Reliable underfill adhesive and preparation method thereof

By combining and combining bisphenol epoxy resin with polyphenol epoxy resin, the bottom filler glue is formed to form a complex three-dimensional structure, which solves the thermal expansion mismatch of the bottom filler in high-frequency and high-temperature environments, and improves the heat cycling performance and Reliability reduces solder joint fatigue damage.

CN118879255APending Publication Date: 2024-11-01QINGDAO DEJU BONDING TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410960535.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The existing underfill glue is in a high frequency and high temperature difference environment, resulting in mismatch of thermal expansion coefficients between chips, substrates, and solder joints, resulting in thermal stress and fatigue damage to solder joints, poor thermal cycle resistance and low reliability.

Method used

Binding bisphenol epoxy resin and polyphenol epoxy resin, forming a complex three-dimensional mesh structure, improving heat resistance, and absorbing and eliminating thermal stress through the flexibility of polyphenol epoxy resin, combined with aromatic amine curing agent The amino silicone oil and end are adjusted to adjust the viscosity and crosslink density to prepare a bottom filler with excellent heat cycling resistance.

Benefits of technology

It significantly improves the heat cycling resistance and reliability of the bottom filler, reduces the occurrence and expansion of thermal fatigue cracks in the welding joints, enhances mechanical strength and adhesion, and maintains stable performance in the high temperature range.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004950132950000051
    Figure BDA0004950132950000051
Patent Text Reader

Abstract

The invention provides a reliable underfill adhesive and a preparation method thereof, the reliable underfill adhesive comprises the following raw materials by weight: 20-30 parts of epoxy resin, 15-20 parts of a curing agent, 50-70 parts of a filler and 3-5 parts of a diluent, the epoxy resin is a compound of bisphenol epoxy resin and polyphenol epoxy resin according to a mass ratio of 10: 1-2, the polyphenol epoxy resin is prepared from poly (4-vinylphenol) and epoxy chloropropane through a reaction, and the dosage of the epoxy chloropropane is 50-100 wt% of that of the poly (4-vinylphenol); the curing agent comprises an aromatic amine curing agent and amino-terminated silicon oil. The side group of the polyphenol epoxy resin contains an epoxy group, so that a more complex three-dimensional network structure can be formed when the underfill adhesive is cured, the heat resistance of the underfill adhesive is improved, and meanwhile, the main chain of the polyphenol epoxy resin has certain flexibility, so that the underfill adhesive can be flexibly adjusted when thermal stress exists, and the heat resistance of the underfill adhesive is improved. The thermal stress is internally absorbed and eliminated, and the heat-resistant cycle performance is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of bottom filling glue, and specifically relates to a reliable bottom filling glue and a preparation method thereof Background Art

[0002] Flip chip is a hot topic in the field of semiconductor packaging today. It is not only a chip interconnection technology, but also an ideal chip bonding technology. Traditional packaging technology is to place the chip with the active area facing up and the back facing the substrate before bonding (such as wire bonding and tape automated bonding TAB). Flip chip is to place the chip active area facing the substrate, and the chip and substrate are interconnected through solder bumps arranged in an array on the chip. This packaging method eliminates the requirement for wire bonding connection; increases the connection density of input / output (I / O); and uses very little space on the printed circuit board. Compared with wire bonding, it achieves a larger number of I / Os and speeds up the operation.

[0003] In order to meet the reliability requirements, an epoxy-based bottom filler with good bonding performance is generally added between the flip chip and the substrate to tighten it, reduce and redistribute stress, reduce crack damage caused by processes such as reflow soldering, and minimize the mismatch of thermal expansion coefficients between the chip, substrate, and solder joints. For example, the bottom filler disclosed in patent CN105462531B, its preparation method, and flip chip include the following components in mass percentage: filler 60-85%, epoxy resin 5-30%, cyanate 5-30%, accelerator 0.05-1.0%, toughening agent 1-10%, diluent 1-10%, dispersant 0.1-3%, defoamer 0.05%-1%, coupling agent 0.1-1%, pigment 0.1-0.5%. Patent CN113403013B discloses a bottom filling glue for semiconductor packaging and a semiconductor packaging structure for flip-chip chip, comprising 13-20wt% epoxy resin, 60-65wt% filler, 10.8-16wt% curing agent, 5-15wt% toughening agent and 0.5-0.8wt% accelerator, wherein the toughening agent is selected from methyl methacrylate-butadiene-styrene terpolymer.

