Modified calcium-based energy storage material compounded with alkali metal salt and metal oxide and preparation method of modified calcium-based energy storage material

By using composite alkali metal salt and metal oxide modification technology in calcium-based energy storage materials, the problem of sintering of calcium-based materials is solved, the cycle stability and energy storage density are improved, and the efficient CO2 adsorption effect is achieved.

CN118879286APending Publication Date: 2024-11-01NORTHEAST DIANLI UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410901236.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-05
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Calcium-based materials will sinter after multiple cycles, resulting in pore collapse and blockage, hindering CO2 from diffusion into the material and reducing the material's energy storage density.

Method used

Using composite alkali metal salts and metal oxides to modify calcium-based energy storage materials, the alkali metal sulfate and alkali metal chloride salt are mixed as a promoter and together with calcium oxide as a modified material to form coordination compounds to increase volume Expansion and delay sintering, and metal oxides are introduced as stabilizers, and prepared by wet mixing, sonication and heat treatment.

Benefits of technology

It improves the circulation stability and energy storage density of the material, extends the service life of the material, and significantly improves the adsorption performance of calcium oxide.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118879286A_ABST
    Figure CN118879286A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of thermochemical energy storage materials, and discloses a modified calcium-based energy storage material compounded with alkali metal salt and metal oxide and a preparation method of the modified calcium-based energy storage material. The modified calcium-based energy storage material is prepared from the following raw materials in percentage by mass: 10-30% of composite alkali metal salt, 10-30% of metal oxide and the balance of calcium oxide, totaling 100%, the composite alkali metal salt is a mixture of alkali metal sulfate and alkali metal chlorate. Alkali metal sulfate and alkali metal chlorate are added in a compounding mode, so that the alkali metal sulfate and the alkali metal chlorate can form a coordination compound with calcium oxide in the circulation process, calcium oxide is modified, meanwhile, the volume of the material is expanded, and the conversion rate of the material is increased; the alkali metal sulfate and the alkali metal chlorate can reduce the viscosity of the material and delay the sintering phenomenon of the calcium-based material in the circulation process; and the modified calcium-based energy storage material prepared by the invention has good cycle stability and energy storage density.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of thermochemical energy storage materials, and in particular to a modified calcium-based energy storage material of a composite alkali metal salt and a metal oxide and a preparation method thereof. Background Art

[0002] The increasing content of CO2 in the atmosphere has caused a series of environmental problems. In order to capture and utilize CO2 in the atmosphere, calcium cycle technology has great potential value in CO2 capture, utilization and storage due to its rich content and low cost.

[0003] Typically, calcium cycle technology uses two reactors to capture and release carbon dioxide at high temperatures. In the first reactor, quicklime is used as an adsorbent to capture carbon dioxide from the gas stream to form slaked lime, that is, calcium carbonate. The slaked lime is then transported to the second reactor and regenerated in the second reactor to produce lime and pure carbon dioxide. Finally, the quicklime is recycled back to the first reactor. That is, the calcium cycle is carried out in two steps. First, the calcium-based material absorbs CO2 and releases heat between 650°C and 950°C, and releases CO2 and absorbs heat above 950°C.

[0004] However, calcium-based materials will sinter after multiple cycles, causing pore collapse and blockage, hindering the diffusion of CO2 into the material, inhibiting the reaction, and thus reducing the material's energy storage density. Therefore, the poor adsorption performance of ordinary calcium oxide particles is also a key factor affecting the direct use of natural calcium oxide.

[0005] To this end, the present invention provides a modified calcium-based energy storage material of a composite alkali metal salt and a metal oxide and a preparation method thereof. Summary of the invention

[0006] In order to solve the above-mentioned deficiencies in the prior art, the present invention provides a modified calcium-based energy storage material of a composite alkali metal salt and a metal oxide and a preparation method thereof.

[0007] The modified calcium-based energy storage material of a composite alkali metal salt and a metal oxide and the preparation method thereof of the present invention are achieved by the following technical scheme:

[0008] The first object of the present invention is to provide a modified calcium-based energy storage material based on a composite alkali metal salt and a metal oxide, wherein the raw materials for preparing the material are composed of the following mass percentages:

[0009] 10% to 30% of composite alkali metal salt, 10% to 30% of metal oxide, and the rest is calcium oxide, totaling 100%.

