Polyimide adhesive and preparation method thereof
By introducing polyimide adhesive with phosphoroxy group and ether bond structure in the polymerization reaction, the problems of failure and insufficient flame retardant performance of polyimide adhesives in the prior art under high temperature environment are solved, and high temperature stability and Improved flame retardancy, suitable for high-demand industrial applications.
Patent Information
- Application Number
- CN202411126337.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing polyimide adhesives fail in high temperature environments and lack flame retardant performance, making it difficult to meet the high requirements in the fields of aerospace, microelectronics and automobile industries.
Under the protection of an inert atmosphere, the polymerization reaction is carried out with a phosphoroxy group-containing aromatic diamine, an ether-bonded aromatic diamine and two aromatic dianhydride compositions, and the polyimide adhesive is prepared by heating and curing, and the phosphoroxy group is introduced and the Ether bond structure to improve flame retardancy and bonding properties.
The prepared polyimide adhesive has excellent high temperature resistance, flame retardant properties and adhesive properties, and can remain stable under high temperature environments, significantly improving its reliability in use under extreme conditions.
Smart Images

Figure CN118879271A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of adhesives, and in particular to a polyimide adhesive and a preparation method thereof. Background Art
[0002] Polyimide (PI) adhesives are a type of special adhesives made from polyimide polymer materials. Due to their excellent performance, they are widely used in many high-demand fields, such as aerospace, microelectronics, automotive industry, and high-temperature equipment manufacturing. In these fields, the use conditions of materials are often extremely harsh. For example, aerospace and satellite components need to withstand extreme temperature changes and radiation environments in space, the packaging of electronic components needs to withstand long-term high-temperature operation, and adhesives in the automotive industry must remain stable in the high-temperature environment of the engine compartment. In order to ensure the reliability of these applications, adhesive materials must maintain good structural integrity and bonding strength at high temperatures to prevent failure due to thermal aging or material decomposition. In addition, with the intensive and high-performance industrial and electronic equipment, higher requirements are placed on the flame retardant properties of adhesives to reduce fire risks and improve equipment safety. At the same time, polyimide adhesives also need to have good bonding properties, be able to firmly bond different materials, and maintain stable bonding effects under various environmental conditions (such as high humidity, high temperature, low temperature, etc.). Summary of the invention
[0003] The problem solved by the invention is: how to obtain a polyimide adhesive with better high temperature resistance, better flame retardancy and better bonding performance.
[0004] In order to solve the above problems, the present invention provides a method for preparing a polyimide adhesive, comprising:
[0005] Step S1, under the protection of an inert atmosphere, using a phosphorus-containing aromatic diamine, an ether-bonded aromatic diamine and an aromatic dianhydride composition as raw materials, to carry out a polymerization reaction in an aprotic solvent to obtain a polyamic acid solution; wherein the aromatic dianhydride composition is composed of two aromatic dianhydrides;
[0006] Step S2, removing the solvent from the polyamic acid solution, heating and curing the solution to obtain a polyimide adhesive.
[0007] Optionally, in step S1, the phosphorus-oxygen-containing aromatic diamine has a structural formula as shown in formula (1):
[0008]
[0009] Optionally, in step S1, the aromatic diamine containing an ether bond is selected from one of 2,2'-bis(trifluoromethyl)-4,4'-diaminophenyl ether, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 1,4-bis(4-aminophenoxy)benzene and 3,4'-diaminodiphenyl ether.
[0010] Optionally, in step S1, the aromatic dianhydride composition is selected from any two of 3,,3',4,4'-dibenzophenone tetracarboxylic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 2,3,3',4'-biphenyltetracarboxylic dianhydride, 4,4'-biphenyl ether dianhydride, 2,3,3',4'-diphenyl ether tetracarboxylic dianhydride and pyromellitic dianhydride.
[0011] Optionally, in step S1, the aromatic dianhydride composition is composed of two aromatic dianhydrides in a molar ratio of (1-2):(1-2), the molar ratio of the phosphorus-containing aromatic diamine to the ether-bonded aromatic diamine is (1-9):(1-9), and the ratio of the total molar number of the phosphorus-containing aromatic diamine and the ether-bonded aromatic diamine to the total molar number of the aromatic dianhydride composition is 1:1.
