069] Specifically, the value of n can be, but is not limited to, 50, 60, 80, 100, 120, 140, 160, 180, 200, etc. If n is too small, it is difficult to form a hyperbranched structure, and it is difficult to improve the toughness of the hardened layer 20 while making the hardening liquid have a low viscosity; if n is too large, the viscosity of the hardening liquid is increased, which is not conducive to the coating of the hardening liquid and reduces the processing performance of the hardened layer 20.
[0070] The use of the hyperbranched acrylic resin of this embodiment can better improve the toughness of the hardened layer 20 while making the hardening liquid have a lower viscosity and better processing performance.
[0071] Furthermore, the hyperbranched acrylic resin may be, but is not limited to, at least one of the following structural formulas:
[0072]
[0073] Here, n is an integer from 50 to 200.
[0074] In some embodiments, the hardening layer 20 further includes short-chain fluoride.
[0075] It can be understood that in this embodiment, the hardening layer 20 at least includes polyurethane acrylate resin, hyperbranched acrylic resin and short-chain fluoride.
[0076] In this embodiment, by adding short-chain fluoride to the hardened layer 20 , the anti-fouling and anti-fingerprint properties of the hardened layer 20 can be improved, the water drop angle of the hardened layer 20 can be increased, the friction coefficient of the hardened layer 20 can be reduced, and the wear resistance of the hardened layer 20 can be increased.
[0077] Optionally, in the hardened layer 20, the mass fraction of the short-chain fluoride ranges from 5% to 15%. Specifically, in the hardened layer 20, the mass fraction of the short-chain fluoride may be, but is not limited to, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, etc. In the hardened layer 20, if the mass fraction of the short-chain fluoride is too low, the fluorine content in the hardened layer 20 is insufficient, which is not conducive to improving the stain resistance, anti-fingerprint performance and wear resistance of the hardened layer 20; in the hardened layer 20, if the mass fraction of the short-chain fluoride is too high, the stain resistance and anti-fingerprint performance of the hardened layer 20 will not be improved, but the hardness and wear resistance of the hardened layer 20 will be greatly reduced.
[0078] Optionally, the short-chain fluorinated compound may be, but is not limited to, at least one of perfluoropolyether (PFPE) and perfluoropolyether derivatives.
[0079] Optionally, the number average molecular weight of the short-chain fluoride ranges from 2000 to 8000. Specifically, the number average molecular weight of the short-chain fluoride may be, but is not limited to, 2000, 3000, 4000, 5000, 6000, 7000, 8000, etc. If the number average molecular weight of the short-chain fluoride is too small, the fluorine content in the hardened layer 20 is insufficient, which is not conducive to improving the stain resistance, anti-fingerprint performance and wear resistance of the hardened layer 20; if the number average molecular weight of the short-chain fluoride is too large, the preparation cost of the short-chain fluoride is increased, or even cannot be obtained.
[0080] In some embodiments, the hardening layer 20 further includes inorganic nanoparticles. Adding inorganic nanoparticles to the hardening layer 20 can increase the wear resistance and hardness of the hardening layer 20 and improve the service life of the protective film 100.
[0081] Optionally, in the hardened layer 20 , the mass fraction of the inorganic nanoparticles ranges from 5% to 20%.
[0082] Specifically, in the hardened layer 20, the mass fraction of the inorganic nanoparticles may be, but is not limited to, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, etc. In the hardened layer 20, if the mass fraction of the inorganic nanoparticles is too low, the improvement of the hardness and wear resistance of the hardened layer 20 is limited; in the hardened layer 20, if the mass fraction of the inorganic nanoparticles is too high, the dispersibility of the inorganic nanoparticles is reduced, and they are prone to agglomeration, forming stress concentration points, thereby reducing the mechanical properties of the hardened layer 20, and in addition, the transparency of the hardened layer 20 is reduced, and the light transmittance of the protective film 100 is reduced.
[0083] Optionally, the inorganic nanoparticles may be, but are not limited to, at least one of aluminum oxide, silicon dioxide, boron nitride, silicon nitride, zirconium oxide, and the like.
[0084] In some embodiments, the raw material components (also referred to as hardening liquid) of the hardening layer 20 include, by mass fraction: 20% to 50% of polyurethane acrylate prepolymer, 10% to 30% of hyperbranched acrylic resin, 3% to 10% of short-chain fluoride, 1% to 10% of inorganic nanoparticles, 5% to 20% of the first reaction monomer, and 0.5% to 2% of the first photoinitiator and the remainder of the first solvent.
[0085] In other words, the hardening liquid includes, by mass fraction: 20% to 50% of polyurethane acrylate prepolymer, 10% to 30% of hyperbranched acrylic resin, 3% to 10% of short-chain fluoride, 1% to 10% of inorganic nanoparticles, 5% to 20% of the first reaction monomer, 0.5% to 2% of the first photoinitiator and the balance of the first solvent.
[0086] Specifically, the mass fraction of the polyurethane acrylate prepolymer in the raw material components of the hardened layer 20 may be, but not limited to, 20%, 25%, 30%, 35%, 40%, 45%, 50%, etc. The mass fraction of the hyperbranched acrylic resin in the raw material components of the hardened layer 20 may be, but not limited to, 10%, 15%, 20%, 25%, 30%, etc. The mass fraction of the short-chain fluoride in the raw material components of the hardened layer 20 may be, but not limited to, 3%, 5%, 7%, 9%, 10%, etc. The mass fraction of the inorganic nanoparticles in the raw material components of the hardened layer 20 may be, but not limited to, 1%, 3%, 5%, 7%, 9%, 10%, etc. The mass fraction of the first reaction monomer in the raw material components of the hardened layer 20 may be, but not limited to, 5%, 8%, 10%, 13%, 15%, 18%, 20%, etc. The mass fraction of the first photoinitiator in the raw material components of the hardened layer 20 may be, but is not limited to, 0.5%, 1%, 1.5%, 2%, etc.
[0087] Optionally, the first reactive monomer may be, but is not limited to, at least one of acrylic monomers such as ethoxylated trimethylolpropane triacrylate, pentaerythritol hexaacrylate, isobornyl acrylate, and 1,6-hexanediol diacrylate.
[0088] Optionally, the first photoinitiator can be, but is not limited to, methyl benzoylformate, diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide (TPO), propyl thioxanthone (ITX), benzophenone (BP), photoinitiator 1700 (25 wt% of photoinitiator 819 and 75 wt% of photoinitiator 1173), bis [2,6-difluoro-3- (1H-pyrrolyl-1) phenyl] titanocene (photoinitiator 784), photoinitiator 1800 (25% photoinitiator 819 and 75% photoinitiator 184), photoinitiator 4265 (50% TPO and 50% photoinitiator 1173), 1-hydroxycyclohexyl phenyl ketone (1-hydroxycyclohexyl phenyl ketone, photoinitiator 184), 2-Hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone (photoinitiator 2959), 2-hydroxy-2-methyl-1-phenyl-1-propanone (photoinitiator 1173), 2-methyl-1-(4-methylthiophenyl)-2-morpholinyl-1-propanone (photoinitiator 907), 2-hydroxy-1-[4-[4-(2-hydroxy-2-methylpropionyl)phenoxy]phenyl]-2-methylpropanone (photoinitiator 160), etc.
[0089] Optionally, the mass fraction of the first solvent in the raw material component of the hardened layer 20 ranges from 20% to 60.5%. Specifically, the mass fraction of the first solvent in the raw material component of the hardened layer 20 can be, but is not limited to, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60.5%, etc.
[0090] Optionally, the first solvent may be, but is not limited to, one or more of ethyl acetate, propyl acetate, butyl acetate, cyclohexanone, propylene glycol methyl ether, propylene glycol methyl ether acetate, ethylene glycol monobutyl ether, ethylene glycol monomethyl ether, isopropanol, butanone, and methyl butanone.
[0091] Optionally, the thickness of the shaping layer 30 is in the range of 60μm to 120μm. Specifically, the thickness of the shaping layer 30 may be, but is not limited to, 60μm, 70μm, 80μm, 90μm, 100μm, 110μm, 120μm, etc. If the thickness of the shaping layer 30 is too thin, when the protective film 100 is applied to the curved screen and shaped, the shaping force provided by the shaping layer 30 is insufficient, so that the protective film 100 is prone to warping. In addition, if the shaping layer 30 is too thin, the hardness and stiffness of the protective film 100 will be reduced, affecting the wear resistance of the protective film 100. If the thickness of the shaping layer 30 is too thick, it will increase the difficulty of coating the shaping layer 30, and it is easy to make the coating of the shaping layer 30 uneven. In addition, after the shaping layer 30 is cured, the volume shrinks too much, and the internal stress generated by the volume shrinkage is easy to cause the protective film 100 to warp when it is attached to the curved screen.