[0010] Wherein, the composite alkali metal salt is a mixture of alkali metal sulfate and alkali metal chloride.

[0011] In some preferred embodiments of the present invention, the alkali metal sulfate is one or more of lithium sulfate, sodium sulfate and potassium sulfate.

[0012] In some preferred embodiments of the present invention, the alkali metal chloride is one or both of sodium chloride and potassium chloride.

[0013] In some preferred embodiments of the present invention, the molar mass ratio of the calcium oxide to the composite alkali metal salt is 2 to 20:1.

[0014] In some preferred embodiments of the present invention, in the composite alkali metal salt, the alkali metal sulfate accounts for 10% to 90% of the total molar amount of the composite alkali metal salt, the alkali metal chloride accounts for 10% to 90% of the total molar amount of the composite alkali metal salt, and the sum of the molar amounts of the alkali metal sulfate and the alkali metal chloride is 100%.

[0015] In some preferred embodiments of the present invention, the metal oxide is any one of zinc oxide, magnesium oxide, manganese oxide, zirconium oxide, cerium oxide, copper oxide, iron oxide, and aluminum oxide.

[0016] The second object of the present invention is to provide a method for preparing the modified calcium-based energy storage material of the above-mentioned composite alkali metal salt and metal oxide, comprising the following steps:

[0017] Step 1: Grind the composite alkali metal salt to obtain composite alkali metal salt powder.

[0018] Step 2, weigh calcium oxide, metal oxide and composite alkali metal salt powder according to the following mass percentage components and set aside:

[0019] 10% to 30% of composite alkali metal salt, 10% to 30% of metal oxide, and the rest is dried calcium oxide, totaling 100%.

[0020] Step 3, the weighed composite alkali metal salt powder, dried calcium oxide and metal oxide are wet-mixed, ultrasonically treated, and then dried, heat-treated and ground to obtain the modified calcium-based energy storage material of the composite alkali metal salt and metal oxide.

[0021] In some preferred embodiments of the present invention, the heat treatment time is 400° C. to 600° C., and the treatment time is 1 h to 3 h.

[0022] In some preferred embodiments of the present invention, when the composite alkali metal salt is ground, it is ground to pass through a 400-mesh sieve.

[0023] In some preferred embodiments of the present invention, when the heat-treated product is ground, it is ground to pass through a 400-mesh sieve.

[0024] In some preferred embodiments of the present invention, the drying temperature is 100° C. to 150° C., and the treatment time is 6 h to 12 h.

[0025] In some preferred embodiments of the present invention, the ultrasonic frequency of the ultrasonic treatment is 40 KHz, and the treatment time is 0.5 h to 2 h.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] The calcium-based energy storage material modified by the composite alkali metal salt and metal oxide provided by the present invention can make the material have good cycle stability and energy storage density.

[0028] The calcium oxide used in the present invention is common commercial calcium oxide, all alkali metal salts are common salts, the preparation method adopted is a wet mixing method, and the preparation process is simple. The addition of alkali metal salts improves the material conversion rate, and the addition of metal oxides can improve the material sintering problem, and improve the cycle stability and service life of the material. There is a synergistic effect between the composite alkali metal salt and the metal oxide, so that the energy storage material has good stability and high energy storage density under long-term operation.

[0029] The present invention provides a new approach for developing efficient and stable calcium-based energy storage materials, which have good cycle stability and high energy storage density.

[0030] The present invention is based on calcium oxide, and first adds a composite alkali metal salt to improve the conversion rate of the material. When the mass ratio of the composite alkali metal salt to calcium oxide is 1:3, the initial conversion rate of the material is 0.85373, which is 51.8% higher than that of pure calcium oxide. The addition of composite alkali metal salts can form coordination compounds with calcium oxide. Taking sodium sulfate and sodium chloride as an example, calcium oxide is modified with sodium sulfate and sodium chloride to obtain a composite alkali metal salt-modified calcium-based energy storage material. During the cyclic treatment process, in-situ XRD was used for testing. The results showed that during the cyclic treatment process, sodium sulfate, sodium chloride and calcium oxide produce Na2Ca(SO4)2 and Na 3.2 Ca 1.8 (SO4)3Cl 0.8 The generation of coordination compounds can expand the volume, produce a popcorn effect, and promote the reaction. However, the addition of alkali metal salts will also promote the sintering of materials. When metal oxides are introduced, this sintering phenomenon can be inhibited. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is the XRD pattern of the modified calcium-based energy storage material prepared in Example 1.