[0004] However, with the rapid development of semiconductor integrated circuit technology, chip stacking technology has evolved from 2D and 2.5D to 3D high-density integration, with local power density reaching 100W / cm 2 As mentioned above, when electronic products are working, it is easy to generate a larger temperature difference in a short time, which is equivalent to electronic products working in a high-frequency and larger temperature difference environment, resulting in the mismatch of thermal expansion coefficients between chips, substrates, and solder joints. Thermal stress is easy to be generated in the solder joints, and the stress changes with the periodic temperature, causing fatigue damage to the solder joints. Therefore, it is necessary to develop a bottom filler with excellent heat cycle resistance and higher reliability. Summary of the invention

[0005] In order to solve the problems of poor heat cycle resistance and low reliability in the above-mentioned prior art, the present invention provides a reliable bottom filling glue and a preparation method thereof, wherein the epoxy resin in the bottom filling glue raw material is compounded by bisphenol epoxy resin and polyphenol epoxy resin, wherein the polyphenol epoxy resin is prepared by poly (4-vinylphenol) and epichlorohydrin as raw materials, and since the side groups of the polyphenol epoxy resin contain epoxy groups, a more complex three-dimensional network structure can be formed when the bottom filling glue is cured, thereby improving the heat resistance of the bottom filling glue, and at the same time, since the main chain of the polyphenol epoxy resin has a certain flexibility, when there is thermal stress, the bottom filling glue can be flexibly adjusted to absorb and eliminate thermal stress internally, thereby improving the heat cycle resistance.

[0006] A reliability bottom filling glue comprises the following raw materials in parts by weight: 20-30 parts of epoxy resin, 15-20 parts of curing agent, 50-70 parts of filler, and 3-5 parts of diluent, wherein the epoxy resin is a compound of bisphenol epoxy resin and polyphenol epoxy resin in a mass ratio of 10:1-2, the polyphenol epoxy resin is prepared by reacting poly(4-vinylphenol) and epichlorohydrin, and the amount of epichlorohydrin is 50-100wt% of the poly(4-vinylphenol); the curing agent comprises an aromatic amine curing agent and amino-terminated silicone oil.

[0007] Furthermore, the amount of epichlorohydrin used is 60-85% of the poly(4-vinylphenol).

[0008] The weight average molecular weight of the poly(4-vinylphenol) is 10,000-12,000 mol / g.

[0009] The epoxy value of the bisphenol epoxy resin is 0.40-0.55.

[0010] Furthermore, the bisphenol epoxy resin is selected from one or a combination of two or more of bisphenol A epoxy resin, bisphenol F epoxy resin, and bisphenol S epoxy resin.

[0011] The polyphenol epoxy resin is prepared by a method comprising the following steps:

[0012] Under an inert atmosphere, poly(4-vinylphenol) and epichlorohydrin are dissolved in an organic solvent, and alkali solution is added for pre-reaction. After the reaction is completed, alkali solution is added again and a ring-closing reaction is carried out under vacuum conditions. After the reaction is completed, a crude product is obtained by distillation. The crude product is dissolved in an organic solvent and then water is added until no precipitation is generated. The product is filtered, washed, and dried to obtain a polyphenol epoxy resin.

[0013] Furthermore, the organic solvent is selected from one or a combination of two or more of ethanol, isopropanol, ethyl acetate, acetone, methyl ethyl ketone, and methyl isobutyl ketone.

[0014] Furthermore, the concentration of the alkali solution in the pre-reaction is 30-50wt%, the alkali in the alkali solution is 0.5-1wt% of poly(4-vinylphenol), the temperature of the pre-reaction is 55-75°C, and the time is 1-5h.

[0015] Furthermore, the concentration of the alkali solution in the ring-closing reaction is 30-50wt%, the alkali in the alkali solution is 1.5-2wt% of poly(4-vinylphenol), the temperature of the ring-closing reaction is 55-75°C, the time is 5-8h, and the vacuum degree is 10-30kPa; the purpose of the distillation is to remove unreacted epichlorohydrin, organic solvent, and water; the solvent is selected from one or a combination of two or more of toluene, xylene, cyclohexanone, and cyclohexane; the alkali solution is selected from one or a combination of two of sodium hydroxide solution and potassium hydroxide solution. The washing is washing with water for 1-3 times.

