Single-component high-hardness dealcoholized transparent sealant and preparation method thereof
By combining polycyclic silane reinforced resin and low viscosity alkoxy end capping 107 resin, the existing high-hard silicone sealant has been solved in terms of transparency and strength, and a single-hardness, high transparency and weather resistance have been prepared. Component sealant is suitable for multiple fields and achieves environmentally friendly and healthy construction results.
Patent Information
- Application Number
- CN202411136823.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-01
AI Technical Summary
The existing high-hardness silicone sealants have shortcomings in transparency and strength, and it is difficult to meet the needs of high hardness, high transparency and weather resistance in many fields.
A single-component high-hardness dehydrating transparent sealant was prepared by combining a polycyclic silane reinforced resin with a low viscosity alkoxy end capping 107 resin. Improve adhesion, hardness and transparency, and improve yellowing and weather resistance with liquid UV absorbers and phthalocyanine blue paste.
It achieves high hardness, high transparency and good weather resistance, and is suitable for many fields, such as solar cells, colored glass and sun visors, and the products are environmentally friendly and healthy, odor-free, and easy to construct.
Smart Images

Figure BDA0004999665760000021 
Figure BDA0004999665760000032 
Figure BDA0004999665760000041
Abstract
Description
Technical Field
[0001] The invention relates to the field of organic silicon sealants, and in particular to a single-component high-hardness dealcoholization type transparent sealant and a preparation method thereof. Background Art
[0002] Silicone sealants are basic polymers with -Si-O- as the main chain and -OH or -OCH3 as the end groups. They have excellent weather resistance and can withstand the erosion of ultraviolet radiation, high and low temperatures, and hot and humid environments, thus winning the favor of the market. According to the reaction mechanism, they can be divided into addition type and condensation type. Among them, condensation type silicone sealants have excellent adhesion to many types of substrates and can be used in multiple scenarios.
[0003] Solar cells, colored glass, acrylic, sun visors and many other fields require transparent adhesives with high light transmittance, high hardness, yellowing resistance and weather resistance. Epoxy adhesives have high strength and hardness, but poor yellowing resistance and weather resistance. Conventional silicone transparent adhesives have good yellowing resistance and weather resistance, but low hardness and strength, and cannot meet the use requirements. According to the published patents related to high-hardness silicone sealants, some patents add high-hardness fillers to improve the hardness and strength of the sealant, and some patents add rosin imide cross-linking agents to improve the strength of the sealant.
[0004] For example, Chinese patent document CN117659935 A discloses a highly transparent and high-strength silicone sealant and a preparation method thereof. The sealant includes polydimethylsiloxane, rosin imide crosslinker and catalyst. The invention patent first uses rosin acid and aminopropyl trimethoxysilane to prepare rosin imide crosslinker, and then adds polydimethylsiloxane and catalyst. Then, the mixture is stirred and mixed under nitrogen protection, and vacuum degassing is performed. The invention patent has high strength, but the silicone sealant with rosin imide is prone to yellowing, and the cured product is very brittle, so there are problems with transparency and strength.
[0005] Chinese patent document CN 115141599 A discloses a method for preparing a high-hardness organic silicon sealant, wherein the sealant comprises polydimethoxysilane, reinforcing filler (including porous ultrafine zeolite, nano calcium carbonate, heavy calcium, white carbon black, etc.), crosslinking agent, coupling agent and catalyst in batches, and vacuuming and stirring evenly. This invention patent cannot achieve the effect of high strength and high hardness, and it is not a transparent sealant.
[0006] Chinese patent CN201611253357 discloses a high-hardness anti-mildew porcelain sealant, wherein the sealant includes dimethoxysilane, trimethoxysilane, aluminum oxide, nano-calcium carbonate, fumed silica, silane coupling agent, etc., which are added in batches and stirred evenly by vacuuming. This invention patent has low strength, opacity, and poor adhesion. Summary of the invention
[0007] In view of the shortcomings of the prior art, the present invention synthesizes a multi-functional, multi-cyclic reactive reinforcing resin to prepare an environmentally friendly, low-odor, high-hardness, good bonding, high-transparency, and aging-resistant single-component dealcoholized transparent adhesive.