[0092] Further, the thickness of the shaping layer 30 is in the range of 70 μm to 80 μm. Specifically, the thickness of the shaping layer 30 may be, but is not limited to, 70 μm, 72 μm, 74 μm, 76 μm, 78 μm, 80 μm, etc. In this way, the shaping layer 30 has a higher shaping force and a more suitable hardness, and is not prone to warping when attached to a curved screen.
[0093] In some embodiments, the raw material components (also referred to as fixing liquid) of the fixing layer 30 include a first raw material component and a second raw material component, the first raw material component includes a first resin and a first coupling agent, the second raw material component includes a second resin and a second coupling agent, the first resin includes a polyurethane acrylate prepolymer, the second resin includes an acrylic monomer, one of the first coupling agent and the second coupling agent is a silane coupling agent, and the other is a silane coupling agent having a thermally reactive group.
[0094] It can be understood that the setting layer 30 is formed by coating and curing a setting liquid.
[0095] It can be understood that the setting liquid includes a first raw material component and a second raw material component.
[0096] Optionally, the silane coupling agent may be, but is not limited to, at least one of 2-chloroethylmethyldimethoxysilane, γ-aminopropyltriethoxysilane (KH550), 3-(2,3-epoxypropoxy)propyltrimethoxysilane (KH560), γ-methacryloxypropyltrimethoxysilane (KH570), and the like.
[0097] Optionally, the thermal reaction group may be, but is not limited to, at least one of an isocyanate group, a hydroxyl group, a carboxyl group, etc. The silane coupling agent having a thermal reaction group may be, but is not limited to, a silane coupling agent having a group such as an isocyanate group, a hydroxyl group, a carboxyl group, etc. Specifically, the silane coupling agent having a thermal reaction group may be, but is not limited to, at least one of 3-isocyanate propyl trimethoxy silane, a dihydroxy silane coupling agent, etc.; that is, the second coupling agent may be, but is not limited to, at least one of 3-isocyanate propyl trimethoxy silane, a dihydroxy silane coupling agent, etc.
[0098] In this embodiment, the shaping layer 30 includes a first raw material component and a second raw material component, the first raw material component includes a first resin and a first coupling agent, the second raw material component includes a second resin and a second coupling agent, one of the first coupling agent and the second coupling agent is a silane coupling agent, and the other is a silane coupling agent with a thermal reaction group. Adding a silane coupling agent to the raw material components of the shaping layer 30 can improve the compatibility of the first raw material component and the second raw material component. The silane coupling agent with a thermal reaction group can form a cross-linked network structure in the shaping layer 30, and increase the cross-linking degree of the shaping layer 30 without affecting the flexibility of the shaping layer 30, so that the shaping layer 30 has better resistance to high and low temperature. In addition, the addition of the first coupling agent and the second coupling agent can also increase the bonding performance of the shaping layer 30 and the film layer directly attached to the substrate layer 10.
[0099] In some embodiments, the first raw material component includes, by mass fraction, 20% to 70% of a polyurethane acrylate prepolymer, 0.1% to 1% of a first coupling agent, 15% to 30% of a second reactive monomer, 5% to 30% of a curing agent, 0.5% to 3% of a second photoinitiator, and the remainder a second solvent.
[0100] Specifically, the mass fraction of the polyurethane acrylate prepolymer in the first raw material component may be, but not limited to, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, etc. The mass fraction of the first coupling agent in the first raw material component may be, but not limited to, 0.1%, 0.2%, 0.4%, 0.5%, 0.8%, 1%, etc. The mass fraction of the second reactive monomer in the first raw material component may be, but not limited to, 15%, 18%, 20%, 23%, 25%, 28%, 30%, etc. The mass fraction of the curing agent in the first raw material component may be, but not limited to, 5%, 8%, 10%, 13%, 15%, 18%, 20%, 23%, 25%, 28%, 30%, etc. The mass fraction of the second photoinitiator in the first raw material component can be, but is not limited to, 0.8%, 1%, 1.3%, 1.5%, 1.8%, 2%, 2.3%, 2.5%, 2.8%, 3%, etc.
[0101] Optionally, the second reactive monomer may be, but is not limited to, at least one of hydroxyethyl methacrylate, ethylene glycol dimethacrylate, diphenylmethane diisocyanate, etc. The second reactive monomer is used to participate in the reaction and dilute the glue solution composed of the first raw material component.
[0102] Optionally, the curing agent may be, but is not limited to, at least one of succinic anhydride, maleic anhydride, and the like.
[0103] Optionally, the second photoinitiator may be but is not limited to at least one of methyl benzoylformate, TPO, ITX, BP, photoinitiator 1700, photoinitiator 784, photoinitiator 1800, photoinitiator 4265, photoinitiator 184, photoinitiator 2959, photoinitiator 1173, photoinitiator 907, photoinitiator 160, etc.
[0104] Optionally, the weight fraction of the second solvent in the first raw material component is 10% to 50%, specifically, it can be but not limited to 10%, 20%, 30%, 40%, 50% and the like.
[0105] Optionally, the second solvent may be, but is not limited to, one or more of ethyl acetate, propyl acetate, butyl acetate, toluene, cyclohexanone, propylene glycol methyl ether, propylene glycol methyl ether acetate, ethylene glycol monobutyl ether, ethylene glycol monomethyl ether, isopropanol, butanone, and methyl butanone.
[0106] Optionally, in the first raw material component, the weight average molecular weight of the polyurethane acrylate prepolymer ranges from 4000 to 12000. Specifically, in the first raw material component, the weight average molecular weight of the polyurethane acrylate prepolymer can be, but is not limited to, 4000, 5000, 6000, 7000, 8000, 9000, 10000, 11000, 12000, etc. In this embodiment, if the weight average molecular weight of the polyurethane acrylate prepolymer in the first raw material component is too low, then after thermal curing, the degree of curing of the shaping layer 30 is too low, which reduces the mechanical properties of the shaping layer 30, or even makes the mechanical properties of the shaping layer 30 fail to meet the requirements; if the weight average molecular weight of the polyurethane acrylate prepolymer in the first raw material component is too high, the viscosity of the shaping liquid is too high, which is not conducive to the construction of the shaping liquid. In addition, if the weight average molecular weight of the polyurethane acrylate prepolymer is too high, after the shaping liquid is thermally cured, a large molecular cross-linking network is formed, and the hardness of the thermally cured shaping layer 30 (before light curing) is too high. When the shaping layer 30 is applied to a curved screen assembly and the film is pasted, it is easy to warp, which is not conducive to the pasting of the protective film 100.
[0107] Optionally, the second raw material component includes, by mass fraction, 40% to 80% of an acrylic monomer, 0.1% to 1% of a second coupling agent, 1% to 5% of a film-forming agent, and the balance a third solvent.
[0108] Specifically, the mass fraction of the acrylic monomer in the second raw material component may be, but not limited to, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, etc. The mass fraction of the second coupling agent in the second raw material component may be, but not limited to, 0.1%, 0.2%, 0.4%, 0.5%, 0.8%, 1%, etc. The mass fraction of the film-forming agent in the second raw material component may be, but not limited to, 1%, 2%, 3%, 4%, 5%, etc.
[0109] Optionally, the acrylic monomer may be, but is not limited to, at least one of hydroxyethyl methacrylate, methacrylic acid (MMA), ethylene glycol dimethacrylate, and the like.
[0110] Alternatively, the film former may be, but is not limited to, poly(melamine-co-formaldehyde)methanol.
[0111] Optionally, the weight fraction of the third solvent in the second raw material component is 18.9% to 60%, specifically, it can be but not limited to 18.9%, 20%, 30%, 40%, 50%, 660%, etc.
[0112] Optionally, the third solvent may be, but is not limited to, one or more of methylal, ethyl acetate, propyl acetate, butyl acetate, cyclohexanone, propylene glycol methyl ether, propylene glycol methyl ether acetate, ethylene glycol monobutyl ether, ethylene glycol monomethyl ether, isopropanol, butanone, and methyl butanone.