[0012] Optionally, in step S1, the solid content of the polyamic acid solution is 25-40%.
[0013] Optionally, in step S1, the polymerization reaction temperature is 20-25°C and the time is 24-28h.
[0014] Optionally, in step S2, the temperature rise curing includes: after removing the solvent from the polyamic acid solution, keeping the temperature at 80°C for 1-2 hours, heating to 120°C, keeping the temperature for 1-2 hours, heating to 150°C, keeping the temperature for 1-2 hours, heating to 180°C, keeping the temperature for 1-2 hours, heating to 210°C, keeping the temperature for 1-2 hours, heating to 240°C, keeping the temperature for 1-2 hours, heating to 280°C, and keeping the temperature for 1-2 hours.
[0015] Optionally, in step S1, the aprotic solvent includes one of N,N-dimethylacetamide, N-methylpyrrolidone and N-methylformamide.
[0016] The present invention also provides a polyimide adhesive, which is prepared by the above-mentioned preparation method of the polyimide adhesive.
[0017] Compared with the prior art, the present invention uses phosphorus-oxygen-containing aromatic diamine, ether-bonded aromatic diamine and two aromatic dianhydrides as raw materials, undergoes polymerization reaction and temperature-raising curing to obtain a polyimide adhesive; wherein the phosphorus-oxygen-containing aromatic diamine participates in the polymerization reaction, and the phosphorus-oxygen-containing is introduced into the molecular structure. Since the phosphorus-oxygen-containing has excellent flame retardant properties, the obtained polyimide adhesive has better flame retardancy; in addition, the phosphorus-containing large group introduced into the polyimide molecular chain by the phosphorus-oxygen-containing aromatic diamine destroys the flame retardant. The symmetry and regularity of the molecular chain are improved, which is beneficial to improving the high temperature resistance of the polyimide adhesive; the aromatic diamine containing ether bonds participates in the polymerization reaction, and the ether bonds are introduced into the molecular structure. Since the ether bonds belong to flexible groups, they can provide flexible molecular chains in the molecular structure of the polyimide adhesive, so that the activity of the polyimide in space is enhanced, which is more conducive to the casting and spreading on the surface of the substrate, and the bonding probability of the polar bonds in the polyimide adhesive and the substrate is increased, which is beneficial to improving the bonding performance of the polyimide adhesive. In addition, the structural rigidity of the two aromatic dianhydride monomers selected by the present invention is relatively large, and they have relatively superior thermal stability, which improves the high temperature resistance of the polyimide adhesive. In summary, the polyimide adhesive provided by the present invention has better high temperature resistance, better flame retardant properties and better bonding properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 Schematic diagram of the preparation method of the polyimide adhesive in the embodiment of the present invention;
[0019] Figure 2 is the Fourier transform infrared spectrum of the polyamidoamine adhesive in Example 2;
[0020] Figure 3 is the DSC spectrum of the polyamidoamine adhesive in Example 2;
[0021] Figure 4 This is a surface image of the failure area of the adhesive component in Example 2 after the single lap shear test. DETAILED DESCRIPTION
[0022] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. Although certain embodiments of the present invention are shown in the accompanying drawings, it should be understood that the present invention can be implemented in various forms and should not be interpreted as being limited to the embodiments described herein. On the contrary, these embodiments are provided to provide a more thorough and complete understanding of the present invention. It should be understood that the drawings and embodiments of the present invention are only for exemplary purposes and are not intended to limit the scope of protection of the present invention.
[0023] Unless otherwise defined, all technical and scientific terms used in this application have the same meanings as those commonly understood by those skilled in the art to which this application belongs; the terms used in the specification of this application are only for the purpose of describing specific implementation methods and are not intended to limit this application;
[0024] The term "including" and its variations used in this article are open inclusions, that is, "including but not limited to"; the term "based on" is "based at least in part on"; the term "one embodiment" means "at least one embodiment"; the term "another embodiment" means "at least one other embodiment"; the term "some embodiments" means "at least some embodiments"; the term "optionally" means "optional embodiments". The relevant definitions of other terms will be given in the following description. It should be noted that the concepts of "first" and "second" mentioned in the present invention are used to distinguish different objects, rather than to describe a specific order or a primary and secondary relationship. In addition, the terms "first" and "second" are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of this application, unless otherwise specified, the meaning of "multiple" is two or more.