[0008] The technical solution of the present invention is:
[0009] The first aspect of the present invention provides a one-component high-hardness dealcoholization type transparent sealant, which comprises, by weight, 1000 parts of low-viscosity alkoxy-terminated 107 resin, 200-500 parts of polycyclic silane reinforced resin, 15-30 parts of dewatering agent, 5-20 parts of silane coupling agent, 50-150 parts of hydrophobic fumed silica, 5-20 parts of liquid ultraviolet absorber, 1-10 parts of catalyst, and 1-5 parts of phthalocyanine blue slurry;
[0010] The low viscosity alkoxy-terminated 107 resin has the following structural formula:
[0011]
[0012] Where n is an integer ranging from 100 to 1000;
[0013] The polycyclic silane reinforced resin has the following structural formula:
[0014] Wherein R is methyl or ethyl, R1 is methyl;
[0015] or Wherein R is methyl or ethyl.
[0016] In the sealant system of the present invention, a polycyclic silane-reinforced resin with a special structure is introduced to achieve good adhesion and higher hardness; a low-viscosity alkoxy-terminated 107 resin and an ultraviolet absorber are used in combination to achieve good weather resistance and better yellowing resistance; and the addition of hydrophobic fumed silica makes the system more transparent.
[0017] Furthermore, the low viscosity alkoxy-terminated 107 resin is prepared by mixing a hydroxy-terminated 107 resin with a viscosity of 500-1000 mPa.s and methyltrimethoxysilane or tetramethoxysilane in a weight ratio of 1000:60-100, heating to 70-80°C, vacuuming and stirring for 1-2 hours, and causing a replacement reaction under the action of a catalyst, dibutylamine formate.
[0018] The reaction principle is as follows:
[0019]
[0020] In a specific embodiment, 2 kg of hydroxy-terminated 107 resin with a viscosity of 500-1000 mPa.s is added to a planetary machine, 120-200 g of methyltrimethoxysilane (or tetramethoxysilane) is added, stirred evenly, a small amount of catalyst dibutylamine formate is added, the temperature is raised to 70-80°C, vacuumed and stirred for 1-2 hours to obtain a low viscosity alkoxy-terminated 107 resin.
[0021] Further, the polycyclic silane enhanced resin is prepared by pouring polyaminopropyl alkoxysilane into a reaction vessel, then dropping cyclohexylethyl alkoxysilane according to a molar ratio of 1:2, adding a small amount of tetrabutylammonium fluoride catalyst, and heating to 50-60°C for ring-opening reaction. Preferably, the dropwise addition and mixing are performed under nitrogen protection; preferably, the reaction time is 60-90min; as in a specific embodiment, 3 mol of polyaminopropyl alkoxysilane is poured into a reactor, nitrogen protection is passed and stirring is started, 6 mol of cyclohexylethyl alkoxysilane is dropped, a small amount of tetrabutylammonium fluoride catalyst is added, and the temperature is controlled at 50-60°C. After the dropwise addition is completed, the nitrogen valve is closed, the vacuum pump is turned on, and stirring is continued for 60-90 minutes to allow it to fully react to obtain a polycyclic silane enhanced resin.
[0022] The reaction mechanism is as follows:
[0023]
[0024] , wherein R is methyl or ethyl, and R1 is methyl.
[0025] The cyclohexylethylalkoxysilane is at least one or more of (3,4-epoxycyclohexyl)ethyltrimethoxysilane, (3,4-epoxycyclohexyl)ethyldimethoxysilane, (3,4-epoxycyclohexyl)ethyltriethoxysilane, and (3,4-epoxycyclohexyl)ethyldiethoxysilane.
[0026] The polyaminopropyl alkoxysilane is at least one or more of diethylenetriaminopropyltrimethoxysilane, diethylenetriaminopropyldimethoxysilane, diethylenetriaminopropyltriethoxysilane and diethylenetriaminopropyldiethoxysilane.
[0027] The polycyclic silane-reinforced resin is prepared by ring-opening reaction using a coupling agent with a special structure, and has good adhesion and higher hardness.
[0028] Furthermore, the specific surface area of the hydrophobic fumed silica is 100 m 2 / g—300m 2 / g. For example, 100m 2 / g, 120m 2 / g, 150m 2 / g, 170m2 / g, 200m 2 / g, 210m 2 / g and 300m 2 / g, etc.