[0016] The curing agent is a mixed curing agent composed of an aromatic amine curing agent and an amino-terminated silicone oil in a mass ratio of 5:0.3-0.45.

[0017] The epoxy resin of the present invention is a compound of a bisphenol epoxy resin and a polyphenol epoxy resin. By adjusting the compounding ratio, excellent heat-resistant cycle performance is obtained. Since the polyphenol epoxy resin is a substance with high polarity, it will make the viscosity of the bottom filling glue larger, so it is necessary to add a proper amount of amino silicone oil to adjust the viscosity of the bottom filling glue and improve the fluidity. However, the amount of the terminal amino silicone oil should not be too large, otherwise the cross-linking density of the bottom filling glue will be reduced. The amount should not be too small either, otherwise it will not improve the fluidity.

[0018] The amino-terminated silicone oil is a linear amino-terminated polydimethylsiloxane with an amine value of 0.6-1 mmol / g.

[0019] The aromatic amine curing agent is selected from one or a combination of two or more of diethyltoluenediamine, diaminodiphenylmethane, 3,-ethyl-4,4'-diaminodiphenylmethane, and 3,3'-diethyl-4,4'-diaminodiphenylmethane.

[0020] The filler is spherical silicon powder with a D50 of 0.1-1 μm.

[0021] The diluent is selected from one or a combination of monofunctional active diluents or bifunctional active diluents, specifically selected from one or a combination of two or more of n-butyl glycidyl ether, 2-ethylhexyl glycidyl ether, phenyl glycidyl ether, cresol glycidyl ether, diglycidyl ether, and butanediol diglycidyl ether.

[0022] The present invention also provides a method for preparing the above-mentioned reliability bottom filling glue, comprising the following steps:

[0023] Mix the epoxy resin and filler evenly, then add the diluent and mix evenly, and finally add the curing agent and mix evenly to obtain the reliability bottom filling glue.

[0024] The epoxy resin and filler are mixed evenly by three-roll grinding. The conditions for mixing evenly after adding the diluent are 20°C-30°C, vacuum degree 0.01-0.1MPa, rotation speed 300-800rpm, and mixing time 30-60min. The conditions for mixing evenly after adding the curing agent are 20°C-30°C, vacuum degree 0.01-0.1MPa, rotation speed 500-800rpm, and mixing time 1-3h.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] The epoxy resin in the raw material of the bottom filling glue of the present invention is compounded by bisphenol epoxy resin and polyphenol epoxy resin, wherein the polyphenol epoxy resin is prepared by poly (4-vinylphenol) and epichlorohydrin as raw materials. Since the side groups of the polyphenol epoxy resin contain epoxy groups, a more complex three-dimensional network structure can be formed when the bottom filling glue is cured, thereby improving the heat resistance of the bottom filling glue. Meanwhile, since the main chain of the polyphenol epoxy resin has certain flexibility, when there is thermal stress, the bottom filling glue can be flexibly adjusted to internally absorb and eliminate the thermal stress, thereby improving the heat resistance cycle performance. DETAILED DESCRIPTION

[0027] The present invention will be further described below in conjunction with specific embodiments, but is not limited to the contents of the specification. Unless otherwise specified, the "parts" described in the embodiments of the present invention are all parts by weight. The reagents used are all commercially available reagents in the art.

[0028] Amino-terminated silicone oil DY-N323, with an amine value of 0.9 mmol, was purchased from Shandong Dayi Chemical Co., Ltd.

[0029] Poly(4-vinylphenol) was purchased from Sigma-Aldrich with a weight average molecular weight of 12,000 mol / g. The phenolic hydroxyl content was measured by using Folin phenol and vanillin with an ultraviolet spectrophotometer (UV) to be 8 mmol / g.

[0030] Spherical silicon powder was purchased from Guangdong Nanhai Xinchuan Mining Co., Ltd., with a uranium content of 0.02 PPb and a D50 of 0.5 μm.

[0031] Bisphenol A epoxy resin E54 was purchased from Dow Chemical Company, and the epoxy value was 0.54.