[0032] Figure 2This is the XRD pattern of the modified calcium-based energy storage material prepared in Comparative Example 2.

[0033] Figure 3 This is the SEM image of Comparative Example 1.

[0034] Figure 4 This is the SEM image of Comparative Example 2.

[0035] Figure 5 This is the SEM image of Example 1.

[0036] Figure 6 This is the SEM image of Example 2.

[0037] Figure 7 This is a conversion efficiency diagram of the energy storage materials prepared in Comparative Examples 1-2 and Examples 1-2 of the present invention.

[0038] Figure 8 This is a conversion efficiency diagram of the energy storage materials prepared in Comparative Examples 1-2 and Examples 1-4 of the present invention.

[0039] Fig. 9 This is a diagram of the energy storage density of the energy storage materials prepared in Comparative Examples 1-2 and Examples 1-2 of the present invention. DETAILED DESCRIPTION

[0040] The technical solutions in the embodiments of the present invention will be described clearly and completely below.

[0041] The present invention provides a modified calcium-based energy storage material based on a composite alkali metal salt and a metal oxide. It should be noted that the present invention takes into account that calcium oxide, as a CO2 adsorption material, will sinter after multiple cycles, hindering CO2 from diffusing internally and inhibiting the diffusion reaction stage, thereby reducing the material energy storage density. Therefore, the low adsorption performance of ordinary large-particle calcium oxide is also a key factor affecting the direct utilization of natural calcium oxide. In order to enhance the adsorption effect of calcium oxide, the present invention attempts to enhance the adsorption effect of calcium oxide by adding alkali metal salts. However, during the process of exploration, the inventor found that if only alkali metal sulfate is used to improve the adsorption effect of calcium oxide, due to the high viscosity of a single alkali metal sulfate, the material will sinter rapidly after the cycle. Therefore, in order to solve this technical problem, the present invention adds alkali metal sulfate and alkali metal chloride as a promoter by compounding. The added composite alkali metal salt can form a coordination compound with calcium oxide during the cyclic treatment process, thereby realizing the modification of calcium oxide. The generation of the coordination compound can expand the volume, produce a popcorn effect, promote the reaction, accelerate the reaction kinetics, and thus improve the conversion rate of the material. At the same time, compounding alkali metal sulfate and alkali metal chloride can reduce the viscosity of the material and delay the sintering phenomenon of calcium-based materials in the circulation process to a certain extent. Therefore, the present invention uses alkali metal sulfate and alkali metal chloride as composite alkali metal salts, and uses the composite alkali metal salt formed by compounding alkali metal sulfate and alkali metal chloride, metal oxide and calcium oxide as raw materials for preparing modified calcium-based energy storage materials, and it is prepared by the following steps:

[0042] Step 1: Grinding the composite alkali metal salt, that is, grinding the alkali metal sulfate and the alkali metal chloride to obtain the composite alkali metal salt powder.

[0043] It should be noted that the present invention takes into account that alkali metal sulfates and alkali metal chlorides, such as sodium sulfate and sodium chloride, are easy to deliquesce and form crystals, and their crystal blocks are not conducive to being fully mixed with other components, and the weighing of the component materials after deliquescing is inaccurate. Therefore, before weighing and mixing, the present invention first grinds and dries the composite alkali metal salt, and grinds the composite alkali metal salt into fine powder by grinding and drying, so that the composite alkali metal salt is dehydrated, so that the weighing is more accurate. And in some preferred embodiments of the present invention, it is ground to be able to pass through a 400 mesh sieve.

[0044] In some preferred embodiments of the present invention, the alkali metal sulfate used can be selected from one or more of lithium sulfate, sodium sulfate and potassium sulfate.

[0045] In some preferred embodiments of the present invention, the alkali metal chloride salt used is one or both of sodium chloride and potassium chloride.

[0046] Step 2, after drying the calcium oxide, weigh the obtained composite alkali metal salt powder and metal oxide according to the following mass percentage components for later use:

[0047] 10% to 30% of the composite alkali metal salt, 10% to 30% of the metal oxide, and the rest of the dried calcium oxide, totaling 100%, wherein the molar mass ratio of the calcium oxide to the composite alkali metal salt is 2 to 20:1.