[0029] Further, the silane coupling agent is at least one of γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropylmethyldimethoxysilane, N-n-butyl-3-aminopropyltrimethoxysilane, 3-ureapropyltrimethoxysilane, bis-[3-(trimethoxysilyl)-propyl]-amine, 3-anilinopropyltrimethoxysilane, N,N-diethyl-3-aminopropyltrimethoxysilane, 3-aminopropylmethyldiethoxysilane, 3-(N-cyclohexylamino)propyltrimethoxysilane, patented silane SIVO203, patented silane SIVO1146, patented silane SIVO210 and patented silane SIVO1189.
[0030] Furthermore, the catalyst is at least one of dibutyltin dilaurate, dibutyltin diacetate, dibutyltin didodecylsulfide, stannous octoate and dioctyltin dilaurate.
[0031] Furthermore, the dehydrating agent is at least one of vinyltrimethoxysilane and vinyltriethoxysilane.
[0032] Furthermore, the liquid UV absorber is at least one of UV-1130, UV-292, UV-400, UV384-2, UV-123, UV-400, UV-1130 of Lianlong (Tianjin Lianlong New Materials Co., Ltd.) and UV-6606 of Ciba (Germany Ciba). It is preferred to use a liquid UV absorber, which is easy to mix and more conducive to transparency.
[0033] In another aspect of the present invention, a method for preparing the one-component high-hardness dealcoholization type transparent sealant is provided, comprising the steps of:
[0034] ① First, vacuum and stir the formulated amount of low-viscosity alkoxy-terminated 107 resin, polycyclic silane-reinforced resin, liquid UV absorber, and phthalocyanine blue slurry for 5-10 minutes;
[0035] ② Then add the formulated amount of hydrophobic fumed silica, stir at low speed for 5-10 minutes to mix the fumed silica into the resin, and then vacuum and stir at high speed for 25-30 minutes;
[0036] ③ Then add the formulated amount of silane coupling agent, dehydrating agent, and catalyst, vacuum and stir for 15-20 minutes to mix evenly.
[0037] Compared with the prior art, the present invention has the following beneficial effects:
[0038] The present invention adopts a coupling agent of special structure to carry out ring-opening reaction to prepare a polycyclic silane reinforced resin with good adhesion and higher hardness. Low viscosity alkoxy-terminated 107 resin has higher strength and hardness, excellent mechanical properties, phthalocyanine blue slurry and liquid ultraviolet absorber, better yellowing resistance and weather resistance, hydrophobic fumed silica, reinforcing effect, better compatibility and higher transparency. The sealant product of the present invention is environmentally friendly, healthy and odorless, does not contain VOC, formaldehyde, is easy to construct, and the cured product has high hardness, transparency, yellowing resistance and good weather resistance. It can be applied to solar cells, colored glass, acrylic, sun visors, billboards, kitchen stoves, washbasins, bathtubs and other fields. DETAILED DESCRIPTION
[0039] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.
[0040] Unless otherwise specified, other reagents, materials, and equipment used in the examples of the present invention are all commercially available; unless otherwise specified, the test methods are all conventional test methods in the art.
[0041] Example 1
[0042] A single-component high-hardness dealcoholized transparent adhesive, the preparation method is as follows:
[0043] ① First prepare a low-viscosity alkoxy-terminated 107 resin, take 2kg of hydroxy-terminated 107 resin with a viscosity of 500mPa.s and add it to a planetary machine, add 150g of methyltrimethoxysilane, stir evenly, add a small amount of catalyst dibutylamine formate, heat to 70℃, vacuum and stir to react for 1h to obtain a low-viscosity alkoxy-terminated 107 resin.
[0044] ② To prepare a polycyclic silane enhanced resin, 3 mol of diethylenetriaminepropyldimethoxysilane was poured into the reaction kettle, and stirring was started under nitrogen protection. 6 mol of (3,4-epoxycyclohexyl)ethyldimethoxysilane was added dropwise, and a small amount of tetrabutylammonium fluoride catalyst was added. The temperature was controlled at 50-60°C. After the addition was completed, the nitrogen valve was closed, the vacuum pump was turned on, and stirring was continued for 60 minutes to allow it to fully react to obtain a polycyclic silane enhanced resin.
[0045] ③ Take 1kg of low-viscosity alkoxy-terminated 107 resin, 200g of polycyclic silane-reinforced resin, 5g of UV-1130 ultraviolet absorber, and 1g of phthalocyanine blue slurry, mix them, and vacuum stir for 5-10 minutes.