[0113] In this embodiment, the first raw material component includes 20% to 70% of polyurethane acrylate prepolymer, 0.1% to 1% of the first coupling agent, 15% to 30% of the second reactive monomer, 5% to 30% of the curing agent and 0.5% to 3% of the second photoinitiator by mass fraction; the second raw material component includes 40% to 80% of acrylic monomer, 0.1% to 1% of the second coupling agent, and 1% to 5% of the film-forming agent by mass fraction. By designing the content of the first raw material component, the prepared shaping layer 30 has a good shaping ability, and the shaping layer 30 has a high structural strength after being applied to the curved screen and shaped, so as to have a good high and low temperature resistance.
[0114] In some embodiments, in the raw material components of the shaping layer 30 , the mass ratio of the first raw material component to the second raw material component is in a range of 3 to 8.
[0115] Specifically, in the raw material components of the setting layer 30 (i.e., in the setting liquid), the mass ratio of the first raw material component to the second raw material component can be, but is not limited to, 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5, 7, 7.5, 8, etc. The first raw material component provides the main thermosetting resin for the raw material components (setting liquid) of the setting layer 30, and the second raw material component is mainly a small molecule containing double bonds and hydroxyl groups, a part of which participates in the thermosetting reaction and a part of which participates in the UV light curing reaction. If the mass ratio of the first raw material component to the second raw material component is too small, the content of the first raw material component is too low, the content of the polyurethane acrylate prepolymer in the setting liquid is insufficient, the main molecular structure strength is poor, and the temperature deformation resistance is poor, which reduces the structural strength and temperature deformation resistance of the setting layer 30; if the mass ratio of the first raw material component to the second raw material component is too large, the content of the polyurethane acrylate prepolymer in the setting liquid is too high, the UV light curing reaction part of the setting liquid is low, and the setting effect is poor. When the mass ratio of the first raw material component to the second raw material component in the raw material components of the shaping layer 30 is in a range of 3 to 8, the shaping layer 30 can have a better shaping ability and a higher structural strength after shaping.
[0116] In some embodiments, the protective film 100 is applied to a curved screen, the shaping layer 30 is a heat-light dual-curing shaping layer 30, and before the protective film 100 is applied to the curved screen, the shaping layer 30 is thermally cured, and when the protective film 100 is applied to the curved screen, the shaping layer 30 is light-cured, and the light-curing energy of the shaping layer 30 is in the range of 6000 mj / cm 2 Up to 12000mj / cm 2 .
[0117] It should be noted that the shaping layer 30 is prepared using a heat-light dual-curing shaping liquid. When the protective film 100 is prepared, the heat-light dual-curing shaping liquid is first heat-cured. When the shaping layer 30 is attached to the curved screen, the shaping layer 30 is illuminated (for example, by a mercury lamp for ultraviolet light), so that the shaping layer 30 is photocured, generating a shaping force toward the curved screen, and coupled with the adhesive force of the adhesive layer, the shaping layer 30 cooperates with the adhesive layer, so that the protective film 100 as a whole is only attached to the curved screen, and the edge of the protective film 100 does not rebound or warp.
[0118] It can be understood that the setting liquid is a heat-light dual-curing setting liquid.
[0119] Specifically, the energy of the light curing of the shaping layer 30 may be, but is not limited to, 6000 mj / cm 2 、7000mj / cm 2 、8000mj / cm 2 、9000mj / cm2 、10000mj / cm 2 、11000mj / cm 2 、12000mj / cm 2 wait.
[0120] In this embodiment, if the energy of the light curing of the shaping layer 30 is too low, the shaping layer 30 will not be completely cured, and the generated shaping force will be insufficient, which will affect the shaping effect, and the shaping layer 30 will not be hard enough, which will affect the anti-nail mark effect of the shaping layer 30; if the energy of the light curing of the shaping layer 30 is too high, the degree of curing of the shaping layer 30 will be too high. After curing, the volume shrinks too much, the internal stress is too large, and the force resisting the direction of the adhesive force is too large, which makes the protective film 100 easy to warp.
[0121] In some embodiments, the curing degree of the shaping layer 30 is in the range of 80% to 95%. It can be understood that before the protective film 100 is applied to the curved screen, the shaping layer 30 is thermally cured but not photocured, and after the shaping layer 30 is thermally cured, the curing degree of the thermally cured is in the range of 80% to 95%.
[0122] Specifically, the curing degree of the shaping layer 30 can be, but is not limited to, 80%, 82%, 84%, 86%, 88%, 90%, 92%, 94%, 95%, etc. If the curing degree of the shaping layer 30 is too low, the mechanical properties of the shaping layer 30 before film lamination are too low, making it difficult to process and shape, and affecting the subsequent coating of the adhesive layer. In addition, when the protective film 100 is attached to the curved screen, the shaping layer 30 is prone to further thermal curing in the environment over time, generating a large shrinkage stress, making the protective film 100 prone to warping; if the curing degree of the shaping layer 30 is too high, the shaping layer 30 is too hard before the protective film 100 is applied to the curved screen assembly, making the hardness of the protective film 100 too high, and when the protective film 100 is attached to the curved screen, the protective film 100 is difficult to be well attached to the surface of the curved screen.
[0123] Optionally, the curing degree of the shaping layer 30 is in the range of 70% to 90%. It can be understood that after the protective film 100 is attached to the curved screen and the curing degree of the shaping layer 30 is in the range of 70% to 90%.
[0124] Specifically, the curing degree of the shaping layer 30 by light curing can be, but is not limited to, 70%, 72%, 74%, 76%, 78%, 80%, 82%, 84%, 86%, 88%, 90%, etc. If the curing degree of the shaping layer 30 by light curing is too low, the shaping force generated by the shaping layer 30 after light curing is low, the shaping effect of the protective film 100 is not good, and the overall hardness of the protective film 100 is low, which reduces the protective effect of the protective film 100 on the curved screen; if the curing degree of the shaping layer 30 by light curing is too high, the protective film 100 is attached to the curved screen, and after the shaping layer 30 is light cured, the shaping layer 30 shrinks too much, and the shrinkage stress generated is too large, so that the four corners of the protective film 100 are prone to warping.
[0125] Figure 3 The protective film 100 of another embodiment of the present application is Figure 1 Schematic diagram of the structure in the AA direction.
[0126] See also Figure 3 In some embodiments, the protective film 100 further includes an adhesive layer 40, which is disposed on the surface of the shaping layer 30 away from the substrate layer 10, and the peeling force of the shaping layer 30 on the surface with a water drop angle of 115° after thermal curing and before light curing is in the range of 40 gf / 25mm to 100 gf / 25mm; after the shaping layer 30 is thermally and lightly cured, the peeling force of the adhesive layer 40 on the surface with a water drop angle of 115° is in the range of 10 gf / 25mm to 40 gf / 25mm.
[0127] It can be understood that the adhesive layer 40 is used to adhere the protective film 100 to the curved screen.
[0128] Optionally, after the shaping layer 30 is thermally cured and before light-curing, the peeling force of the adhesive layer 40 on the curved screen with a water drop angle of 115° ranges from 40gf / 25mm to 100gf / 25mm; after the shaping layer 30 is thermally-light-durable, the surface peeling force of the adhesive layer 40 on the curved screen with a water drop angle of 115° ranges from 10gf / 25mm to 40gf / 25mm.
[0129] It should be noted that after the shaping layer 30 is photocured, the shaping layer shrinks in volume and becomes hard, generating a shrinking tensile force or internal stress on the adhesive layer 40, thereby making the adhesive layer 40 hard as a whole and reducing its viscosity. Therefore, after the shaping layer 30 is dual-cured by heat and light, the peeling force of the adhesive layer 40 on the curved screen or surface is reduced.
[0130] Specifically, after the shaping layer 30 is thermally cured and before light cured, the peeling force of the adhesive layer 40 on a surface with a water drop angle of 115° may be, but is not limited to, 40gf / 25mm, 45gf / 25mm, 50gf / 25mm, 55gf / 25mm, 60gf / 25mm, 65gf / 25mm, 70gf / 25mm, 80gf / 25mm, 90gf / 25mm, 100gf / 25mm, etc.
[0131] Specifically, after the shaping layer 30 is cured by heat and light, the peeling force of the adhesive layer 40 on the surface with a water drop angle of 115° can be but not limited to 10gf / 25mm, 15gf / 25mm, 20gf / 25mm, 25gf / 25mm, 30gf / 25mm, 35gf / 25mm, 40gf / 25mm, etc.