[0032] Prepare the bottom filler:

[0033] Example 1

[0034] 1) Under a nitrogen atmosphere, 100 g of poly (4-vinyl phenol) and 85 g of epichlorohydrin are dissolved in 200 g of methyl isobutyl ketone to obtain a mixture, 2.5 g of a 40 wt % sodium hydroxide solution is added to the mixture to carry out a pre-reaction at 70° C. for 3 h, and 4 g of a 50 wt % sodium hydroxide solution is added to carry out a ring-closing reaction at 70° C. and a vacuum degree of 30 kPa for 6 h. After the reaction, unreacted epichlorohydrin, water and methyl isobutyl ketone are removed by distillation to obtain a crude product, the crude product is dissolved in toluene and then water is added until no precipitation is generated, filtered, washed with water 3 times, and dried at 100° C. to constant weight to obtain a polyphenol epoxy resin.

[0035] 2) 300 g of epoxy resin prepared by compounding E54 and the polyphenol epoxy resin in step 1) in a mass ratio of 10:2 and 700 g of spherical silicon powder were mixed evenly by three-roll grinding, and then 50 g of n-butyl glycidyl ether was added and mixed for 30 min at 20° C., a vacuum degree of 0.085 MPa, and a rotation speed of 300 rpm. Finally, 150 g of a mixed curing agent composed of diaminodiphenylmethane and terminal amino silicone oil DY-N323 in a mass ratio of 5:0.45 was added and mixed for 2.5 h at 20° C., a vacuum degree of 0.085 MPa, and a rotation speed of 600 rpm to obtain a reliability bottom filling glue.

[0036] Example 2

[0037] The rest is the same as Example 1, except that the amount of epichlorohydrin used in step 1) is 60 g.

[0038] Example 3

[0039] The rest is the same as Example 1, except that the amount of epichlorohydrin used in step 1) is 50 g.

[0040] Example 4

[0041] The rest is the same as Example 1, except that the amount of epichlorohydrin used in step 1) is 100 g.

[0042] Example 5

[0043] The rest is the same as Example 1, except that in step 2), the mixed curing agent is prepared by mixing diaminodiphenylmethane and amino-terminated silicone oil DY-N323 in a mass ratio of 5:0.3.

[0044] Example 6

[0045] The rest is the same as Example 1, except that the amount of the mixed curing agent in step 2) is 200 g.

[0046] Example 7

[0047] The rest is the same as Example 1, except that, in step 2), 300 g of epoxy resin is compounded by E54 and the polyphenol epoxy resin in step 1) at a mass ratio of 10:1.

[0048] Example 8

[0049] The rest is the same as Example 1, except that, in step 2), 200 g of epoxy resin prepared by compounding E54 and polyphenol epoxy resin in step 1) in a mass ratio of 10:1 and 500 g of spherical silicon powder are evenly mixed by three-roll grinding, and then 30 g of n-butyl glycidyl ether is added and mixed for 30 min at 20° C., a vacuum degree of 0.085 MPa, and a rotation speed of 300 rpm, and finally 200 g of a mixed curing agent composed of diaminodiphenylmethane and terminal amino silicone oil DY-N323 in a mass ratio of 5:0.3 is added and mixed for 2.5 h at 20° C., a vacuum degree of 0.085 MPa, and a rotation speed of 600 rpm to obtain a reliability bottom filling glue.

[0050] Comparative Example 1

[0051] The rest is the same as Example 1, except that the curing agent is all diaminodiphenylmethane.

[0052] Comparative Example 2

[0053] The rest is the same as Example 1, except that all epoxy resins are E54.

[0054] The bottom filling glue prepared in the above embodiment and comparative example was then subjected to the following performance tests:

[0055] Fluidity: simulate the packaged chip, use a 20mm×20mm×0.5mm transparent glass plate for the upper silicon chip, and a FR-4 substrate for the lower substrate. Use a feeler gauge to form a 30μm-high gap between the substrate and the glass plate. Use a fine steel needle to apply the bottom filling glue to be tested horizontally along one edge of the glass plate at 25°C. Start timing at the same time and record the time it takes for the bottom filling glue to be filled, in seconds.

[0056] Tg: After the bottom filler is cured at 150℃ for 30 minutes, the TMA is measured with a heating rate of 5℃ / min to confirm the glass transition temperature during heating from 30-300℃, in °C.

[0057] Shear strength: After the bottom filler is cured at 150°C for 30 minutes, the Al / Al shear strength is measured according to the ASTM D1002 test method, in MPa.