[0046] ④Start adding 80g of the specific surface area of 100m 2 / g of hydrophobic fumed silica, first stir at low speed for 10 minutes to allow the gas phase to mix into the resin, then evacuate and stir at high speed for 25 minutes.
[0047] ⑤ Add 5g of silane coupling agent γ-aminopropyltrimethoxysilane, 15g of dehydrating agent vinyltrimethoxysilane, and 1g of catalyst dibutyltin dilaurate, and stir in a vacuum for 15 minutes to mix them evenly.
[0048] ⑥Discharge the materials by packing.
[0049] Example 2
[0050] A single-component high-hardness dealcoholized transparent adhesive, the preparation method is as follows:
[0051] ① First prepare a low-viscosity alkoxy-terminated 107 resin, take 2kg of hydroxy-terminated 107 resin with a viscosity of 1000mPa.s and add it to a planetary machine, add 150g of methyltrimethoxysilane, stir evenly, add a small amount of dibutylamine formate catalyst, heat to 75℃, vacuum and stir to react for 1h to obtain a low-viscosity alkoxy-terminated 107 resin.
[0052] ② To prepare a polycyclic silane-enhanced resin, 3 mol of diethylenetriaminepropyldimethoxysilane was poured into the reaction kettle, and stirring was started under nitrogen protection. 6 mol of (3,4-epoxycyclohexyl)ethyldimethoxysilane was added dropwise, and a small amount of tetrabutylammonium fluoride catalyst was added. The temperature was controlled at 50-60°C. After the addition was completed, the nitrogen valve was closed, the vacuum pump was turned on, and stirring was continued for 80 minutes to allow it to fully react to obtain a polycyclic silane-enhanced resin.
[0053] ③ Take 1 kg of low-viscosity alkoxy-terminated 107 resin, 250 g of polycyclic silane-reinforced resin, 8 g of UV-1130 ultraviolet absorber, and 1 g of phthalocyanine blue slurry, mix them, and vacuum stir for 8 minutes.
[0054] ④Start by adding 100g of a specific surface area of 100m 2 / g hydrophobic fumed silica, first stir at low speed for 10 minutes to allow the gas phase to mix into the resin, then evacuate and stir at high speed for 27 minutes.
[0055] ⑤ Add 10g of silane coupling agent N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, 15g of dehydrating agent vinyltrimethoxysilane, and 3g of catalyst dibutyltin dilaurate, and stir in a vacuum for 20 minutes to mix evenly.
[0056] ⑥Discharge the materials by packing.
[0057] Example 3
[0058] A single-component high-hardness dealcoholized transparent adhesive, the preparation method is as follows:
[0059] ① First prepare a low-viscosity alkoxy-terminated 107 resin, take 2 kg of hydroxy-terminated 107 resin with a viscosity of 1000 mPa.s and add it to a planetary machine, add 150 g of tetramethoxysilane, stir evenly, add a small amount of dibutylamine formate catalyst, heat to 70°C, vacuum and stir to react for 1 hour to obtain a low-viscosity alkoxy-terminated 107 resin.
[0060] ② To prepare a polycyclic silane-enhanced resin, 3 mol of diethylenetriaminopropyltrimethoxysilane was poured into the reaction kettle, and stirring was started under nitrogen protection. 6 mol of (3,4-epoxycyclohexyl)ethyltrimethoxysilane was added dropwise, and a small amount of tetrabutylammonium fluoride catalyst was added. The temperature was controlled at 50-60°C. After the addition was completed, the nitrogen valve was closed, the vacuum pump was turned on, and stirring was continued for 90 minutes to allow it to fully react to obtain a polycyclic silane-enhanced resin.
[0061] ③ Take 1 kg of low-viscosity alkoxy-terminated 107 resin, 300 g of polycyclic silane-reinforced resin, 10 g of UV-1130 ultraviolet absorber, and 3 g of phthalocyanine blue slurry, mix them, and vacuum stir for 10 minutes.
[0062] ④Start adding 120g of the specific surface area of 150m 2 / g hydrophobic fumed silica, first stir at low speed for 10 minutes to allow the gas phase to mix into the resin, then evacuate and stir at high speed for 30 minutes;
[0063] ⑤ Add 15g of silane coupling agent N-n-butyl-3-aminopropyltrimethoxysilane, 3-ureapropyltrimethoxysilane, 20g of dehydrating agent vinyltrimethoxysilane, 4g of catalyst dibutyltin dilaurate, vacuum stir for 20 minutes to mix evenly.