[0025] like Figure 1 As shown, a method for preparing a polyimide adhesive provided by an embodiment of the present invention comprises:
[0026] Step S1, under the protection of an inert atmosphere, using a phosphorus-containing aromatic diamine, an ether-bonded aromatic diamine and an aromatic dianhydride composition as raw materials, to carry out a polymerization reaction in an aprotic solvent to obtain a polyamic acid solution; wherein the aromatic dianhydride composition is composed of two aromatic dianhydrides;
[0027] Step S2, removing the solvent from the polyamic acid solution, heating and curing the solution to obtain a polyimide adhesive.
[0028] In the embodiment of the present invention, a polyimide adhesive is obtained by using a phosphorus-oxyl-containing aromatic diamine, an ether-bond-containing aromatic diamine and two aromatic dianhydrides as raw materials through polymerization reaction and temperature curing; wherein the phosphorus-oxyl-containing aromatic diamine participates in the polymerization reaction to introduce the phosphorus-oxyl group into the molecular structure. Since the phosphorus-oxyl group has excellent flame retardant properties, the obtained polyimide adhesive has better flame retardancy; in addition, the phosphorus-containing large group introduced into the polyimide molecular chain by the phosphorus-oxyl-containing aromatic diamine destroys the symmetry and regularity of the molecular chain, which is beneficial to improving the high temperature resistance of the polyimide adhesive; the ether-bond-containing aromatic diamine participates in the polymerization reaction to introduce the ether bond into the molecular structure. Since the ether bond is a flexible group, it can provide a flexible molecular chain in the molecular structure of the polyimide adhesive, so that the activity of the polyimide in space is enhanced, which is more conducive to casting and spreading on the surface of the substrate, and the bonding probability of the polar bond in the polyimide adhesive and the substrate is increased, which is beneficial to improving the bonding performance of the polyimide adhesive. In addition, the two aromatic dianhydride monomers selected in the embodiment of the present invention have greater structural rigidity and superior thermal stability, which improves the high temperature resistance of the polyimide adhesive. In summary, the polyimide adhesive provided by the embodiment of the present invention has better high temperature resistance, better flame retardant properties and better bonding properties.
[0029] It should be noted that phosphorus oxy groups have excellent flame retardant properties as follows: during the combustion process, phosphorus can generate phosphoric acid or polyphosphate, which can form a stable carbon layer to isolate oxygen and heat sources, thereby effectively inhibiting combustion. In addition, phosphorus oxy groups can also reduce the propagation speed of flames and reduce the heat release rate.
[0030] In some embodiments of the present invention, in step S1, the phosphorus-oxygen-containing aromatic diamine has a structural formula as shown in formula (1):
[0031]
[0032] In some embodiments of the present invention, in step S1, the aromatic diamine containing an ether bond is selected from one of 2,2'-bis(trifluoromethyl)-4,4'-diaminophenyl ether, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 1,4-bis(4-aminophenoxy)benzene and 3,4'-diaminodiphenyl ether.
[0033] In some embodiments of the present invention, in step S1, the aromatic dianhydride composition is selected from any two of 3,3',4,4'-dibenzophenone tetracarboxylic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 2,3,3',4'-biphenyltetracarboxylic dianhydride, 4,4'-biphenyl ether dianhydride, 2,3,3',4'-diphenyl ether tetracarboxylic dianhydride and pyromellitic dianhydride.
[0034] In some embodiments of the present invention, in step S1, the aromatic dianhydride composition is composed of two aromatic dianhydrides in a molar ratio of (1-2):(1-2), the molar ratio of the phosphorus-containing aromatic diamine to the ether-containing aromatic diamine is (1-9):(1-9), and the ratio of the total molar number of the phosphorus-containing aromatic diamine and the ether-containing aromatic diamine to the total molar number of the aromatic dianhydride composition is 1:1.
[0035] In some embodiments of the present invention, in the step S1, the solid content of the polyamic acid solution is 25-40%.
[0036] In some embodiments of the present invention, in the step S1, the polymerization reaction is carried out at a temperature of 20-25° C. and for a time of 24-28 hours.
