Formula of liquid glue applied to flexible heat preservation pad

By using the formula of methylvinyl dimethyl (siloxane and polysiloxane), silica and platinum complex in the liquid glue of a flexible insulation pad, the problem of odor of liquid glue was solved, and the problem of odor of liquid glue was achieved without Odor, single color, good flow and strength performance improves user experience and product quality.

CN118879274APending Publication Date: 2024-11-01DONGGUAN LIFENG ELECTRONICS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411146554.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The liquid glue used in existing flexible insulation pads has odor problems, which affects the user's appetite and the taste of the meal.

Method used

Using the formula of methylvinyl dimethyl (siloxane and polysiloxane), silica and platinum complex, the composition ratio is adjusted to prepare odor-free, single color, good flow and strength performance. liquid glue.

Benefits of technology

It effectively solves the odor problem of liquid glue, improves user experience, and meets the production needs of flexible insulation pads.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118879274A_ABST
    Figure CN118879274A_ABST
Patent Text Reader

Abstract

The invention discloses a liquid glue formula applied to a flexible heat preservation pad. The liquid glue formula comprises methyl vinyl dimethyl (siloxane and polysiloxane), silicon dioxide and a platinum complex. The value range of the parts of the methyl vinyl dimethyl (siloxane and polysiloxane) is 49.95 to 79.95 parts; the value range of the part number of the silicon dioxide is 20.05 to 50.05; the value range of the parts of the platinum complex is 0.01 to 0.08. By blending methyl vinyl dimethyl (siloxane and polysiloxane), silicon dioxide and a platinum complex, the problem that liquid glue adopted by an existing flexible heat preservation pad has peculiar smell is effectively solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of liquid glue, and in particular to a liquid glue formula applied to a flexible thermal insulation pad. Background Art

[0002] As people's living standards continue to improve, they pay more attention to nutrition and flavor in their diet, and pay more attention to keeping the food fresh from beginning to end. At present, the existing dining table can provide convenience for diners to get food, but it cannot keep hot food at a constant temperature, thus affecting the diners' taste; and many users want to eat hot meals when they return home after overtime, and they have to reheat the meals, which will affect the taste of the meals.

[0003] Publication number CN219742383U provides a flexible thermal insulation board, including a heating pad and a heating wire; the heating pad is formed with a limiting groove for the heating wire to pass through, and the limiting grooves are evenly distributed around the heating pad; the heating pad is provided with a power supply, and the end of the heating wire is connected to the power supply; a plurality of protruding structures are formed on the end surface of one end of the heating pad, and the heights of all the protruding structures are equal; the heating pad and the heating wire are made of flexible materials; the heating wire is fixed in the limiting groove by liquid glue. A cross-linking agent and a coupling agent are added to the liquid glue in this technical solution, so that the liquid glue has a pungent smell, thereby affecting the user's appetite; therefore, a liquid glue formula applied to a flexible thermal insulation pad is provided to solve the above problems. Summary of the invention

[0004] One of the purposes of the present invention is to provide a liquid glue formula for use in a flexible thermal insulation pad, so as to solve the problem that the liquid glue used in the existing flexible thermal insulation pad has an odor.

[0005] A liquid glue formula for a flexible thermal insulation pad of the present invention can be realized by the following technical solutions:

[0006] The invention discloses a liquid adhesive formula for a flexible thermal insulation pad, comprising methyl vinyl dimethyl (siloxane and polysiloxane), silicon dioxide and a platinum complex;

[0007] Among them, the proportion of the methylvinyl dimethyl (siloxane and polysiloxane) ranges from 49.95 to 79.95 parts; the proportion of the silicon dioxide ranges from 20.05 to 50.05 parts; and the proportion of the platinum complex ranges from 0.01 to 0.08 parts.

[0008] In one embodiment, the proportion of methylvinyl dimethyl (siloxane and polysiloxane) ranges from 59.95 to 69.95 parts; the proportion of silicon dioxide ranges from 30.05 to 40.05 parts; and the proportion of the platinum complex is 0.05 parts.

[0009] In one embodiment, the proportion of methylvinyl dimethyl (siloxane and polysiloxane) is 65 parts; the proportion of silicon dioxide is 34.95 parts; and the proportion of platinum complex is 0.05 parts.