[0058] Heat cycle resistance: The temperature range of general consumer electronic products does not exceed 100°C, and the temperature requirements of industrial or automotive electronic products are higher, and the common temperature range is -55°C to 125°C or -65°C to 155°C. Using a high and low temperature rapid change test machine, the temperature range of the present invention is set to -65°C to 150°C, the number of cycles is 1000 times, the temperature change rate is 18°C / min, and it stays at -65°C and 150°C for 10 minutes, re-measures the above shear strength, calculates the shear strength loss rate, and visually inspects whether the bottom filling glue has collapse or cracks.

[0059] Table 1 Performance test results

[0060]

[0061] It can be seen from Table 1 that the bottom filling glue prepared by the present invention has excellent fluidity and heat cycle resistance, can reduce the initiation and expansion of thermal fatigue cracks in the solder joint, improve reliability, can overcome the problem of solder joint detachment or breakage in the thermal cycle test, has long-term usability, good adhesion and excellent mechanical strength.

[0062] The above detailed description is a specific description of one feasible embodiment of the present invention. The embodiment is not intended to limit the patent scope of the present invention. Any equivalent implementation or modification that does not deviate from the present invention should be included in the scope of the technical solution of the present invention.

Claims

1. A reliability bottom filling glue, characterized in that: The invention comprises the following raw materials in parts by weight: 20-30 parts of epoxy resin, 15-20 parts of curing agent, 50-70 parts of filler and 3-5 parts of diluent, wherein the epoxy resin is a compound of bisphenol epoxy resin and polyphenol epoxy resin in a mass ratio of 10:1-2, the polyphenol epoxy resin is prepared by reacting poly(4-vinylphenol) and epichlorohydrin, and the amount of epichlorohydrin is 50-100wt% of the poly(4-vinylphenol); and the curing agent comprises an aromatic amine curing agent and amino-terminated silicone oil.

2. The reliability bottom filling glue according to claim 1, characterized in that: The amount of epichlorohydrin used is 60-85% of poly(4-vinylphenol).

3. The reliability bottom filling glue according to claim 1, characterized in that: The weight average molecular weight of the poly(4-vinylphenol) is 10,000-12,000 mol / g; and the epoxy value of the bisphenol epoxy resin is 0.40-0.

55.

4. The reliability bottom filling glue according to claim 3, characterized in that: The bisphenol epoxy resin is selected from one or a combination of two or more of bisphenol A epoxy resin, bisphenol F epoxy resin and bisphenol S epoxy resin.

5. The reliability bottom filling glue according to claim 1, characterized in that: The polyphenol epoxy resin is prepared by a method comprising the following steps: Under an inert atmosphere, poly(4-vinylphenol) and epichlorohydrin are dissolved in an organic solvent, and alkali solution is added for pre-reaction. After the reaction is completed, alkali solution is added again and a ring-closing reaction is carried out under vacuum conditions. After the reaction is completed, a crude product is obtained by distillation. The crude product is dissolved in an organic solvent and then water is added until no precipitation is generated. The product is filtered, washed, and dried to obtain a polyphenol epoxy resin.

6. The reliability bottom filling glue according to claim 5, characterized in that: The concentration of the alkali solution in the pre-reaction is 30-50wt%, the alkali in the alkali solution is 0.5-1wt% of poly(4-vinylphenol), the temperature of the pre-reaction is 55-75°C, and the time is 1-5h.

7. The reliability bottom filling glue according to claim 5, characterized in that: The concentration of the alkali solution in the ring-closing reaction is 30-50wt%, the alkali in the alkali solution is 1.5-2wt% of poly(4-vinylphenol), the temperature of the ring-closing reaction is 55-75°C, the time is 5-8h, and the vacuum degree is 10-30kPa.

8. The reliability bottom filling glue according to claim 1, characterized in that: The curing agent is a mixed curing agent composed of an aromatic amine curing agent and an amino-terminated silicone oil in a mass ratio of 5:0.3-0.

45.

9. The reliability bottom filling glue according to claim 8, characterized in that: The amino-terminated silicone oil is a linear amino-terminated polydimethylsiloxane with an amine value of 0.6-1 mmol / g; the aromatic amine curing agent is selected from one or a combination of two or more of diethyltoluenediamine, diaminodiphenylmethane, 3,-ethyl-4,4'-diaminodiphenylmethane, and 3,3'-diethyl-4,4'-diaminodiphenylmethane.

10. The method for preparing the reliability bottom filling glue according to any one of claims 1 to 9, characterized in that: The steps include: Mix the epoxy resin and filler evenly, then add the diluent and mix evenly, and finally add the curing agent and mix evenly to obtain the reliability bottom filling glue.