[0037] In some embodiments of the present invention, in step S2, the heating curing includes: after removing the solvent in the polyamic acid solution, keeping the temperature at 80°C for 1-2 hours, heating to 120°C, keeping the temperature for 1-2 hours, heating to 150°C, keeping the temperature for 1-2 hours, heating to 180°C, keeping the temperature for 1-2 hours, heating to 210°C, keeping the temperature for 1-2 hours, heating to 240°C, keeping the temperature for 1-2 hours, heating to 280°C, and keeping the temperature for 1-2 hours.
[0038] Optionally, in step S1, the aprotic solvent includes one of N,N-dimethylacetamide, N-methylpyrrolidone and N-methylformamide.
[0039] The embodiment of the present invention further provides a polyimide adhesive, which is prepared by the preparation method of the polyimide adhesive as described above.
[0040] Example 1
[0041] A1. In a 100 mL three-necked flask connected to a spherical condenser, a thermometer and nitrogen, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (2.1617 g, 0.01 mol), p-aminoacetophenone (1.3517 g, 0.01 mol), aniline (3.9119 g, 0.05 mol) and catalyst p-toluenesulfonic acid (0.0216 g) were added to obtain a mixture.
[0042] A2. In a nitrogen atmosphere, the mixture was heated to 110° C. under magnetic stirring, and refluxed at 110° C. for 24 h. After the reactant was cooled to room temperature, it was poured into methanol, and recrystallized multiple times in a 75° C. water bath. Light yellow crystals were obtained by suction filtration, and dried in a vacuum oven at 100° C. for 8 h to obtain a phosphorus-containing aromatic diamine with a yield of 62.7%. The structural formula of the phosphorus-containing aromatic diamine is shown in formula (1):
[0043]
[0044] The characterization data of the phosphorus-oxy-containing aromatic diamine are: 1 H NMR (400MHz, DMSO-d6) δ8.09 (dd, J = 8.3, 4.7Hz, 1H), 8.01 (dd, J = 8.2, 1.6Hz, 1H), 7.65 (t, J = 7..7Hz, 1H), 7.42-7.26 (m, 2H), 7.25-7.01 (m, 5H), 6.99-6.88 (m, 2H), 6.57-6.23 (m, 4H), 5.04 (s, 4H), 1.49 (d, J = 17.7Hz, 3H). The above characterization data prove the synthesis of the phosphorus-containing aromatic diamine.
[0045] Example 2
[0046] M1. At room temperature, a 100 ml three-necked flask was fixed on a mechanical stirring column, 30 ml of N-methylpyrrolidone (NMP), the phosphorus-containing aromatic diamine prepared in Example 1 (1.9979 g), and 3,4'-diaminodiphenyl ether (2.1889 g) were added to the three-necked flask, and mechanical stirring was performed for 30 min under the protection of N2 atmosphere. 3,3',4,4'-dibenzophenone tetracarboxylic dianhydride (2.5160 g) and 3,3',4,4'-biphenyl tetracarboxylic dianhydride (2.2973 g) were mixed evenly and added to the three-necked flask, and stirring was continued for 24 h to obtain a polyamide solution with a solid content of 30%; wherein, the characterization data of the polyamide in the polyamide solution are: 1 H NMR (400MHz, DMSO-d6) δ10.57 (s, 1H), 8.08 (d, J = 27.6Hz, 1H), δ7.74 (s, 1H), 7.58 (s, 1H), 7.42 (s, 1H), 3.31 (t, J = 7.0Hz, 6H), 2.70 (s, 9H), 2.18 (t, J = 8.1Hz, 6H), 1.98-1.84 (m, 6H). The above characterization data prove the synthesis of the polyamic acid.
[0047] M2. Apply the polyamic acid solution on the metal plate and heat it in a vacuum oven at 100° C. for 30 minutes to fully evaporate the solvent to obtain a polyamic acid coating; wherein the thickness of the polyamic acid coating is 0.2 mm.
[0048] M3. Bond two metal plates coated with polyamic acid together, place them in a vacuum oven for heating and curing to obtain a bonded piece; a polyamic acid adhesive is formed on the bonded piece, and the heating and curing temperature program is: keep warm at 80°C for 1 hour, heat to 120°C, keep warm for 1 hour, heat to 150°C, keep warm for 1 hour, heat to 180°C, keep warm for 1 hour, heat to 210°C, keep warm for 1 hour, heat to 240°C, keep warm for 1 hour, heat to 280°C, and keep warm for 1 hour.