[0132] Optionally, the material of the adhesive layer 40 may be, but is not limited to, at least one of silicone glue, acrylic glue, and the like.
[0133] In this embodiment, if the peeling force of the adhesive layer 40 on the surface with a water drop angle of 115° is too small, then when the protective film 100 is attached to the curved screen, the adhesion between the protective film 100 and the curved screen is insufficient, and it is easy to be lifted or even fail to stick; if the peeling force of the adhesive layer 40 on the surface with a water drop angle of 115° is too large, the adhesion between the adhesive layer 40 and the curved screen is too high, and the air exhaust is poor. In addition, when the protective film 100 is replaced, the adhesion between the protective film 100 and the curved screen is too large, and the curved screen is easily damaged.
[0134] Optionally, the thickness of the adhesive layer 40 ranges from 8 μm to 20 μm. Specifically, the thickness of the adhesive layer 40 may be, but is not limited to, 8 μm, 10 μm, 12 μm, 14 μm, 16 μm, 18 μm, 20 μm, etc. If the thickness of the adhesive layer 40 is too thin, the adhesive force provided by the adhesive layer 40 is different, and the protective film 100 is prone to warping and bubbles when applied to a curved screen; if the thickness of the adhesive layer 40 is too thick, since the adhesive layer 40 is relatively soft, the hardness of the protective film 100 is reduced, thereby reducing the anti-nail mark effect of the protective film 100.
[0135] Furthermore, the thickness of the adhesive layer 40 is in the range of 10 μm to 16 μm, so that the adhesive layer 40 has a good adhesive force, and at the same time the protective film 100 is kept at a high hardness, thereby improving the anti-nail mark effect of the protective film 100.
[0136] The protective film 100 of the embodiment of the present application can be prepared by the method described in the following embodiments of the present application. In addition, it can also be prepared by other methods. The preparation method of the embodiment of the present application is only one or more preparation methods of the protective film 100 of the present application and should not be understood as a limitation on the protective film 100 provided by the embodiment of the present application.
[0137] Figure 4 1 is a schematic diagram of a process for preparing a protective film 100 according to an embodiment of the present application.
[0138] See also Figure 4 The present application also provides a method for preparing a protective film 100, which includes:
[0139] S201, providing a substrate layer 10;
[0140] S202, forming a hardening layer 20 on one side of the substrate layer 10, wherein the hardening layer 20 comprises a polyurethane acrylate prepolymer and a hyperbranched acrylic resin, wherein the mass ratio of the polyurethane acrylate prepolymer to the hyperbranched acrylic resin in the hardening layer 20 is in a range of 1 to 4; and
[0141] S203 , forming a shaping layer 30 on a side of the base material layer 10 away from the hardening layer 20 .
[0142] For detailed description of other aspects such as the substrate layer 10, the hardening layer 20, the shaping layer 30, the polyurethane acrylate prepolymer and the hyperbranched acrylic resin, please refer to the description of the corresponding part of the above embodiment, which will not be repeated here.
[0143] The protective film 100 prepared by the preparation method of the protective film 100 of the embodiment of the present application includes a substrate layer 10, a hardening layer 20 and a shaping layer 30 which are stacked in sequence, and the hardening layer 20 includes a polyurethane acrylate resin and a hyperbranched acrylic resin. In the hardening layer 20, the mass ratio of the polyurethane acrylate resin to the hyperbranched acrylic resin is in the range of 1 to 4. The polyurethane acrylate is the main molecular structure, providing the main mechanical properties and molecular chain structure, and the hyperbranched acrylic resin plays a toughening and strengthening role. Through the coordination of the polyurethane acrylate resin and the hyperbranched acrylic resin, the hardening layer 20 has higher hardness and rigidity, higher wear resistance and scratch resistance, and better toughness. When applied to a curved screen, it can be better bent and is not prone to cracking. In addition, the hyperbranched acrylic resin has the characteristics of good fluidity, low viscosity, not easy to crystallize, good film-forming properties, etc., and has good solubility and good weather resistance. The application of hyperbranched acrylic resin in the polyurethane acrylate resin system can effectively increase the double bond content of the system, thereby effectively improving the rate of light curing (such as UV curing) and the mechanical properties of the hardened layer 20; furthermore, at the same solid content, the hyperbranched acrylic resin can significantly reduce the viscosity of the system, which is beneficial to the construction of the hardened layer 20 and saves energy. Furthermore, the hyperbranched acrylic resin has more side chains, which can better form a cross-linked network structure in the hardened layer 20, increase the cross-linking degree of the hardened layer 20, and make the hardened layer 20 have better toughness and wear resistance.
[0144] In some embodiments, in S201, providing the substrate layer 10 includes:
[0145] (1) providing a glue solution composed of raw material components of an optical-grade process film and a substrate layer 10;
[0146] Optionally, the adhesive may be, but is not limited to, an adhesive composed of raw material components of thermoplastic polyurethane (eg, a mixture of polyols such as polyether or polyester and diisocyanate), an adhesive composed of raw material components of silicone rubber, etc.
[0147] Optionally, the glue may be, but is not limited to, a thermal-optical dual-curing glue, or a thermal-curing glue.
[0148] (2) coating the adhesive on the surface of the optical-grade process film to form an adhesive layer;
[0149] (3) baking at a temperature of 80° C. to 150° C.; and
[0150] Specifically, the temperature for baking the glue layer may be, but is not limited to, 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, etc.
[0151] Optionally, the glue layer is baked for 2 minutes (min) to 5 minutes. Specifically, the baking time can be, but is not limited to, 2 minutes, 3 minutes, 4 minutes, 5 minutes, etc.
[0152] (4) The glue layer is cured to form the substrate layer 10, thereby obtaining the optical-grade process film and the substrate layer 10 stacked thereon.
[0153] Optionally, the glue layer is irradiated under an electron beam curing or ultraviolet light curing device (such as a mercury lamp or an LED lamp) for 5 seconds (s) to 15 seconds to obtain the substrate layer 10 .
[0154] In this embodiment, for detailed description of other aspects of the substrate layer 10, please refer to the description of the corresponding parts of the above embodiment, which will not be repeated here.
[0155] In this embodiment, an optical-grade process film is used as a substrate to prepare the base material layer 10. The optical-grade process film has good flatness, which can make the prepared base material layer 10 smoother and less prone to orange peel, wrinkles, etc.
[0156] In some embodiments, in S202, the hardening layer 20 is formed on one side of the substrate layer 10, including: coating a hardening liquid (i.e., a glue liquid composed of raw material components of the hardening layer 20) on the surface of the substrate layer 10 away from the optical-grade process film, baking at a temperature of 80°C to 150°C to remove the first solvent in the hardening liquid to form a hardening liquid layer; and performing photocuring to cure the hardening liquid layer to form the hardening layer 20, thereby obtaining an optical-grade process film, a substrate layer 10, and a hardening layer 20 stacked in sequence.
[0157] Specifically, the baking temperature may be, but is not limited to, 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, etc. If the temperature is too low, the first solvent is not completely removed and the hardened liquid layer is not baked dry; if the temperature is too low, the first solvent in the hardening liquid evaporates too quickly, and the hardened layer 20 formed is prone to have pores, which reduces the mechanical properties and hardness of the hardened layer 20.
[0158] Optionally, the baking time is 2 minutes (min) to 5 minutes. Specifically, the baking time can be but is not limited to 2 minutes, 3 minutes, 4 minutes, 5 minutes, etc.
[0159] For detailed description of other aspects of the hardening liquid, please refer to the description of the corresponding parts of the above embodiments, which will not be repeated here.
[0160] Optionally, the hardening liquid layer is irradiated under an ultraviolet light curing device (such as a mercury lamp or an LED lamp) for 5 seconds (s) to 15 seconds to photo-cure the hardening liquid layer to form a hardened layer 20 .
[0161] Optionally, S202 further includes: removing the optical-grade process film to obtain a laminated substrate layer 10 and a hardening layer 20 .
[0162] In some embodiments, in S203, a fixing layer 30 is formed on the side of the substrate layer 10 away from the hardening layer 20, including: applying a fixing liquid on the surface of the substrate layer 10 away from the hardening layer 20 to form a fixing liquid glue layer; and baking the fixing liquid glue layer at a high temperature of 80°C to 150°C for 2min to 5min to thermally cure the fixing liquid glue layer to form the fixing layer 30.