[0064] ⑥Discharge the materials by packing.
[0065] Example 4
[0066] A single-component high-hardness dealcoholized transparent adhesive, the preparation method is as follows:
[0067] ① First prepare a low-viscosity alkoxy-terminated 107 resin, take 2 kg of hydroxy-terminated 107 resin with a viscosity of 1000 mPa.s and add it to a planetary machine, add 150 g of tetramethoxysilane, stir evenly, add a small amount of dibutylamine formate catalyst, heat to 70°C, vacuum and stir to react for 1 hour to obtain a low-viscosity alkoxy-terminated 107 resin.
[0068] ② To prepare a polycyclic silane-enhanced resin, 3 mol of diethylenetriaminopropyltrimethoxysilane was poured into the reaction kettle, and stirring was started under nitrogen protection. 6 mol of (3,4-epoxycyclohexyl)ethyltrimethoxysilane was added dropwise, and a small amount of tetrabutylammonium fluoride catalyst was added. The temperature was controlled at 50-60°C. After the addition was completed, the nitrogen valve was closed, the vacuum pump was turned on, and stirring was continued for 90 minutes to allow it to fully react to obtain a polycyclic silane-enhanced resin.
[0069] ③ Take 1 kg of low-viscosity alkoxy-terminated 107 resin, 400 g of polycyclic silane-reinforced resin, 15 g of ultraviolet absorber UV-1130, and 4 g of phthalocyanine blue slurry, mix them, and vacuum stir for 10 minutes.
[0070] ④Start adding 150g of the specific surface area of 200m 2 / g of hydrophobic fumed silica, first stir at low speed for 10 minutes to allow the gas phase to mix into the resin, then evacuate and stir at high speed for 30 minutes.
[0071] ⑤ Add 10g of silane coupling agent γ-aminopropyltrimethoxysilane, 24g of dehydrating agent vinyltrimethoxysilane, and 5g of catalyst dibutyltin dilaurate, and stir in a vacuum for 20 minutes to mix evenly.
[0072] ⑥Discharge the materials by packing.
[0073] Example 5
[0074] A single-component high-hardness dealcoholized transparent adhesive, the preparation method is as follows:
[0075] ① First prepare a low-viscosity alkoxy-terminated 107 resin, take 2kg of hydroxy-terminated 107 resin with a viscosity of 1000mPa.s and add it to a planetary machine, add 150g of methyltrimethoxysilane, stir evenly, add a small amount of dibutylamine formate catalyst, heat to 75℃, vacuum and stir to react for 1h to obtain a low-viscosity alkoxy-terminated 107 resin.
[0076] ② To prepare a polycyclic silane-enhanced resin, 3 mol of diethylenetriaminopropyltrimethoxysilane was poured into the reaction kettle, and stirring was started under nitrogen protection. 6 mol of (3,4-epoxycyclohexyl)ethyltrimethoxysilane was added dropwise, and a small amount of tetrabutylammonium fluoride catalyst was added. The temperature was controlled at 50-60°C. After the addition was completed, the nitrogen valve was closed, the vacuum pump was turned on, and stirring was continued for 90 minutes to allow it to fully react to obtain a polycyclic silane-enhanced resin.
[0077] ③ Take 1 kg of low-viscosity alkoxy-terminated 107 resin, 500 g of polycyclic silane-reinforced resin, 20 g of ultraviolet absorber UV-1130, and 5 g of phthalocyanine blue slurry, mix them, and vacuum stir for 10 minutes.
[0078] ④Start adding 150g of specific surface area of 300m 2 / g of hydrophobic fumed silica, first stir at low speed for 10 minutes to allow the gas phase to mix into the resin, then evacuate and stir at high speed for 30 minutes.
[0079] ⑤ Add 20g of silane coupling agent γ-aminopropyltrimethoxysilane, 30g of dehydrating agent vinyltrimethoxysilane, and 7g of catalyst dibutyltin dilaurate, and stir in a vacuum for 20 minutes to mix evenly.
[0080] ⑥Discharge the materials by packing.
[0081] Comparative Example 1
[0082] A transparent adhesive, which differs from Example 4 in that it does not contain a polycyclic silane-reinforced resin, and the specific preparation method is as follows:
[0083] ① First prepare a low-viscosity alkoxy-terminated 107 resin, take 2 kg of hydroxy-terminated 107 resin with a viscosity of 1000 mPa.s and add it to a planetary machine, add 150 g of tetramethoxysilane, stir evenly, add a small amount of dibutylamine formate catalyst, heat to 70°C, vacuum and stir to react for 1 hour to obtain a low-viscosity alkoxy-terminated 107 resin.