[0049] The polyamidoamine adhesive in Example 2 was characterized by Fourier transform infrared spectroscopy. Figure 2 ,from Figure 2 It can be seen that the polyimide adhesive has a -1 The characteristic peak at 1722 cm is caused by the asymmetric stretching vibration of C=O in the imide ring, while -1 The characteristic peak at 1375cm is caused by the symmetrical stretching vibration of C=O. -1 and 728cm -1 The characteristic peaks at 1206 cm-1 are the stretching vibration peaks and bending vibration peaks of CN in the imide ring. -1 The characteristic peak at corresponds to the characteristic absorption peak of P=O; and the characteristic absorption peak of -COOH in polyamic acid has disappeared, further indicating that the polyamic acid has been completely imidized and converted into polyimide.
[0050] Example 3
[0051] M1. At room temperature, a 100 ml three-necked flask was fixed on a mechanical stirring column, 30 ml of N, N-dimethylacetamide (DMAc), the phosphorus-containing aromatic diamine (3.5563 g) obtained in Example 1, and 3,4'-diaminodiphenyl ether (1.6698 g) were added to the three-necked flask, and mechanical stirring was performed for 30 min under the protection of N2 atmosphere. 3,3',4,4'-dibenzophenone tetracarboxylic dianhydride (2.6871 g) and 2,3,3',4'-diphenyl ether tetracarboxylic dianhydride (2.5868 g) were mixed evenly and added to the three-necked flask, and stirring was continued for 24 h to obtain a polyamide solution with a solid content of 35%.
[0052] M2. Apply the polyamic acid solution on the metal plate and heat it in a vacuum oven at 100° C. for 30 minutes to fully evaporate the solvent to obtain a polyamic acid coating; wherein the thickness of the polyamic acid coating is 0.2 mm.
[0053] M3. Bond two metal plates coated with polyamic acid together, place them in a vacuum oven for heating and curing to obtain a bonded piece; a polyamic acid adhesive is formed on the bonded piece, and the heating and curing temperature program is: keep warm at 80°C for 1 hour, heat to 120°C, keep warm for 1 hour, heat to 150°C, keep warm for 1 hour, heat to 180°C, keep warm for 1 hour, heat to 210°C, keep warm for 1 hour, heat to 240°C, keep warm for 1 hour, heat to 280°C, and keep warm for 1 hour.
[0054] Example 4
[0055] M1. At room temperature, a 100 ml three-necked flask was fixed on a mechanical stirring column, 30 ml of N, N-dimethylformamide (DMF), the phosphorus-containing aromatic diamine prepared in Example 1 (1.9938 g), and 2,2-bis[4-(4-aminophenoxy)phenyl]propane (4.4782 g) were added into the three-necked flask, and mechanical stirring was performed for 30 min under the protection of N2 atmosphere. 2,3,3',4'-biphenyltetracarboxylic dianhydride (2.2926 g) and 2,3,3',4'-diphenyl ether tetracarboxylic dianhydride (2.4172 g) were mixed evenly and added into the three-necked flask, and stirring was continued for 24 h to obtain a polyamide solution with a solid content of 38%.
[0056] M2. Apply the polyamic acid solution on the metal plate and heat it in a vacuum oven at 100° C. for 30 minutes to fully evaporate the solvent to obtain a polyamic acid coating; wherein the thickness of the polyamic acid coating is 0.2 mm.
[0057] M3. Bond two metal plates coated with polyamic acid together, place them in a vacuum oven for heating and curing to obtain a bonded piece; a polyamic acid adhesive is formed on the bonded piece, and the heating and curing temperature program is: keep warm at 80°C for 1 hour, heat to 120°C, keep warm for 1 hour, heat to 150°C, keep warm for 1 hour, heat to 180°C, keep warm for 1 hour, heat to 210°C, keep warm for 1 hour, heat to 240°C, keep warm for 1 hour, heat to 280°C, and keep warm for 1 hour.