[0048] It should be noted that the present invention takes into account that calcium oxide easily absorbs water in the air and turns into calcium hydroxide. In order to avoid that the calcium oxide used may partially turn into calcium hydroxide, the present invention first performs a drying treatment on the calcium oxide raw material before mixing the calcium oxide with other components to dehydrate the calcium hydroxide and convert the calcium hydroxide back into calcium oxide. In order to ensure that the calcium hydroxide is completely dehydrated, in some preferred embodiments of the present invention, vacuum drying is performed at 400°C to 600°C for 1h to 3h.

[0049] In order to ensure that the dried calcium oxide can be evenly mixed with the composite alkali metal salt powder, the metal oxide and water, in some preferred embodiments of the present invention, during the ultrasonic treatment, the ultrasonic frequency is 40 kHz and the ultrasonic time is 0.5 h to 2 h.

[0050] Calcium oxide is mixed with composite alkali metal salt powder and metal oxide by wet mixing. In some preferred embodiments of the present invention, water is used as a mixing aid, calcium oxide is mixed with composite alkali metal salt powder and metal oxide in water, and the ratio of water to calcium oxide is 15mL-30mL:1.4g.

[0051] In order to avoid the effect of reducing the overall energy storage density of the material due to adding too much or too little composite alkali metal salt, the amount of composite alkali metal salt added in the present invention is 10% to 30% of the mass of the overall energy storage material.

[0052] In order to promote the synergistic relationship between alkali metal sulfate and alkali metal chloride in reducing viscosity and melting point, in some preferred embodiments of the present invention, in the composite alkali metal salt, the alkali metal sulfate accounts for 10% to 90% of the total molar amount of the composite alkali metal salt, the alkali metal chloride accounts for 10% to 90% of the total molar amount of the composite alkali metal salt, and the sum of the molar amounts of the alkali metal sulfate and the alkali metal chloride is 100%.

[0053] In order to avoid the problem of calcium oxide being easily deactivated during high-temperature cycling, the present invention further improves the sintering problem of the sintered material and adds metal oxides. The metal oxides are inert carriers with high melting points and can serve as atomic skeletons to stabilize the microstructure of the calcium-based adsorbent, delaying the growth of grains and the closure of pores, increasing the cyclic stability of the calcium-based adsorbent, and thus preventing the problem of calcium oxide being easily deactivated during high-temperature cycling.

[0054] In order to ensure that the problem of calcium oxide being easily deactivated during high-temperature cycling can be prevented by the added metal oxide, in other preferred embodiments of the present invention, the metal oxide used is selected from any one of zinc oxide, magnesium oxide, manganese oxide, zirconium oxide, cerium oxide, copper oxide, iron oxide, and aluminum oxide.

[0055] In order to avoid the effect of adding too much or too little metal oxide, which will cause the overall energy storage density of the material to decrease, the amount of metal oxide added in the present invention is 10% to 30% of the mass of the overall energy storage material.

[0056] Based on the above, the present invention adds composite alkali metal salts and metal oxides as modifiers of calcium oxide on the basis of calcium oxide, wherein the metal oxide is an inert carrier with a high melting point temperature, which can be used as an atomic skeleton to stabilize the microstructure of the calcium-based adsorbent, delaying the growth of grains and the closure of pores, and increasing the cyclic stability of the calcium-based adsorbent. Alkali metal salts can effectively improve the reaction kinetics as promoters. In addition, the lattice constant of the coordination compound should be large, and the formation of the coordination compound will produce a popcorn effect, resulting in volume expansion, which is beneficial to the transportation and transfer of CO2. The combined action of alkali metal salts and metal oxides allows the material to have good cyclic stability while maintaining a high conversion rate.

[0057] Step 3, the weighed composite alkali metal salt powder, dried calcium oxide, and metal oxide are wet-mixed, ultrasonically treated, and then dried, heat-treated, and then ground to obtain the modified calcium-based energy storage material of the composite alkali metal salt and metal oxide.

[0058] In order to remove moisture during the uniform mixing process, in some preferred embodiments of the present invention, the product obtained by ultrasonic treatment is dried at a temperature of 100° C. to 150° C. and a treatment time of 6 to 12 h.