[0010] Compared with the prior art, the liquid glue formula of the present invention applied to the flexible thermal insulation pad has the following beneficial effects:

[0011] The invention discloses a liquid adhesive formula for a flexible thermal insulation pad, which effectively solves the problem that the liquid adhesive used in the existing flexible thermal insulation pad has odor by combining methyl vinyl dimethyl (siloxane and polysiloxane), silicon dioxide and a platinum complex. At the same time, the liquid adhesive prepared by the invention has the characteristics of no odor, single color, good vulcanization, flowability and strength performance through precise proportions, and can meet the production requirements of the flexible thermal insulation pad and improve the user experience. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0013] Figure 1 This is a comparison table of the proportions of the components in the first comparison group of a liquid glue formula for a flexible thermal insulation pad of the present invention;

[0014] Figure 2 This is a comparison table of the proportions of the components in the second comparison group of a liquid glue formula for a flexible thermal insulation pad of the present invention;

[0015] Figure 3 This is a comparison table of the proportions of the components in the third comparison group of a liquid glue formula for a flexible thermal insulation pad of the present invention;

[0016] Figure 4 This is a comparison table of the proportions of the components in the fourth comparison group of a liquid glue formula used for a flexible thermal insulation pad of the present invention. DETAILED DESCRIPTION

[0017] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be described clearly and completely in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Generally, the components of the embodiments of the present invention described and shown in the drawings here can be arranged and designed in various different configurations.

[0018] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0019] See also Figure 1-Figure 4 As shown, the liquid adhesive formula used for the flexible thermal insulation pad of the present invention includes methyl vinyl dimethyl (siloxane and polysiloxane), silicon dioxide and platinum complex.

[0020] The CAS number of methylvinyl dimethyl (siloxane and polysiloxane) is 67762-94-1; methylvinyl dimethyl siloxane has many excellent properties; first, methylvinyl dimethyl siloxane has good heat resistance and cold resistance, and can maintain its stable performance at extremely low and high temperatures; second, methylvinyl dimethyl siloxane has excellent electrical insulation and dielectric properties, and can be used in electronic devices and electrical insulation materials; third, methylvinyl dimethyl siloxane also has excellent waterproof, antioxidant and anti-purple properties, and can be used in coatings, sealing materials and surface modifiers. Polysiloxane is a polymer formed by silicon and oxygen elements connected to each other through silicon-oxygen bonds; polysiloxane has excellent heat resistance, chemical stability and electrical insulation properties; polysiloxane materials can have different properties and uses according to different polymerization degrees and the introduction of functional groups; in the field of materials, polysiloxane can be used as adhesives, fillers, coatings and lubricants, etc.

[0021] The CAS number of silicon dioxide is 7631-86-9. Silicon dioxide is a colorless, transparent crystal or amorphous powder, and is odorless. The melting point of silicon dioxide is 1710℃ (cristobalite) and 1670℃ (tridymite). Its boiling point is 2230℃. Silicon dioxide is almost insoluble in water and ordinary acid, but can be dissolved in hydrofluoric acid to generate silicon fluoride gas, which slowly reacts with hot concentrated phosphoric acid. The amorphous powder can react with alkali. It has stable physical and chemical properties, is easy to shape, is inert, and the melt is layered, with a small expansion coefficient when heated. Silicon dioxide is a highly active, renewable substance with a multi-microporous structure and high thermal stability, and has a strong adsorption capacity for liquid and gas phase substances. Silicon dioxide can be used as a dehumidifying desiccant, dehydrating agent, moisture-proof agent and air humidity regulator, and is also used for gas drying, as a catalyst and catalyst carrier, a reinforcing agent for silicone rubber, and a sizing agent used in the textile industry.

[0022] The CAS number of platinum complex is 68478-92-2; platinum complex is a commonly used catalyst used in the process of catalytic addition reaction of silicon and hydrogen; platinum complex has a rapid and effective effect on the addition reaction of unsaturated hydrocarbon compounds and silicon hydride compounds. It is a light-colored transparent solution with good stability, can be stored for a long time, does not turn yellow, is compatible with a variety of organic solvents, and is easily soluble in aromatic hydrocarbons, silicone oils and non-polar solvents.