[0058] Example 5
[0059] The difference from Example 2 is that step M2 is: applying the polyamic acid solution on the metal plate, heating it in a vacuum oven at 80° C. for 50 minutes to fully evaporate the solvent to obtain a polyamic acid coating; wherein the thickness of the polyamic acid coating is 0.2 mm.
[0060] Comparative Example 1
[0061] The difference from Example 2 is that the phosphorus-containing aromatic diamine in step M1 is replaced by an equimolar amount of a diamine monomer not containing phosphorus-containing groups, and the diamine monomer not containing phosphorus-containing groups is 9,9-bis(4-aminophenyl)fluorene.
[0062] Comparative Example 2
[0063] The difference from Example 2 is that the 2-(4-aminophenyl)-5-aminobenzimidazole in step M1 is replaced by an equimolar amount of a diamine monomer without an ether bond, and the diamine monomer without an ether bond is a 2-(4-aminophenyl)-5-aminobenzimidazole monomer.
[0064] Comparative Example 3
[0065] The difference from Example 2 is that in step M1, 3,3',4,4'-biphenyltetracarboxylic dianhydride is replaced by an equal molar amount of bisphenol A type diether dianhydride, and 3,3',4,4'-dibenzophenone tetracarboxylic dianhydride is replaced by an equal molar amount of 4,4'-biphenyl ether dianhydride. Compared with 3,3',4,4'-dibenzophenone tetracarboxylic dianhydride and 3,3',4,4'-biphenyltetracarboxylic acid, 4,4'-biphenyl ether dianhydride and bisphenol A type diether dianhydride are more flexible.
[0066] Experimental example
[0067] The polyamidoamine adhesive in Example 2 was characterized by DSC spectra, and the results are shown in Figure 3 ,from Figure 3 It can be seen that the glass transition temperature of the polyimide adhesive in Example 2 is 263.7° C., which ensures the high-temperature performance of the polyimide adhesive. Figure 4 This is a surface picture of the failure area of the adhesive member in Example 2 after the single lap shear test. Figure 4 It can be seen that the polyimide adhesive is in a torn state, that is, the damage occurs inside the adhesive layer, indicating that its bonding strength with the metal sheet surface is greater than the strength of the polymer itself, indicating that the prepared polyimide adhesive has a good bonding effect with metal.
[0068] The flame retardant properties of the polyimide adhesives prepared in Examples 2-5 and Comparative Examples 1-3 were tested, and the results are shown in Table 1. The results of the single lap tensile shear strength test of the bonded parts prepared in Example 2-5 are shown in Table 1. It can be seen from Table 1 that compared with Comparative Example 1, the flame retardant grade of the polyimide adhesive in Example 2-5 is higher and the limiting oxygen index is larger, indicating that the flame retardant properties of the bonded parts in Example 2-5 are better. Compared with Comparative Example 2, the bonded parts in Example 2-5 have a higher single lap tensile shear strength at room temperature, indicating that the bonding properties of the polyimide adhesive in Example 2-5 are better. Compared with Comparative Example 3, the single lap tensile shear strength of the bonded parts in Example 2-5 at room temperature is not much different. The bonded parts in Example 2-5 still have a higher single lap tensile shear strength at 200°C, indicating that the high temperature resistance of the polyimide adhesive in Example 2-5 is better. In summary, the polyimide adhesives in Examples 2-5 have better high temperature resistance, better flame retardancy and better bonding properties.
[0069] Table 1
[0070]
[0071] It should be noted that flame retardant grade V0 is one of the flame retardant performance grades of plastic materials evaluated according to the US UL94 standard. The UL94 standard mainly has the following flame retardant grades, arranged from high to low in terms of flame retardant performance:
[0072] V0: After two 10-second flame combustion tests, the flame will extinguish itself for no more than 10 seconds after each removal of the fire source, and the total burning time will not exceed 50 seconds. There will be no dripping of burning material (i.e., it will not ignite cotton).
[0073] V1: Under the same test conditions, the flame self-extinguishing time of the material shall not exceed 30 seconds each time the fire source is removed, the total burning time shall not exceed 250 seconds, and there shall be no dripping of burning material.
[0074] V2: Under the same test conditions, the flame self-extinguishing time of the material shall not exceed 30 seconds each time the fire source is removed, and the total burning time shall not exceed 250 seconds, but the dripping material may ignite the cotton.