[0084] ② Take 1 kg of low-viscosity alkoxy-terminated 107 resin, 15 g of ultraviolet absorber UV-1130, and 4 g of phthalocyanine blue slurry, mix them, and vacuum stir for 10 minutes.
[0085] ③Start adding 150g of the specific surface area of 200m 2 / g of hydrophobic fumed silica, first stir at low speed for 10 minutes to allow the gas phase to mix into the resin, then evacuate and stir at high speed for 30 minutes.
[0086] ④ Add 10g of silane coupling agent γ-aminopropyltrimethoxysilane, 24g of dehydrating agent vinyltrimethoxysilane, and 5g of catalyst dibutyltin dilaurate, and stir in a vacuum for 20 minutes to mix them evenly.
[0087] ⑤Discharge the materials by packing.
[0088] Comparative Example 2
[0089] A transparent adhesive, which is different from Example 4 in that the low-viscosity alkoxy-terminated 107 resin is different, and the preparation method is as follows:
[0090] ① First prepare a low-viscosity alkoxy-terminated 107 resin, take 2kg of hydroxy-terminated 107 resin with a viscosity of 2000mPa.s and add it to a planetary machine, add 150g of tetramethoxysilane, stir evenly, add a small amount of dibutylamine formate catalyst, heat to 70℃, vacuum and stir to react for 1h to obtain a low-viscosity alkoxy-terminated 107 resin.
[0091] ② To prepare a polycyclic silane-enhanced resin, 3 mol of diethylenetriaminopropyltrimethoxysilane was poured into the reaction kettle, and stirring was started under nitrogen protection. 6 mol of (3,4-epoxycyclohexyl)ethyltrimethoxysilane was added dropwise, and a small amount of tetrabutylammonium fluoride catalyst was added. The temperature was controlled at 50-60°C. After the addition was completed, the nitrogen valve was closed, the vacuum pump was turned on, and stirring was continued for 90 minutes to allow it to fully react to obtain a polycyclic silane-enhanced resin.
[0092] ③ Take 1 kg of low-viscosity alkoxy-terminated 107 resin, 400 g of polycyclic silane-reinforced resin, 15 g of ultraviolet absorber UV-1130, and 4 g of phthalocyanine blue slurry, mix them, and vacuum stir for 10 minutes.
[0093] ④Start adding 150g of the specific surface area of 200m 2 / g of hydrophobic fumed silica, first stir at low speed for 10 minutes to allow the gas phase to mix into the resin, then evacuate and stir at high speed for 30 minutes.
[0094] ⑤ Add 10g of silane coupling agent γ-aminopropyltrimethoxysilane, 24g of dehydrating agent vinyltrimethoxysilane, and 5g of catalyst dibutyltin dilaurate, and stir in a vacuum for 20 minutes to mix evenly.
[0095] ⑥Discharge the materials by packing.
[0096] Comparative Example 3
[0097] A transparent adhesive, which differs from Example 4 in that it does not contain fumed silica, and the preparation method is as follows:
[0098] ① First prepare a low-viscosity alkoxy-terminated 107 resin, take 2 kg of hydroxy-terminated 107 resin with a viscosity of 1000 mPa.s and add it to a planetary machine, add 150 g of tetramethoxysilane, stir evenly, add a small amount of dibutylamine formate catalyst, heat to 75°C, vacuum and stir to react for 1 hour to obtain a low-viscosity alkoxy-terminated 107 resin.
[0099] ② To prepare a polycyclic silane-enhanced resin, 3 mol of diethylenetriaminopropyltrimethoxysilane was poured into the reaction kettle, and stirring was started under nitrogen protection. 6 mol of (3,4-epoxycyclohexyl)ethyltrimethoxysilane was added dropwise, and a small amount of tetrabutylammonium fluoride catalyst was added. The temperature was controlled at 50-60°C. After the addition was completed, the nitrogen valve was closed, the vacuum pump was turned on, and stirring was continued for 90 minutes to allow it to fully react to obtain a polycyclic silane-enhanced resin.