[0163] Specifically, the temperature of thermal curing of the setting liquid glue layer can be, but is not limited to, 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, etc. If the temperature of thermal curing of the setting liquid glue layer is too low, the setting liquid glue layer is prone to incomplete reaction, and even the solvent is not completely volatilized, which reduces the mechanical properties of the setting layer 30 before light curing, and affects the subsequent coating of the adhesive layer 40; in addition, the thermal curing of the setting layer 30 is incomplete. When the protective film 100 is attached to the curved screen, the setting layer 30 will further undergo thermal curing over time, generating a large shrinkage stress, thereby making the protective film 100 prone to warping. If the temperature of thermal curing of the setting liquid glue layer is too high, the reaction speed of the setting liquid glue layer is too fast, and air is easily trapped and bubbles are generated; in addition, the degree of thermal curing reaction is too high, so that the hardness of the setting layer 30 is too high before being attached to the curved screen, and the flexibility is low, which reduces the degree of adhesion between the protective film 100 and the curved screen.
[0164] Optionally, the thermal curing time of the setting liquid glue layer can be, but is not limited to, 2 minutes, 3 minutes, 4 minutes, 5 minutes, etc.
[0165] Figure 5 It is a schematic flow chart of a method for preparing a protective film 100 according to another embodiment of the present application.
[0166] See also Figure 5 The present application also provides a method for preparing a protective film 100, which includes:
[0167] S301, providing a substrate layer 10;
[0168] S302, forming a hardening layer 20 on one side of the substrate layer 10, wherein the hardening layer 20 comprises a polyurethane acrylate prepolymer and a hyperbranched acrylic resin, wherein the mass ratio of the polyurethane acrylate prepolymer to the hyperbranched acrylic resin in the hardening layer 20 is in a range of 1 to 4; and
[0169] S303 , forming a shaping layer 30 on a side of the base material layer 10 away from the hardening layer 20 .
[0170] For a detailed description of S301 to S303 , please refer to the description of the corresponding parts of the above embodiment, which will not be repeated here.
[0171] S304, forming an adhesive layer 40 on the surface of the shaping layer 30 facing away from the substrate.
[0172] Optionally, an adhesive is coated on the surface of the shaping layer 30 facing away from the substrate, and baked at a temperature of 120° C. to 150° C. for 1 min to 5 min to cure the adhesive to form the adhesive layer 40 .
[0173] Optionally, the curing temperature of the adhesive may be, but is not limited to, 120° C., 130° C., 140° C., 150° C., etc. If the curing temperature of the adhesive is too low, the adhesive reaction is incomplete, which reduces the adhesiveness of the adhesive; if the curing temperature of the adhesive is too high, the adhesive reaction speed is too fast, bubbles are easily generated, and the formed adhesive layer 40 is uneven.
[0174] Figure 6 It is a schematic structural diagram of a curved screen assembly 200 according to an embodiment of the present application. Figure 7 It is a schematic diagram of the exploded structure of the curved screen assembly 200 according to an embodiment of the present application. Figure 8 It is a schematic side view of the curved screen assembly 200 according to an embodiment of the present application.
[0175] See also Figures 6 to 8 The embodiment of the present application also provides a curved screen assembly 200, which includes: a curved screen 210 and the protective film 100 described in the embodiment of the present application. The curved screen 210 has a display surface 211; the protective film 100 is disposed on the display surface 211, and the shaping layer 30 is between the substrate layer 10 and the curved screen 210.
[0176] For a detailed description of the protective film 100 , please refer to the description of the corresponding part of the above embodiment, which will not be repeated here.
[0177] It can be understood that the shaping layer 30 is closer to the curved screen 210 than the substrate layer 10. The protective film 100 is bonded to the curved screen 210 via the adhesive layer 40.
[0178] It can be understood that in the present embodiment, the protective film 100 is a 3D protective film 100 , and the shaping layer 30 of the protective film 100 is a shaping layer 30 that has been thermally cured and photocured.
[0179] It can be understood that after the protective film 100 is prepared and before being attached to the curved screen 210, the protective film 100 is a flat structure. When the protective film 100 is applied to the curved screen assembly 200 and attached to the curved screen 210, the adhesive layer 40 of the protective film 100 is adhered to the display surface 211 of the curved screen 210, and the protective film 100 is pressed so that the protective film 100 is completely attached to the curved screen 210; then the protective film 100 is illuminated to further photo-cure the shaping layer 30 of the protective film 100, thereby shaping the protective film 100 to form a 3D protective film 100, so that the protective film 100 matches the shape of the curved screen 210 and is tightly attached to the surface of the curved screen 210.
[0180] Optionally, the curved screen 210 may be curved on two relatively long sides, or on two relatively short sides, or on all four sides. The drawings of the present application are only one of the various forms of the curved screen 210, and should not be construed as limiting the curved screen 210 of the embodiment of the present application, nor should they be construed as limiting the protective film 100 of the present application.
[0181] Optionally, the energy range of the light curing of the shaping layer 30 is 6000 mj / cm 2 Up to 12000mj / cm 2 Specifically, the energy of the light curing of the shaping layer 30 may be, but is not limited to, 6000 mj / cm 2 、7000mj / cm 2 、8000mj / cm 2 、9000mj / cm 2 、10000mj / cm 2 、11000mj / cm 2 、12000mj / cm 2 In this embodiment, if the energy of the light curing of the shaping layer 30 is too low, the shaping layer 30 is not completely cured, the generated shaping force is insufficient, the shaping effect is affected, and the hardness of the shaping layer 30 is insufficient, which affects the anti-nail mark effect of the shaping layer 30; if the energy of the light curing of the shaping layer 30 is too high, the degree of curing of the shaping layer 30 is too high, and after curing, the volume shrinks too much, the internal stress is too large, and the force resisting the bonding force direction is too large, so that the protective film 100 is easy to warp.
[0182] Optionally, the curved screen 210 may be, but is not limited to, one or more of a liquid crystal display, a light emitting diode display (LED display), a micro light emitting diode display (Micro LED display), a sub-millimeter light emitting diode display (Mini LED display), an organic light emitting diode display (OLED display), etc.
[0183] The curved screen assembly 200 of the present application includes a curved screen 210 and a protective film 100. The protective film 100 includes a material layer, a hardening layer 20 and a shaping layer 30 which are stacked in sequence. The hardening layer 20 includes a polyurethane acrylate resin and a hyperbranched acrylic resin. In the hardening layer 20, the mass ratio of the polyurethane acrylate resin to the hyperbranched acrylic resin is in the range of 1 to 4. Polyurethane acrylate is the main molecular structure, providing the main mechanical properties and molecular chain structure, and the hyperbranched acrylic resin plays a toughening and strengthening role. Through the combination of polyurethane acrylate resin and hyperbranched acrylic resin, the hardening layer 20 has higher hardness and rigidity, higher wear resistance and scratch resistance, and better toughness. When applied to the curved screen 210, it can be bent better and is not prone to cracking. In addition, the hyperbranched acrylic resin has the characteristics of good fluidity, low viscosity, not easy to crystallize, good film-forming properties, etc., and has good solubility and good weather resistance. The application of hyperbranched acrylic resin in the polyurethane acrylate resin system can effectively increase the double bond content of the system, thereby effectively improving the rate of light curing (such as UV curing) and the mechanical properties of the hardened layer 20; furthermore, at the same solid content, the hyperbranched acrylic resin can significantly reduce the viscosity of the system, which is beneficial to the construction of the hardened layer 20 and saves energy. Furthermore, the hyperbranched acrylic resin has more side chains, which can better form a cross-linked network structure in the hardened layer 20, increase the cross-linking degree of the hardened layer 20, and make the hardened layer 20 have better toughness and wear resistance.
[0184] Fig. 9 It is a structural diagram of an electronic device 300 according to an embodiment of the present application. Fig.10 It is a schematic diagram of a partial exploded structure of an electronic device 300 according to an embodiment of the present application. Fig.11 FIG. 3 is a side view of an electronic device 300 according to an embodiment of the present application. Fig.12 It is a circuit block diagram of an electronic device 300 according to an embodiment of the present application.
[0185] See also Figures 9 to 12 The embodiment of the present application also provides an electronic device 300, which includes: the curved screen assembly 200 described in the embodiment of the present application and a processor 310, wherein the processor 310 is electrically connected to the curved screen assembly 200 and is used to control the curved screen assembly 200 to display.
[0186] For a detailed description of the curved screen assembly 200, please refer to the description of the corresponding part of the above embodiment, which will not be repeated here.