[0075] It should be noted that the limiting oxygen index refers to the oxygen concentration (expressed as volume fraction) that can just maintain the combustion of the material under normal pressure. It is generally believed that a limiting oxygen index of more than 25% indicates that the material has good flame retardant properties.
[0076] Although the present invention is disclosed as above, the protection scope of the present invention is not limited thereto. Those skilled in the art may make various changes and modifications without departing from the spirit and scope of the present invention, and these changes and modifications will fall within the protection scope of the present invention.
Claims
1. A method for preparing a polyimide adhesive, characterized in that: include: Step S1, under the protection of an inert atmosphere, using a phosphorus-containing aromatic diamine, an ether-bonded aromatic diamine and an aromatic dianhydride composition as raw materials, to carry out a polymerization reaction in an aprotic solvent to obtain a polyamic acid solution; wherein the aromatic dianhydride composition is composed of two aromatic dianhydrides; Step S2, removing the solvent from the polyamic acid solution, heating and curing the solution to obtain a polyimide adhesive.
2. The method for preparing a polyimide adhesive according to claim 1, characterized in that: In the step S1, the structural formula of the phosphorus-oxygen-containing aromatic diamine is shown in formula (1):
3. The method for preparing the polyimide adhesive according to claim 1, characterized in that: In step S1, the aromatic diamine containing an ether bond is selected from one of 2,2'-bis(trifluoromethyl)-4,4'-diaminophenyl ether, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 1,4-bis(4-aminophenoxy)benzene and 3,4'-diaminodiphenyl ether.
4. The method for preparing a polyimide adhesive according to claim 1, characterized in that: In step S1, the aromatic dianhydride composition is selected from any two of 3,3',4,4'-benzophenone tetracarboxylic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 2,3,3',4'-biphenyltetracarboxylic dianhydride, 4,4'-biphenyl ether dianhydride, 2,3,3',4'-diphenyl ether tetracarboxylic dianhydride and pyromellitic dianhydride.
5. The method for preparing the polyimide adhesive according to claim 1, characterized in that: In step S1, the aromatic dianhydride composition is composed of two aromatic dianhydrides in a molar ratio of (1-2):(1-2), the molar ratio of the phosphorus-containing aromatic diamine to the ether-bonded aromatic diamine is (1-9):(1-9), and the ratio of the total molar number of the phosphorus-containing aromatic diamine and the ether-bonded aromatic diamine to the total molar number of the aromatic dianhydride composition is 1:
1.
6. The method for preparing the polyimide adhesive according to claim 5, characterized in that: In the step S1, the solid content of the polyamic acid solution is 25-40%.
7. The method for preparing a polyimide adhesive according to claim 1, characterized in that: In the step S1, the polymerization reaction is carried out at a temperature of 20-25°C and for a time of 24-28 hours.
8. The method for preparing a polyimide adhesive according to claim 1, characterized in that: In the step S2, the temperature rise curing includes: after removing the solvent in the polyamic acid solution, keeping the temperature at 80°C for 1-2 hours, heating to 120°C, keeping the temperature for 1-2 hours, heating to 150°C, keeping the temperature for 1-2 hours, heating to 180°C, keeping the temperature for 1-2 hours, heating to 210°C, keeping the temperature for 1-2 hours, heating to 240°C, keeping the temperature for 1-2 hours, heating to 280°C, and keeping the temperature for 1-2 hours.
9. The method for preparing a polyimide adhesive according to claim 1, characterized in that: In the step S1, the aprotic solvent includes one of N,N-dimethylacetamide, N-methylpyrrolidone and N-methylformamide.
10. A polyimide adhesive, characterized in that: The polyimide adhesive is prepared by the preparation method of the polyimide adhesive according to any one of claims 1 to 9.
Citation Information
Patent Citations
Novel polyimide film with improved adhesiveness
CN101098909A
Polyimide adhesive and preparation method thereof
CN103865471A
High-fire-retardant soluble transparent polyimide film and preparation method thereof
CN106478969A
High-flame-retardant soluble polyimide film and preparation method thereof
CN106750426A
Aromatic imide film
CN115926218A
Cited By
High-temperature-resistant adhesive suitable for adhesion of large-size and non-planar composite materials and preparation method of high-temperature-resistant adhesive