[0100] ③ Take 1 kg of low-viscosity alkoxy-terminated 107 resin, 400 g of polycyclic silane-reinforced resin, 15 g of ultraviolet absorber UV-1130, and 4 g of phthalocyanine blue slurry, mix them, and vacuum stir for 10 minutes.
[0101] ④ Add 10g of silane coupling agent γ-aminopropyltrimethoxysilane, 24g of dehydrating agent vinyltrimethoxysilane, and 5g of catalyst dibutyltin dilaurate, and stir in a vacuum for 20 minutes to mix them evenly.
[0102] ⑤Discharge the materials by packing.
[0103] Sample testing
[0104] The sealant samples obtained in the above examples and comparative examples were tested, and the test results are as follows.
[0105] Test Example 1
[0106] Surface drying time: Tested according to GB / T 13477.5-2002, fill the sealing material sample into a mold frame of specified shape under specified conditions, and use the time required for a film to be placed on the sample surface or for the sample to remain unadhered to the finger.
[0107] Tensile strength and elongation at break: tested according to GB / T528-2009 "Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber".
[0108] Hardness: Tested according to GB / T2411-2008;
[0109] Light transmittance: Tested according to GB / T2410-2008 "Determination of light transmittance and haze of transparent plastics", with a film thickness of 1mm.
[0110] Table 1 Performance test results
[0111]
[0112] From the test results in Table 1, it can be seen that compared with Comparative Examples 1-3, the tensile strength, hardness and light transmittance of the sealant prepared in Examples 1-4 of the present invention are better.
[0113] Test Example 2
[0114] UV aging test: Prepare the sample and place it in a UVA-340 UV aging box for 3 days to test the color change of the glue sample and whether it is powdery or cracked.
[0115] Table 2 UV performance test results
[0116]
[0117]
[0118] From the test results in Table 2, it can be seen that compared with Comparative Examples 1-3, the sealants prepared in Examples 1-4 of the present invention have better UV resistance, no obvious color change, and no powdering or cracking on the surface.
[0119] Test Example 3
[0120] Adhesion test: stick anti-adhesive tape on one side of the substrate surface, apply glue on the surface of different substrates (wood, stainless steel, aluminum alloy and PVC), pull up the sealant from the anti-adhesive tape after it is completely cured for 5 days, and peel it off at 90° at the bonding point to determine the type of bonding surface damage. The thickness of the coating is 1mm.
[0121] Table 3 Adhesion performance test results
[0122] wood Stainless steel Aluminum Alloy PVC Example 1 Cohesive failure 85% cohesive failure 90% cohesive failure 95% cohesive failure Example 2 Cohesive failure 90% cohesive failure 95% cohesive failure Cohesive failure Example 3 Cohesive failure Cohesive failure Cohesive failure Cohesive failure Example 4 Cohesive failure Cohesive failure Cohesive failure Cohesive failure Example 5 Cohesive failure Cohesive failure Cohesive failure Cohesive failure Comparative Example 1 80% cohesive failure 75% cohesive failure 80% cohesive failure 75% cohesive failure Comparative Example 2 90% cohesive failure 80% cohesive failure 80% cohesive failure 95% cohesive failure Comparative Example 3 70% cohesive failure 50% cohesive failure 60% cohesive failure 50% cohesive failure
[0123] From the test results in Table 3, it can be seen that compared with Comparative Examples 1-4, the sealant prepared in Examples 1-4 has excellent adhesion to different substrates such as wood, stainless steel, aluminum alloy, and PVC.
[0124] It can be seen from the above results that the polycyclic silane reinforced resin of the present invention has a significant effect on the tensile strength, hardness, light transmittance and bonding performance of the sealant, the low viscosity alkoxy-terminated 107 resin has a greater effect on the tensile strength and hardness, the hydrophobic fumed silica has a significant reinforcing effect, better compatibility and higher transparency. The components of the present invention cooperate and support each other, and the obtained sealant product has high hardness, transparency, yellowing resistance and good weather resistance.
[0125] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0126] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A one-component high-hardness dealcoholization type transparent sealant, It is characterized in that The components include, by weight, 1000 parts of low-viscosity alkoxy-terminated 107 resin, 200-500 parts of polycyclic silane-reinforced resin, 15-30 parts of dewatering agent, 5-20 parts of silane coupling agent, 50-150 parts of hydrophobic fumed silica, 5-20 parts of liquid ultraviolet absorber, 1-10 parts of catalyst, and 1-5 parts of phthalocyanine blue slurry; The low viscosity alkoxy-terminated 107 resin has the following structural formula: or Where n is an integer ranging from 100 to 1000; The polycyclic silane reinforced resin has the following structural formula: Where R is methyl or ethyl, R 1 is methyl; or Wherein R is methyl or ethyl.