[0023] See also Figure 1 As shown, in this comparative group, by using a constant value for the proportion of the platinum complex and a variable value for the proportion of methylvinyldimethyl (siloxane and polysiloxane), the proportion of silicon dioxide changes with the proportion of methylvinyldimethyl (siloxane and polysiloxane), and a total of eight groups are tested;

[0024] The first group's ratio: 19.95 parts of p-methylvinyl dimethyl; 80 parts of silicon dioxide; 0.05 parts of platinum complex;

[0025] The second group's ratio: 29.95 parts of p-methylvinyl dimethyl; 70 parts of silicon dioxide; 0.05 parts of platinum complex;

[0026] The third group's ratio: 39.95 parts of p-methylvinyl dimethyl; 60 parts of silicon dioxide; 0.05 parts of platinum complex;

[0027] The fourth group's ratio: 49.95 parts of p-methylvinyl dimethyl; 50 parts of silicon dioxide; 0.05 parts of platinum complex;

[0028] The fifth group's ratio: 59.95 parts of p-methylvinyl dimethyl; 40 parts of silicon dioxide; 0.05 parts of platinum complex;

[0029] The sixth group's ratio: 69.95 parts of p-methylvinyl dimethyl; 30 parts of silicon dioxide; 0.05 parts of platinum complex;

[0030] The proportion of the seventh group: 79.95 parts of p-methylvinyl dimethyl; 20 parts of silicon dioxide; 0.05 parts of platinum complex;

[0031] The proportions of the eighth group: 89.95 parts of p-methylvinyl dimethyl; 10 parts of silicon dioxide; and 0.05 parts of platinum complex.

[0032] By observing the above groups of different proportions of liquid glue, the following is the situation:

[0033] Group 1: no odor, extremely poor flow properties, excellent strength properties, and not a single color;

[0034] The second group: no odor, poor flow performance, strong strength performance, and not a single color;

[0035] Group 3: no odor, poor flow properties, strong strength, single color;

[0036] Group 4: no odor, average flowability, strong strength, single color;

[0037] Group 5: no odor, good flowability, strong strength, single color;

[0038] Group 6: no odor, good flowability, average strength, single color;

[0039] Group 7: no odor, good flowability, poor strength, single color;

[0040] Group 8: Slight odor, good fluidity, poor strength performance, and single color.

[0041] From the above observation results, it can be seen that: the first, second and third groups are not suitable as liquid glue because they have no odor but poor flow properties; the fourth, fifth, sixth and seventh groups are suitable as liquid glue because they have no odor and their flow properties, strength properties and color can meet the requirements; the eighth group is not suitable as liquid glue because it has a slight odor and poor strength properties; therefore, the range of the value of the portion of methyl vinyl dimethyl (siloxane and polysiloxane) is: 49.95 parts-79.95 parts.

[0042] See also Figure 2 As shown, in this comparative group, by using a constant value for the proportion of the platinum complex and a variable value for the proportion of methylvinyldimethyl (siloxane and polysiloxane), the proportion of silicon dioxide changes with the proportion of methylvinyldimethyl (siloxane and polysiloxane), and a total of eight groups are tested;

[0043] The ninth group's ratio: 45 parts of p-methylvinyl dimethyl; 54.95 parts of silicon dioxide; 0.05 parts of platinum complex;

[0044] The tenth group's proportions: 50 parts of p-methylvinyl dimethyl; 49.95 parts of silicon dioxide; 0.05 parts of platinum complex;

[0045] The proportion of the eleventh group: 55 parts of p-methylvinyl dimethyl; 44.95 parts of silicon dioxide; 0.05 parts of platinum complex;

[0046] The proportion of the twelfth group: 60 parts of p-methylvinyl dimethyl; 39.95 parts of silicon dioxide; 0.05 parts of platinum complex;

[0047] The proportion of the thirteenth group: 65 parts of p-methylvinyl dimethyl; 34.95 parts of silicon dioxide; 0.05 parts of platinum complex;

[0048] The ratio of the fourteenth group: 70 parts of p-methylvinyl dimethyl; 29.95 parts of silicon dioxide; 0.05 parts of platinum complex;

[0049] The proportion of the fifteenth group: 75 parts of p-methylvinyl dimethyl; 24.95 parts of silicon dioxide; 0.05 parts of platinum complex;

[0050] The formulation of the sixteenth group: 80 parts of p-methylvinyl dimethyl; 19.95 parts of silicon dioxide; and 0.05 parts of platinum complex.