[0059] The present invention takes into account that after drying, calcium oxide and water will react to form calcium hydroxide. At this time, the water that has reacted with the calcium oxide cannot be removed at a drying temperature of 100 to 150° C. Therefore, in some preferred embodiments of the present invention, the product after drying is heat treated at a high temperature of 400 to 600° C. to cause the calcium hydroxide to undergo a decomposition reaction to remove water, so that the calcium hydroxide is converted into calcium oxide, and the treatment time of the heat treatment is 1 to 3 hours.

[0060] The present invention takes into account that agglomeration may occur during the heat treatment process, resulting in agglomeration of the mixed material. Therefore, in some preferred embodiments of the present invention, when the product after the heat treatment is ground, it is ground to 400 mesh and sieved to obtain a granular or powdery modified calcium-based energy storage material based on a composite alkali metal salt and a metal oxide with uniform components.

[0061] Example 1

[0062] This embodiment provides a modified calcium-based energy storage material based on a composite alkali metal salt and a metal oxide, and the modified calcium-based energy storage material is prepared by the following steps:

[0063] Step 1: Grind sodium sulfate and sodium chloride separately, and pass through a 400-mesh sieve to obtain sodium sulfate powder and sodium chloride powder.

[0064] Step 2: Place the purchased analytically pure calcium oxide in a vacuum drying oven at 100° C. and dry for 4 hours to obtain dried calcium oxide.

[0065] Step 3, weigh 1.4g of calcium oxide, 0.3295g of sodium sulfate, 0.1566g of sodium chloride, and 0.2035g of zinc oxide. At this time, the molar ratio of calcium oxide to the composite alkali metal salt is 5:1, sodium sulfate accounts for 46.4% of the total molar amount of the composite alkali metal salt; sodium chloride accounts for 53.6% of the total molar amount of the composite alkali metal salt.

[0066] Step 4, after mixing the above materials, place them in 20 mL of deionized water to mix well, then ultrasonically stir them at an ultrasonic frequency of 40 kHz for 2 hours, then place them in a vacuum drying oven at 120°C for 12 hours, and then place the dried product in a tube furnace and heat treat it at 500°C under vacuum for 2 hours. Grind the heat-treated material until it passes through a 400-mesh sieve to obtain a modified calcium-based energy storage material of a composite alkali metal salt and a metal oxide.

[0067] Example 2

[0068] This embodiment provides a modified calcium-based energy storage material based on a composite alkali metal salt and a metal oxide, and the modified calcium-based energy storage material is prepared by the following steps:

[0069] Step 1: Grind sodium sulfate and sodium chloride separately, and pass through a 400-mesh sieve to obtain sodium sulfate powder and sodium chloride powder.

[0070] Step 2: Place the purchased analytically pure calcium oxide in a vacuum drying oven at 100° C. and dry for 4 hours to obtain dried calcium oxide.

[0071] Step 3, weigh 1.4g of calcium oxide, 0.3295g of sodium sulfate, 0.1566g of sodium chloride, and 0.814g of zinc oxide. At this time, the molar ratio of calcium oxide to the composite alkali metal salt is 5:1, sodium sulfate accounts for 46.4% of the total molar amount of the composite alkali metal salt; sodium chloride accounts for 53.6% of the total molar amount of the composite alkali metal salt.

[0072] Step 4, after mixing the above materials, place them in 20 mL of deionized water to mix well, then ultrasonically stir them at an ultrasonic frequency of 40 kHz for 2 hours, then place them in a vacuum drying oven at 120°C for 12 hours, and then place the dried product in a tube furnace and heat treat it at 500°C under vacuum for 2 hours. Grind the heat-treated material until it passes through a 400-mesh sieve to obtain a modified calcium-based energy storage material of a composite alkali metal salt and a metal oxide.

[0073] Example 3

[0074] This embodiment provides a modified calcium-based energy storage material based on a composite alkali metal salt and a metal oxide, and the modified calcium-based energy storage material is prepared by the following steps:

[0075] Step 1: Grind sodium sulfate and sodium chloride separately, and pass through a 400-mesh sieve to obtain sodium sulfate powder and sodium chloride powder.

[0076] Step 2: Place the purchased analytically pure calcium oxide in a vacuum drying oven at 100° C. and dry for 4 hours to obtain dried calcium oxide.