[0187] The electronic device 300 of the embodiment of the present application may be, but is not limited to, a mobile phone, a tablet computer, a laptop computer, a desktop computer, a smart bracelet, a smart watch, an e-reader, a game console, and other portable electronic devices 300. It can be understood that the electronic device 300 described in this embodiment is only one form of the electronic device 300 applied by the curved screen assembly 200, and should not be understood as a limitation on the electronic device 300 provided in the present application, nor should it be understood as a limitation on the curved screen assembly 200 provided in each embodiment of the present application.
[0188] Optionally, the processor 310 includes one or more general-purpose processors, wherein the general-purpose processor can be any type of device capable of processing electronic instructions, including a central processing unit (CPU), a microprocessor, a microcontroller, a main processor, a controller, and an ASIC, etc. The processor 310 is used to execute various types of digital storage instructions, such as software or firmware programs stored in a memory, which enables the computing device to provide a wide variety of services.
[0189] Optionally, the electronic device 300 of the present application further includes a memory 320. The memory 320 is electrically connected to the processor 310 and is used to store program codes required for the processor 310 to run, program codes required for controlling the curved screen assembly 200, display content of the curved screen 210, and the like.
[0190] Optionally, the memory 320 may include a volatile memory (Volatile Memory), such as a random access memory (Random Access Memory, RAM); the memory 320 may also include a non-volatile memory (NVM), such as a read-only memory (Read-Only Memory, ROM), a flash memory (Flash Memory, FM), a hard disk drive (Hard Disk Drive, HDD) or a solid-state drive (SSD). The memory 320 may also include a combination of the above-mentioned types of memory.
[0191] In some embodiments, the electronic device 300 of the embodiment of the present application further includes a housing 330, a middle frame 340 and a camera module 350, wherein the housing 330 is disposed opposite to the curved screen assembly 200, the middle frame 340 is disposed between the curved screen assembly 200 and the housing 330, and the side of the middle frame 340 is exposed to the housing 330 and the curved screen assembly 200. The middle frame 340 and the housing 330 enclose a housing space (not shown), and the housing space is used to accommodate the processor 310, the memory 320 and the camera module 350. The camera module 350 is electrically connected to the processor 310 for shooting under the control of the processor 310.
[0192] Optionally, the housing 330 has a light-transmitting portion (not shown), and the camera module 350 can shoot through the light-transmitting portion on the housing 330, that is, the camera module 350 in this embodiment is a rear camera module 350. It can be understood that in other embodiments, the light-transmitting portion can be provided on the curved screen assembly 200, that is, the camera module 350 is a front camera module 350. In the schematic diagram of this embodiment, the light-transmitting portion is illustrated as an opening. In other embodiments, the light-transmitting portion may not be an opening, but a light-transmitting material, such as plastic, glass, etc.
[0193] The protective film 100 of the embodiment of the present application is further described below through specific examples.
[0194] Example 1
[0195] The protective film 100 of this embodiment is prepared by the following steps:
[0196] (1) Preparing the substrate layer 10: coating the polyurethane adhesive on the surface of the optical-grade process film, baking at 100° C. for 3 minutes, and irradiating the film under an electron beam curing device for 10 seconds to obtain the thermoplastic polyurethane substrate layer 10;
[0197] The thickness of the substrate layer 10 is 20 μm; the elastic modulus of the substrate layer 10 is 2 GPa, the tensile strength of the substrate layer 10 is 50 MPa, and the elongation at break of the substrate layer 10 is 2%.
[0198] (2) coating the surface of the substrate layer 10 with a hardening liquid, and baking at a temperature of 120° C. for 3 minutes to dry out the solvent; then irradiating the surface with a UV curing device for 10 seconds to cure the hardening liquid to form a hardened layer 20;
[0199] The thickness of the hardened layer 20 is 3 μm; the hardening liquid includes, by mass fraction, 20% of a polyurethane acrylic resin prepolymer, 10% of a hyperbranched acrylic resin (with an octagonal ring in the middle, i.e., the acrylic resin molecule includes eight branches), 5% of ethoxylated trimethylolpropane triacrylate (a first reaction monomer), 3% of methyl benzoylformate (a first photoinitiator), 5% of a double-bond terminated perfluoropolyether (a short-chain fluoride) with a weight average molecular weight of 3000, 5% of an aluminum oxide (inorganic nanoparticle) with an average particle size of 20 nm, and 52% of propylene glycol methyl ether (a first solvent);
[0200] (3) removing the optical-grade process film, applying a setting liquid on the surface of the substrate layer 10 away from the hardening layer 20, and baking at a temperature of 120° C. for 3 minutes to perform thermal curing to form a setting layer 30; and
[0201] The thickness of the setting layer 30 is 75 μm; the setting liquid comprises a first raw material component and a second raw material component, and the mass ratio of the first raw material component to the second raw material component is 5; the first raw material component comprises 50% of a polyurethane acrylate prepolymer with a weight average molecular weight of 10,000, 15% of diphenylmethane diisocyanate (a second reactive monomer), 5% of succinic anhydride (a curing agent), 3% of a photoinitiator 184, 0.5% of 2-chloroethylmethyldimethoxysilane (a first coupling agent), and 26.5% of ethyl acetate (a second solvent); the second raw material component comprises 50% of hydroxyethyl methacrylate (an acrylic monomer), 0.5% of 3-isocyanatepropyltrimethoxysilane (a second coupling agent), 3% of poly(melamine-co-formaldehyde) methanol (a film-forming agent), and 46.5% of methylal (a third solvent);
[0202] (4) coating a silicone adhesive on the surface of the shaping layer 30 facing away from the substrate layer 10, and baking at a high temperature of 150° C. for 2 minutes to form an adhesive layer 40;
[0203] The thickness of the adhesive layer 40 is 10 μm.
[0204] Example 2
[0205] The protective film 100 of this embodiment is different from that of the embodiment 1 in that: the thickness of the base material layer 10 is 25 μm, the thickness of the hardening layer 20 is 3 μm; the thickness of the shaping layer 30 is 80 μm; and the thickness of the adhesive layer 40 is 12 μm.
[0206] Example 3
[0207] The protective film 100 of this embodiment is different from that of the embodiment 1 in that: the thickness of the base material layer 10 is 30 μm, the thickness of the hardening layer 20 is 3 μm; the thickness of the shaping layer 30 is 100 μm; and the thickness of the adhesive layer 40 is 15 μm.
[0208] Example 4
[0209] The protective film 100 of this embodiment is different from that of the embodiment 1 in that: the thickness of the base material layer 10 is 30 μm, the thickness of the hardening layer 20 is 3 μm; the thickness of the shaping layer 30 is 120 μm; and the thickness of the adhesive layer 40 is 20 μm.
[0210] The protective film 100 prepared in each embodiment is attached to the display surface 211 of the curved screen 210 or the curved screen 210 of the electronic device 300, and the adhesive layer 40 is located between the curved screen 210 and the hardening layer 20; ultraviolet light is irradiated to make the shaping layer 30 photocured, and the protective film 100 is shaped into a 3D structure, wherein the energy of the photocuring of the shaping layer 30 is 10000 mj / cm 2 According to the test, after the shaping layer 30 is thermally cured and light-cured, the peeling force of the adhesive layer 40 on the curved screen 210 with a water drop angle of 115° is 30 gf / 25 mm.
[0211] The test method of the peeling force of the adhesive layer 40 on the curved screen 210 with a water drop angle of 115° is as follows: 1) the sample to be tested (protective film 200) is made into specifications: 25 mm in width and the length is the length of the sample body to be tested, and is pasted on the test steel plate & test anti-fingerprint screen (abbreviated as AF screen, the AF screen used for testing requires a water drop angle ≥ 115°), ensuring that one end is aligned and parallel to the steel plate / AF screen; 2) A 2Kg weight is used to roll the sample to be tested back and forth three times at a speed of about 120mm / s under its own weight, and placed at room temperature for 20 minutes; 3) The free end of the sample to be tested is folded back 180°, and the adhesive surface is peeled off by about 20mm. The sample to be tested is clamped on the lower clamp, and the free end is extended (if the length of the sample to be tested is not enough, TESA 7475 tape can be used as the extension end) and is adhered to the metal straightening plate and clamped on the upper clamp. The peeling surface should be kept consistent with the force line of the testing machine; 4) Select a 5KG range sensor and set the experimental parameters: peeling speed 300mm / min; 5) Click to execute the test to obtain the peeling curve.