[0051] By observing the above groups of different proportions of liquid glue, the following is the situation:

[0052] Group 9: no odor, poor flow properties, strong strength, single color;

[0053] Group 10: no odor, average flowability, strong strength, single color;

[0054] Group 11: no odor, good flowability, strong strength, single color;

[0055] Group 12: no odor, good flowability, strong strength, single color;

[0056] Group 13: No odor, good flowability, strong strength, single color;

[0057] Group 14: no odor, good flowability, average strength, single color;

[0058] Group 15: no odor, good flowability, average strength, single color;

[0059] Group 16: No odor, good flowability, poor strength, and single color.

[0060] From the above observation results, it can be seen that: the first group is not suitable as liquid glue because it has no odor but poor flowability; the second, third, fourth, fifth, sixth, seventh and eighth groups are suitable as liquid glue because they have no odor and their flowability, strength and color can meet the requirements; therefore, the range of the value of the portion of methylvinyl dimethyl (siloxane and polysiloxane) is: 50 parts-79.95 parts; among them, preferably, the portion of methylvinyl dimethyl (siloxane and polysiloxane) is 65 parts.

[0061] See also Figure 3 As shown, in this comparative group, by using a constant value for the proportion of p-methylvinyl dimethyl (siloxane and polysiloxane); using a variable value for the proportion of the platinum complex, the proportion of silicon dioxide changes with the proportion of the platinum complex, and a total of eight groups are tested;

[0062] The proportion of the seventeenth group: 65 parts of p-methylvinyl dimethyl; 34.99 parts of silicon dioxide; 0.01 parts of platinum complex;

[0063] The proportion of the eighteenth group: 65 parts of p-methylvinyl dimethyl; 34.95 parts of silicon dioxide; 0.05 parts of platinum complex;

[0064] The ratio of the 19th group: 65 parts of p-methylvinyl dimethyl; 34.90 parts of silicon dioxide; 0.10 parts of platinum complex;

[0065] The proportion of the 20th group: 65 parts of p-methylvinyl dimethyl; 34.85 parts of silicon dioxide; 0.15 parts of platinum complex;

[0066] The proportion of the twenty-first group: 65 parts of p-methylvinyl dimethyl; 34.80 parts of silicon dioxide; 0.20 parts of platinum complex;

[0067] The proportion of the 22nd group: 65 parts of p-methylvinyl dimethyl; 34.75 parts of silicon dioxide; 0.25 parts of platinum complex;

[0068] The proportion of the 23rd group: 65 parts of p-methylvinyl dimethyl; 34.70 parts of silicon dioxide; 0.30 parts of platinum complex;

[0069] The formulation of the twenty-fourth group: 65 parts of p-methylvinyl dimethyl; 34.65 parts of silicon dioxide; and 0.35 parts of platinum complex.

[0070] By observing the above groups of different proportions of liquid glue, the following is the situation:

[0071] Group 17: no odor, average vulcanization, single color;

[0072] Group 18: no odor, good vulcanization, single color;

[0073] Group 19: no odor, fast vulcanization, single color;

[0074] Group 20: no odor, fast vulcanization, single color;

[0075] Group 21: No odor, fast vulcanization, and not a single color;

[0076] Group 22: No odor, fast vulcanization, and different colors;

[0077] Group 23: No odor, vulcanization is too fast, and the color is not uniform;

[0078] Group 24: No odor, vulcanization too fast, and color is not uniform.

[0079] From the above observation results, it can be seen that the seventeenth and eighteenth groups are suitable as liquid glue because they have no odor, and the vulcanization performance and color can meet the requirements; although the nineteenth to twenty-fourth groups have no odor, their vulcanization speed is fast and they are not suitable for liquid glue; therefore, the value range of the platinum complex portion is: 0.01 part-0.1 part; among them, preferably, the platinum complex portion is 0.05 part.