[0077] Step 3, weigh 1.4g of calcium oxide, 0.16g of sodium sulfate, 0.08g of sodium chloride, and 0.7g of zinc oxide. At this time, the molar ratio of calcium oxide to the composite alkali metal salt is 10:1, sodium sulfate accounts for 45.1% of the total molar amount of the composite alkali metal salt; sodium chloride accounts for 54.9% of the total molar amount of the composite alkali metal salt.

[0078] Step 4, mix the above materials and place them in 20 mL of deionized water to mix well, then ultrasonically stir them at an ultrasonic frequency of 40 kHz for 2 hours, then place them in a vacuum drying oven at 120°C for 12 hours, and then place the dried product in a tubular furnace and heat treat it at 500°C under vacuum for 2 hours. Grind the heat-treated material until it passes through a 400-mesh sieve to obtain a modified calcium-based energy storage material of a composite alkali metal salt and a metal oxide.

[0079] Example 4

[0080] This embodiment provides a modified calcium-based energy storage material based on a composite alkali metal salt and a metal oxide, and the modified calcium-based energy storage material is prepared by the following steps:

[0081] Step 1: Grind sodium sulfate and sodium chloride separately, and pass through a 400-mesh sieve to obtain sodium sulfate powder and sodium chloride powder.

[0082] Step 2: Place the purchased analytically pure calcium oxide in a vacuum drying oven at 100° C. and dry for 4 hours to obtain dried calcium oxide.

[0083] Step 3, weigh 1.4g of calcium oxide, 0.45g of sodium sulfate, 0.225g of sodium chloride, and 0.225g of zinc oxide. At this time, the molar ratio of calcium oxide to the composite alkali metal salt is 3.56:1, sodium sulfate accounts for 45.1% of the total molar amount of the composite alkali metal salt; sodium chloride accounts for 54.9% of the total molar amount of the composite alkali metal salt.

[0084] Step 4, mix the above materials and place them in 20 mL of deionized water to mix well, then ultrasonically stir them at an ultrasonic frequency of 40 kHz for 2 hours, then place them in a vacuum drying oven at 120°C for 12 hours, and then place the dried product in a tubular furnace and heat treat it at 500°C under vacuum for 2 hours. Grind the heat-treated material until it passes through a 400-mesh sieve to obtain a modified calcium-based energy storage material of a composite alkali metal salt and a metal oxide.

[0085] Comparative Example 1

[0086] This comparative example provides a calcium-based energy storage material, which is prepared by the following steps:

[0087] The purchased analytically pure calcium oxide was placed in a vacuum drying oven at 100° C. for 4 hours to obtain dried calcium oxide, which was directly used as a calcium-based energy storage material.

[0088] That is, the difference between this comparative example and Example 1 is only that:

[0089] No zinc oxide, sodium sulfate or sodium chloride added.

[0090] Comparative Example 2

[0091] This comparative example provides a modified calcium-based energy storage material of a composite alkali metal salt, and the modified calcium-based energy storage material is prepared by the following steps:

[0092] Step 1: Grind sodium sulfate and sodium chloride separately, and pass through a 400-mesh sieve to obtain sodium sulfate powder and sodium chloride powder.

[0093] Step 2: Place the purchased analytically pure calcium oxide in a vacuum drying oven at 100° C. and dry for 4 hours to obtain dried calcium oxide.

[0094] Step 3, weigh 1.4g of calcium oxide, 0.3295g of sodium sulfate, and 0.1566g of sodium chloride. At this time, the molar ratio of calcium oxide to the composite alkali metal salt is 5:1, sodium sulfate accounts for 46.4% of the total molar amount of the composite alkali metal salt; sodium chloride accounts for 53.6% of the total molar amount of the composite alkali metal salt.

[0095] Step 4, mix the above materials and place them in 20 mL of deionized water to mix well, then ultrasonically stir them at an ultrasonic frequency of 40 kHz for 2 hours, then place them in a vacuum drying oven at 120°C for 12 hours, and then place the dried product in a tubular furnace and heat treat it at 500°C under vacuum for 2 hours. Grind the heat-treated material until it passes through a 400-mesh sieve to obtain a modified calcium-based energy storage material of a composite alkali metal salt and a metal oxide.