[0212] The curved screen 210 with the protective film 100 is subjected to various performance tests:
[0213] (1) Abrasion resistance test: Use 0000# steel wool with a weight of 1 kg to rub the exterior surface of the protective film 100 (i.e., the surface of the hardened layer 20) back and forth. After rubbing back and forth 5000 times, measure the water drop angle of the surface of the protective film 100.
[0214] (2) Pencil hardness test: GB / T 6739-2006 was used to measure the hardness of a 500g pencil.
[0215] (3) High temperature 50°C test: The protective film 100 is bonded to a curved screen mobile phone with an anti-fingerprint layer using the above-mentioned screen bonding method; after bonding, the curved screen mobile phone with the protective film 100 is placed in a constant temperature and humidity environment at 50°C, taken out after 24 hours, and inspected after returning to normal temperature for 1 hour.
[0216] (4) Low temperature test at -15°C: The protective film 100 is bonded to a curved screen mobile phone with an anti-fingerprint layer using the above-mentioned screen bonding method. After bonding, the curved screen mobile phone with the protective film 100 is placed in a constant temperature and humidity environment at -15°C for 24 hours and then taken out and inspected after returning to normal temperature for 1 hour.
[0217] The test results of Examples 1 to 4 are shown in Table 1 below:
[0218] Table 1 Performance parameters of the protective film 100 of Examples 1 to 4 attached to the curved screen 210
[0219]
[0220] It can be seen from the test results in Table 1 that when the protective film 100 of the embodiment of the present application is applied to the curved screen assembly 200 or the electronic device 300, it can fit the curved screen 210 well, has a good fit to the curved screen 210, is not prone to rebound and warping, and has good high and low temperature performance.
[0221] It can be seen from the test results of Examples 1 to 4 that the protective film 100 of the embodiments of the present application has higher hardness and better wear resistance, and the water drop angle after being rubbed with steel wool 5000 times is greater than or equal to 102°.
[0222] In addition, the thicker the substrate layer 10 and the shaping layer 30 are, the higher the hardness of the protective film 100 is, and the thicker the adhesive layer 40 is, the lower the hardness of the protective film 100 is. Therefore, when the thickness of the hardening layer 20 remains unchanged, as the thickness of the substrate layer 10 and the shaping layer 30 increases, the wear resistance of the protective film 100 will also increase, and the hardness of the protective film 100 will increase. However, as the thickness of the adhesive layer 40 increases, the hardness of the protective film 100 will decrease, and the wear resistance of the protective film 100 will also decrease.
[0223] Example 5
[0224] The difference between this embodiment and embodiment 1 is that the hardening liquid of this embodiment includes, by mass fraction, 15% of polyurethane acrylic resin prepolymer, 15% of hyperbranched acrylic resin, 5% of ethoxylated trimethylolpropane triacrylate (first reaction monomer), 3% of methyl benzoylformate (photoinitiator), 5% of double-bond terminated perfluoropolyether (short-chain fluoride) with a weight average molecular weight of 3000, 5% of aluminum oxide (inorganic nanoparticles) with an average particle size of 20 nm, and 52% of propylene glycol methyl ether (first solvent), wherein the mass ratio of the polyurethane acrylic resin to the hyperbranched acrylic resin in the hardening layer 20 is 1.
[0225] Example 6
[0226] The difference between this embodiment and embodiment 1 is that the hardening liquid of this embodiment includes, by mass fraction, 22.5% of polyurethane acrylic resin prepolymer, 7.5% of hyperbranched acrylic resin, 5% of ethoxylated trimethylolpropane triacrylate (first reaction monomer), 3% of methyl benzoylformate (photoinitiator), 5% of double-bond terminated perfluoropolyether (short-chain fluoride) with a weight average molecular weight of 3000, 5% of aluminum oxide (inorganic nanoparticles) with an average particle size of 20 nm, and 52% of propylene glycol methyl ether (first solvent), wherein the mass ratio of the polyurethane acrylic resin to the hyperbranched acrylic resin in the hardening layer 20 is 3.
[0227] Example 7
[0228] The difference between this embodiment and embodiment 1 is that the hardening liquid of this embodiment includes, by mass fraction, 24% of polyurethane acrylic resin prepolymer, 6% of hyperbranched acrylic resin, 5% of ethoxylated trimethylolpropane triacrylate (first reaction monomer), 3% of methyl benzoylformate (photoinitiator), 5% of double-bond terminated perfluoropolyether (short-chain fluoride) with a weight average molecular weight of 3000, 5% of aluminum oxide (inorganic nanoparticles) with an average particle size of 20 nm, and 52% of propylene glycol methyl ether (first solvent), wherein the mass ratio of the polyurethane acrylic resin to the hyperbranched acrylic resin in the hardening layer 20 is 4.
[0229] Example 8
[0230] The difference between this embodiment and embodiment 1 is that the setting liquid of this embodiment does not include the first coupling agent.
[0231] Example 9
[0232] The difference between this embodiment and embodiment 1 is that the setting liquid of this embodiment does not include a second coupling agent.
[0233] Example 10
[0234] The difference between this embodiment and embodiment 1 is that the setting liquid of this embodiment does not include the first coupling agent and the second coupling agent.
[0235] Embodiment 11
[0236] The difference between this embodiment and embodiment 1 is that the hardening liquid of this embodiment does not include perfluoropolyether.
[0237] Example 12
[0238] The difference between this embodiment and embodiment 1 is that the hardening liquid of this embodiment does not include inorganic nanoparticles.
[0239] Example 13
[0240] The difference between this embodiment and embodiment 1 is that the hardening liquid of this embodiment does not include perfluoropolyether and inorganic nanoparticles.
[0241] Comparative Example 1
[0242] The difference between this comparative example and Example 1 is that the hardening liquid of this example includes, by mass fraction, 10% of a polyurethane acrylic resin prepolymer, 20% of a hyperbranched acrylic resin, 5% of ethoxylated trimethylolpropane triacrylate (a first reaction monomer), 3% of methyl benzoylformate (a photoinitiator), 5% of a double-bond terminated perfluoropolyether (a short-chain fluoride) having a weight average molecular weight of 3000, 5% of an alumina having an average particle size of 20 nm (an inorganic nanoparticle), and 52% of propylene glycol methyl ether (a first solvent), wherein the mass ratio of the polyurethane acrylic resin to the hyperbranched acrylic resin in the hardening layer 20 is 0.5.
[0243] Comparative Example 2
[0244] The difference between this comparative example and Example 1 is that the hardening liquid of this example includes, by mass fraction, 36.25% of polyurethane acrylic resin prepolymer, 3.75% of hyperbranched acrylic resin, 5% of ethoxylated trimethylolpropane triacrylate (first reaction monomer), 3% of methyl benzoylformate (photoinitiator), 5% of double-bond terminated perfluoropolyether (short-chain fluoride) with a weight average molecular weight of 3000, 5% of aluminum oxide (inorganic nanoparticles) with an average particle size of 20 nm, and 52% of propylene glycol methyl ether (first solvent), wherein the mass ratio of the polyurethane acrylic resin to the hyperbranched acrylic resin in the hardening layer 20 is 7.
[0245] Comparative Example 3
[0246] The difference between this comparative example and Example 1 is that the hardening liquid of this example includes, by mass fraction, 36.25% of polyurethane acrylic resin prepolymer, 3.75% of acrylic resin, 5% of ethoxylated trimethylolpropane triacrylate (first reaction monomer), 3% of methyl benzoylformate (photoinitiator), 5% of double-bond terminated perfluoropolyether (short-chain fluoride) with a weight average molecular weight of 3000, 5% of aluminum oxide (inorganic nanoparticles) with an average particle size of 20 nm, and 52% of propylene glycol methyl ether (first solvent), wherein the mass ratio of the polyurethane acrylate resin to the acrylic resin in the hardening layer 20 is 2.
[0247] Various performance tests were performed on the protective films 100 of Examples 5 to 10 and Comparative Examples 1 to 3. The test results are shown in Table 2 below:
[0248] Table 2 Performance parameters of the protective film 100 of Example 1, Examples 5-10, and Comparative Examples 1-3 applied to the curved screen 210
[0249]
[0250] From the test results of Example 1, Example 5 to Example 7 in Table 1, it can be seen that as the mass ratio of the polyurethane acrylate resin to the hyperbranched acrylic resin in the hardening layer 20 increases, the water drop angle of the protective film 100 after being rubbed with steel wool 5000 times gradually increases, which indicates that the overall hardness of the protective film 100 gradually increases. In addition, when the protective film 100 is applied to the curved screen assembly 210 or the electronic device 300, it can be well attached to the curved screen 210, has a good fit to the curved screen 210, is not prone to rebound and warping, and has good high and low temperature performance.