[0080] See also Figure 4 As shown, in this comparative group, by using a constant value for the proportion of p-methylvinyl dimethyl (siloxane and polysiloxane); using a variable value for the proportion of the platinum complex, the proportion of silicon dioxide changes with the proportion of the platinum complex, and a total of eight groups are tested;

[0081] The proportion of the 25th group: 65 parts of p-methylvinyl dimethyl; 34.945 parts of silicon dioxide; 0.055 parts of platinum complex;

[0082] The proportion of the twenty-sixth group: 65 parts of p-methylvinyl dimethyl; 34.940 parts of silicon dioxide; 0.060 parts of platinum complex;

[0083] The proportion of the twenty-seventh group: 65 parts of p-methylvinyl dimethyl; 34.935 parts of silicon dioxide; 0.065 parts of platinum complex;

[0084] The proportion of the twenty-eighth group: 65 parts of p-methylvinyl dimethyl; 34.930 parts of silicon dioxide; 0.070 parts of platinum complex;

[0085] The proportion of the twenty-ninth group: 65 parts of p-methylvinyl dimethyl; 34.925 parts of silicon dioxide; 0.075 parts of platinum complex;

[0086] The proportion of the 30th group: 65 parts of p-methylvinyl dimethyl; 34.920 parts of silicon dioxide; 0.080 parts of platinum complex;

[0087] The proportion of the 31st group: 65 parts of p-methylvinyl dimethyl; 34.915 parts of silicon dioxide; 0.085 parts of platinum complex;

[0088] The proportions of the 32nd group: 65 parts of p-methylvinyl dimethyl; 34.910 parts of silicon dioxide; and 0.090 parts of platinum complex.

[0089] By observing the above groups of different proportions of liquid glue, the following is the situation:

[0090] Group 25: no odor, good vulcanization, single color;

[0091] Group 26: no odor, good vulcanization, single color;

[0092] Group 27: no odor, good vulcanization, single color;

[0093] Group 28: no odor, good vulcanization, single color;

[0094] Group 29: no odor, general sulfur, single color;

[0095] Group 30: no odor, general vulcanization, single color;

[0096] Group 31: no odor, fast vulcanization, single color;

[0097] Group 32: No odor, fast vulcanization, single color.

[0098] From the above observation results, it can be seen that the 25th to 30th groups are suitable as liquid glue because they have no odor, and their vulcanization performance and color can meet the requirements; although the 31st to 32nd groups have no odor, their vulcanization speed is fast and they are not suitable for liquid glue; therefore, the value range of the platinum complex portion is 0.01 parts-0.08 parts; among them, preferably, the platinum complex portion is 0.05-0.075 parts.

[0099] See also Figure 1-Figure 4 As shown, in a liquid glue formula of the present invention applied to a flexible thermal insulation pad, the proportion of methylvinyldimethyl (siloxane and polysiloxane) ranges from 49.95 to 79.95 parts; the proportion of silicon dioxide ranges from 20.05 to 50.05 parts; the proportion of platinum complex ranges from 0.01 to 0.08 parts; preferably, the proportion of methylvinyldimethyl (siloxane and polysiloxane) is 65 parts; the proportion of silicon dioxide is 34.95 parts; and the proportion of platinum complex is 0.05 parts.

[0100] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0101] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A liquid glue formula for a flexible thermal insulation pad, characterized in that: include: Methylvinyl dimethyl (siloxanes and polysiloxanes), silica, and platinum complex; Among them, the proportion of the methylvinyl dimethyl (siloxane and polysiloxane) ranges from 49.95 to 79.95 parts; the proportion of the silicon dioxide ranges from 20.05 to 50.05 parts; and the proportion of the platinum complex ranges from 0.01 to 0.08 parts.

2. The liquid glue formula for flexible thermal insulation pad according to claim 1, characterized in that: The proportion of the methylvinyl dimethyl (siloxane and polysiloxane) is in the range of 59.95-69.95 parts; the proportion of the silicon dioxide is in the range of 30.05-40.05 parts; and the proportion of the platinum complex is 0.05 parts.

3. The liquid glue formula for flexible thermal insulation pad according to claim 2, characterized in that: The amount of methylvinyl dimethyl (siloxane and polysiloxane) is 65 parts; the amount of silicon dioxide is 34.95 parts; The amount of the platinum complex was 0.05 parts.