[0096] That is, the difference between this comparative example and Example 1 is only that:

[0097] No zinc oxide added.

[0098] Experimental Section

[0099] (I) XRD test

[0100] The present invention takes the modified calcium-based energy storage material prepared in Example 1 and Comparative Example 2 as an example, and performs XRD test on the material obtained at 800°C during the cycle treatment process, and the test results are as follows: Figure 1 and Figure 2 shown.

[0101] in, Figure 1 XRD pattern of the modified calcium-based energy storage material prepared in Example 1; Figure 2 is the XRD pattern of the modified calcium-based energy storage material prepared in Comparative Example 2. Figure 1 and Figure 2 It can be seen that in the circulation process, sodium sulfate, sodium chloride and calcium oxide produce Na2Ca(SO4)2 and Na 3.2 Ca 1.8 (SO4)3Cl 0.8 The generation of coordination compounds can expand the volume, produce a popcorn effect, and promote the reaction. However, the addition of alkali metal salts will also promote the sintering of materials. When metal oxides are introduced, this sintering phenomenon can be inhibited.

[0102] (ii) SEM test

[0103] The present invention takes the energy storage materials prepared in Comparative Example 1, Comparative Example 2, and Examples 1-2 as examples, and performs SEM tests on the materials obtained after 80 cycles of treatment, and the test results are as follows: Figure 3-6 shown.

[0104] Figure 3is the SEM picture of Comparative Example 1, Figure 4 This is the SEM picture of Comparative Example 2. Figure 5 is the SEM picture of Example 1, Figure 6 This is the SEM image of Example 2.

[0105] And by Figure 3-6 It can be seen that the addition of composite alkali metal salts and metal oxides enables the material to maintain a rich porous structure after multiple cycles, which facilitates the material to absorb CO2 and significantly improves the recycling conversion rate of the material.

[0106] (III) Cyclic stability test

[0107] The present invention takes the energy storage materials prepared in Comparative Example 1, Comparative Example 2, and Examples 1-4 as examples, and tests the conversion efficiency thereof respectively, and the test results are as follows: Figure 7 and Figure 8 shown.

[0108] Figure 7 The conversion efficiency diagram of the energy storage materials prepared in Comparative Example 1, Comparative Example 2 and Examples 1-2 is shown. Figure 7 It can be seen that after eighty cycles of testing, the effective conversion rate of comparative example 1 is 21%, the effective conversion rate of comparative example 2 is 44%, the effective conversion rate of embodiment 1 is 57%, and the effective conversion rate of embodiment 2 is 80%.

[0109] Among them, by comparing the test results of Example 1 with those of Comparative Example 1, it can be seen that when the dried calcium oxide is directly used as the calcium-based energy storage material, its effective conversion rate is much lower than the effective conversion rate of Example 1, indicating that the present invention can significantly improve the conversion efficiency of the energy storage material by adding composite alkali metal salts and metal oxides.

[0110] Compared with comparative example 2, the 80th conversion efficiency of Example 1 and Example 2 increased by 28.1% and 79.95% respectively. This shows that the preparation method of the present invention can effectively improve the conversion efficiency and cycle stability of calcium oxide. Figure 3-6 The results are consistent.

[0111] Figure 8 The conversion efficiency diagram of the energy storage materials prepared in Comparative Examples 1-2 and Examples 1-4 of the present invention. Figure 8It can be seen that the ratio of the composite alkali metal salt and the metal oxide has a certain effect on its conversion rate, and the increase in the proportion of the composite alkali metal salt will increase the initial conversion rate of the material, but as the number of cycles increases, the subsequent conversion rate of the material will decrease, and the more the proportion of the composite alkali metal salt, the more obvious this reduction effect; the presence of metal oxides can improve the cyclic stability of the material, and as the proportion of metal oxides increases, the cyclic stability of the material is better. Preferably, the present invention performs eighty cycles of test analysis on the energy storage materials prepared by Comparative Example 1, Comparative Example 2, and Examples 1-2.

[0112] (IV) Energy storage density test

[0113] The present invention takes the energy storage materials prepared in Comparative Example 1, Comparative Example 2, and Examples 1-2 as examples, and tests the energy storage density thereof respectively, and the test results are as follows: Fig. 9 shown.