[0251] It can be seen from the test results of Comparative Examples 1 and 2 that if the mass ratio of the polyurethane acrylate resin to the hyperbranched acrylic resin in the hardening layer 20 is too high or too low, the hardness of the protective film 100 will decrease, the wear resistance will decrease, and the water drop angle will decrease after being rubbed with steel wool 5000 times.
[0252] It can be seen from the test results of Example 1 and Comparative Example 3 that when the hyperbranched acrylic resin in the hardening layer 20 is replaced by ordinary acrylic resin, under the same other conditions, the hardness and wear resistance of the protective film 100 of Comparative Example 1 using ordinary acrylic resin are greatly reduced, and the water drop angle after being rubbed with steel wool 5000 times is greatly reduced and is less than 100°.
[0253] From the test results of Examples 1, 8 and 10, it can be seen that when the shaping layer 30 does not include one of the first coupling agent or the second coupling agent, the protective film 100 is more likely to produce gray edges after being attached to the curved screen 210, and the shaping effect is relatively poor. When the shaping layer 30 includes the first coupling agent and the second coupling agent, the protective film 100 has a better shaping effect, is less likely to produce gray edges when attached to the curved screen 210, has a better appearance effect and a longer service life.
[0254] It can be seen from the test results of Example 1 and Example 11 that when the hardening layer 20 does not include short-chain fluorides such as perfluoropolyether, the shaping effect of the protective film 100 is not affected, but the wear resistance of the protective film 100 is greatly reduced, and the water drop angle after rubbing with steel wool 5000 times is less than 100°.
[0255] It can be seen from the test results of Example 1 and Example 12 that when the hardening layer 20 does not include inorganic nanoparticles, the shaping effect of the protective film 100 is not affected, but the hardness and wear resistance of the protective film 100 are greatly reduced, and the water drop angle after rubbing with steel wool 5000 times is less than 100°.
[0256] It can be seen from the test results of Example 1 and Example 13 that when the hardening layer 20 does not include perfluoropolyether and inorganic nanoparticles, the shaping effect of the protective film 100 is not affected, but the hardness and wear resistance of the protective film 100 are greatly reduced, and the water drop angle after rubbing with steel wool 5000 times is less than 100°.
[0257] Mentioning "embodiment" and "implementation method" in this application means that the specific features, structures or characteristics described in conjunction with the embodiment may be included in at least one embodiment of the present application. The appearance of the phrases in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described in this application can be combined with other embodiments. In addition, it should also be understood that the features, structures or characteristics described in the various embodiments of the present application can be arbitrarily combined to form another embodiment that does not deviate from the spirit and scope of the technical solution of the present application, if there is no contradiction between them.
[0258] Finally, it should be noted that the above implementation modes are only used to illustrate the technical solution of the present application and are not intended to limit it. Although the present application has been described in detail with reference to the above preferred implementation modes, a person of ordinary skill in the art should understand that the technical solution of the present application may be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present application.
Claims
1. A protective film, characterized in that: include: substrate layer; A hardening layer, the hardening layer being disposed on one side of the substrate layer, the hardening layer comprising a polyurethane acrylate resin and a hyperbranched acrylic resin, wherein the mass ratio of the polyurethane acrylate resin to the hyperbranched acrylic resin in the hardening layer is in a range of 1 to 4; as well as A shaping layer is arranged on a side of the substrate layer away from the hardening layer.
2. The protective film according to claim 1, characterized in that: The number average molecular weight of the hyperbranched acrylic resin ranges from 5,000 to 20,000.
3. The protective film according to claim 1, characterized in that: The structural formula of the hyperbranched acrylic resin is: Herein, m is an integer from 1 to 14, and n is an integer from 50 to 200.
4. The protective film according to claim 1, characterized in that: The hardening layer further comprises short-chain fluorides. In the hardening layer, the mass fraction of the short-chain fluorides is in a range of 5% to 15%.
5. The protective film according to claim 1, characterized in that: The hardening layer further comprises inorganic nanoparticles. In the hardening layer, the mass fraction of the inorganic nanoparticles is in a range of 5% to 20%.
6. The protective film according to claim 1, characterized in that: The raw material components of the hardening layer include, by mass fraction: 20% to 50% of polyurethane acrylate prepolymer, 10% to 30% of hyperbranched acrylic resin, 3% to 10% of short-chain fluoride, 1% to 10% of inorganic nanoparticles, 5% to 20% of first reaction monomer, 0.5% to 2% of first photoinitiator and the remainder of first solvent.
7. The protective film according to claim 1, characterized in that: The raw material components of the shaping layer include a first raw material component and a second raw material component, the first raw material component includes a first resin and a first coupling agent, the second raw material component includes a second resin and a second coupling agent, the first resin includes a polyurethane acrylate prepolymer, the second resin includes an acrylic monomer, one of the first coupling agent and the second coupling agent is a silane coupling agent, and the other is a silane coupling agent with a thermally reactive group.
8. The protective film according to claim 7, characterized in that: The first raw material component comprises, by mass fraction, 20% to 70% of a polyurethane acrylate prepolymer, 0.1% to 1% of a first coupling agent, 15% to 30% of a second reactive monomer, 5% to 30% of a curing agent, 0.5% to 3% of a second photoinitiator, and the remainder a second solvent; the second raw material component comprises, by mass fraction, 40% to 80% of an acrylic monomer, 0.1% to 1% of a second coupling agent, 1% to 5% of a film-forming agent, and the remainder a third solvent.
9. The protective film according to claim 7, characterized in that: In the raw material components of the shaping layer, the mass ratio of the first raw material component to the second raw material component is in a range of 3 to 8.
10. The protective film according to claim 1, characterized in that: The substrate layer is isotropic and includes at least one of thermoplastic polyurethane and silicone rubber.
11. The protective film according to claim 1, characterized in that: The elastic modulus of the substrate layer ranges from 1.5 GPa to 4 GPa; the tensile strength of the substrate layer ranges from 40 MPa to 100 MPa; and the elongation at break of the substrate layer ranges from 1% to 5%.
12. The protective film according to any one of claims 1 to 11, characterized in that: The protective film is applied to the curved screen, the shaping layer is a heat-light dual-curing shaping layer, before the protective film is applied to the curved screen, the shaping layer is thermally cured, when the protective film is applied to the curved screen, the shaping layer is light-cured, and the light-curing energy of the shaping layer is in the range of 6000mj / cm 2 Up to 12000mj / cm 2 .
13. The protective film according to claim 12, characterized in that: The curing degree of the shaping layer by thermal curing ranges from 80% to 95%; the curing degree of the shaping layer by light curing ranges from 70% to 90%.
14. The protective film according to claim 12, characterized in that: The protective film also includes an adhesive layer, which is arranged on the surface of the shaping layer away from the substrate layer. After the shaping layer is thermally cured and before light cured, the peeling force of the adhesive layer on the surface with a water drop angle of 115° ranges from 40gf / 25mm to 100gf / 25mm; after the shaping layer is thermally and lightly dual-cured, the peeling force of the adhesive layer on the surface with a water drop angle of 115° ranges from 10gf / 25mm to 40gf / 25mm.
15. A method for preparing a protective film, characterized in that: include: providing a substrate layer; forming a hardening layer on one side of the substrate layer, wherein the hardening layer comprises a polyurethane acrylate prepolymer and a hyperbranched acrylic resin, wherein the mass ratio of the polyurethane acrylate prepolymer to the hyperbranched acrylic resin in the hardening layer is in a range of 1 to 4; as well as A shaping layer is formed on a side of the substrate layer facing away from the hardening layer.
16. A curved screen assembly, characterized in that: include: A curved screen, wherein the curved screen has a display surface; as well as The protective film according to any one of claims 1 to 14 is arranged on the display surface, between the shaping layer, the substrate layer and the curved screen.
17. An electronic device, characterized in that: include: The curved screen assembly according to claim 16; as well as A processor is electrically connected to the curved screen assembly and is used to control the curved screen assembly to display.
Citation Information
Cited By
Ultrahigh-water-drop-angle 9H curved-surface protective film capable of being bent and shaped and production process
CN120382702A