2. The one-component high-hardness dealcoholization type transparent sealant according to claim 1, It is characterized in that The low viscosity alkoxy-terminated 107 resin is prepared by mixing a hydroxy-terminated 107 resin with a viscosity of 500-1000 mPa.s and methyltrimethoxysilane or tetramethoxysilane in a weight ratio of 1000:60-100, heating to 70-80°C, vacuuming and stirring for 1-2 hours, and causing a replacement reaction under the action of a catalyst, dibutylamine formate.
3. The one-component high-hardness dealcoholization type transparent sealant according to claim 1, It is characterized in that The polycyclic silane enhanced resin is prepared by pouring polyaminopropyl alkoxysilane into a reaction container, then adding cyclohexylethyl alkoxysilane in a molar ratio of 1:2, adding a small amount of tetrabutylammonium fluoride catalyst, and heating to 50-60°C for ring-opening reaction.
4. The one-component high-hardness dealcoholization type transparent sealant according to claim 1, It is characterized in that The cyclohexylethylalkoxysilane is at least one or more of (3,4-epoxycyclohexyl)ethyltrimethoxysilane, (3,4-epoxycyclohexyl)ethyldimethoxysilane, (3,4-epoxycyclohexyl)ethyltriethoxysilane, and (3,4-epoxycyclohexyl)ethyldiethoxysilane; The polyaminopropyl alkoxysilane is at least one or more of diethylenetriaminopropyltrimethoxysilane, diethylenetriaminopropyldimethoxysilane, diethylenetriaminopropyltriethoxysilane and diethylenetriaminopropyldiethoxysilane.
5. The one-component high-hardness dealcoholization type transparent sealant according to claim 1, It is characterized in that The specific surface area of the hydrophobic fumed silica is 100 m 2 / g—300m 2 / g.
6. The one-component high-hardness dealcoholization type transparent sealant according to claim 1, It is characterized in that The silane coupling agent is at least one of γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, γ-glycidoxypropyltrimethoxysilane and γ-methacryloxypropyltrimethoxysilane, 3-aminopropylmethyldimethoxysilane, N-n-butyl-3-aminopropyltrimethoxysilane, 3-ureapropyltrimethoxysilane, bis-[3-(trimethoxysilyl)-propyl]-amine, 3-anilinopropyltrimethoxysilane, N,N-diethyl-3-aminopropyltrimethoxysilane, 3-aminopropylmethyldiethoxysilane, 3-(N-cyclohexylamino)propyltrimethoxysilane, patented silane SIVO203, patented silane SIVO1146, patented silane SIVO210, and patented silane SIVO1189.
7. The one-component high-hardness dealcoholization type transparent sealant according to claim 1, It is characterized in that The catalyst is at least one of dibutyltin dilaurate, dibutyltin diacetate, dibutyltin didodecylsulfide, stannous octoate and dioctyltin dilaurate.
8. The one-component high-hardness dealcoholization type transparent sealant according to claim 1, It is characterized in that The dewatering agent is at least one of vinyl trimethoxy silane and vinyl triethoxy silane.
9. The one-component high-hardness dealcoholization type transparent sealant according to claim 1, It is characterized in that The liquid ultraviolet absorber is at least one of Lianlong UV-1130, UV-292, UV-400, UV384-2, UV-123, UV-400, UV-1130, and Ciba UV-6606.
10. A method for preparing a one-component high-hardness dealcoholization type transparent sealant according to any one of claims 1 to 9, It is characterized in that Includes steps: ① First, vacuum and stir the formulated low-viscosity alkoxy-terminated 107 resin, polycyclic silane-reinforced resin, liquid UV absorber, and phthalocyanine blue slurry for 5-10 minutes; ② Then add the formulated amount of hydrophobic fumed silica, stir at low speed for 5-10 minutes to mix the fumed silica into the resin, and then vacuum and stir at high speed for 25-30 minutes; ③ Then add the formulated amount of silane coupling agent, dehydrating agent, and catalyst, vacuum and stir for 15-20 minutes to mix them evenly.