[0114] And by Fig. 9 It can be seen that after eighty cycles of testing, the energy storage density of comparative example 1 is 1429.3 J / g, the energy storage density of comparative example 2 is 1923.6 J / g, the energy storage density of embodiment 1 is 2056.6 J / g, and the energy storage density of embodiment 2 is 2096.6 J / g. Among them, by comparing the test results of embodiment 1 with comparative example 1, it can be seen that when the dried calcium oxide is directly used as the calcium-based energy storage material, its energy storage density is much lower than the energy storage density of embodiment 1, indicating that the present invention can significantly improve the energy storage density of the energy storage material by adding composite alkali metal salts and metal oxides.

[0115] Compared with comparative example 2, the 80th energy storage density of Example 1 and Example 2 increased by 6.91% and 8.41% respectively, indicating that the energy storage density of the material can be increased by the preparation method of the present invention.

[0116] Based on the above, it can be seen that when ordinary calcium oxide in Comparative Example 1 adsorbs CO2, it will first react on the surface to form CaCO3, which hinders the internal reaction of CO2. Moreover, calcium-based energy storage materials will have the problem of high-temperature sintering, and long-term high-temperature environment will cause the material to be deactivated. Therefore, the smaller the particles of calcium oxide and the higher the specific surface area, the better the adsorption effect on CO2. The present invention adopts a composite alkali metal salt as a promoter and a metal oxide as a stabilizer. The prepared calcium-based energy storage material improves the adsorption performance while ensuring that the material has good stability and high energy storage density under long-term work. Good cycle stability is specifically reflected in the cycle conversion rate. The cycle conversion rate is the CO2 that can be absorbed per unit of calcium oxide. The more stable the material conversion rate after multiple cycles, the more stable the adsorption effect of calcium oxide in the material on CO2.

[0117] Obviously, the above embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

Claims

1. A modified calcium-based energy storage material based on a composite alkali metal salt and a metal oxide, It is characterized in that The raw materials for its preparation are composed of the following components in percentage by weight: 10% to 30% of composite alkali metal salt, 10% to 30% of metal oxide, and the rest is calcium oxide, totaling 100%; Wherein, the composite alkali metal salt is a mixture of alkali metal sulfate and alkali metal chloride.

2. The modified calcium-based energy storage material according to claim 1, It is characterized in that The alkali metal sulfate is one or more of lithium sulfate, sodium sulfate and potassium sulfate.

3. The modified calcium-based energy storage material according to claim 1, It is characterized in that The alkali metal chloride is one or both of sodium chloride and potassium chloride.

4. The modified calcium-based energy storage material according to claim 1, It is characterized in that The molar ratio of the calcium oxide to the composite alkali metal salt is 2 to 20:

1.

5. The modified calcium-based energy storage material according to claim 1, It is characterized in that In the composite alkali metal salt, the alkali metal sulfate accounts for 10% to 90% of the total molar amount of the composite alkali metal salt, the alkali metal chloride accounts for 10% to 90% of the total molar amount of the composite alkali metal salt, and the sum of the molar amounts of the alkali metal sulfate and the alkali metal chloride is 100%.

6. The modified calcium-based energy storage material according to claim 1, It is characterized in that The metal oxide is any one of zinc oxide, magnesium oxide, manganese oxide, zirconium oxide, cerium oxide, copper oxide, iron oxide and aluminum oxide.

7. A method for preparing the modified calcium-based energy storage material according to any one of claims 1 to 6, It is characterized in that The following steps are involved: Grinding the composite alkali metal salt to obtain composite alkali metal salt powder; Calcium oxide, metal oxide and the composite alkali metal salt powder are weighed according to the following mass percentage components and set aside: 10% to 30% of composite alkali metal salt powder, 10% to 30% of metal oxide, and the rest is dried calcium oxide, totaling 100%; The weighed composite alkali metal salt powder, dried calcium oxide and metal oxide are wet mixed and then ultrasonically treated, and then dried, heat treated and ground to obtain the modified calcium-based energy storage material of the composite alkali metal salt and metal oxide.

8. The preparation method according to claim 7, It is characterized in that The heat treatment time is 400° C. to 600° C., and the treatment time is 1 hour to 3 hours.

9. The preparation method according to claim 7, It is characterized in that When the composite alkali metal salt is ground, it is ground until it passes through a 400-mesh sieve.