Preparation method of high-resolution high-viscosity fluorescent polyacrylamide
By preparing high-component high-viscosity fluorescent polyacrylamide, the problems of poor salt resistance and poor recovery in oil fields are solved, efficient oil-water separation and flood control concentration detection are achieved, and oil production efficiency is improved.
Patent Information
- Application Number
- CN202410898921.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-11-01
AI Technical Summary
The existing polyacrylamide has poor salt resistance when adjusting and discharging oil in oil fields, resulting in poor recovery rate and the inability to accurately determine the concentration of the discharging agent, which affects the oil field's sewage mineralization and offshore oil production efficiency.
The preparation method of high-component high-viscosity fluorescent polyacrylamide is adopted. By adding 2-acrylamide-2-methylpropanesulfonic acid and fluorescent monomer, isophthalyl chloride and N,N-dimethylformamide, use The composite initiator system and carrier form a three-dimensional network structure to improve the molecular weight and salt resistance of the polymer, and add fluorescent monomers during the polymerization process to achieve online detection and adjustment of the drive concentration.
It improves the temperature, salt resistance and oil-repellent resistance of polyacrylamide, enhances the oil-water separation ability, realizes accurate detection and adjustment of the concentration of the mixing of the drive, and improves the oil production efficiency.
Smart Images

Figure CN118879296A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of polymer synthesis, and in particular to a method for preparing high-resolution and high-viscosity fluorescent polyacrylamide. Background Art
[0002] In the process of oil extraction, polymer flooding is mainly carried out by utilizing the viscosity-increasing property of polyacrylamide on water. With the increasing discharge of oilfield wastewater, the mineralization degree of oilfield wastewater is also continuously increasing, making the effect of ordinary polyacrylamide flooding worse and worse. In addition, offshore oil production has entered a period of higher water content, and polymers are needed to adjust the profile and plug water to increase the recovery rate. At the same time, it is impossible to use a large amount of clean water to prepare polymers in offshore oil production. Therefore, seawater is mostly used to prepare polymers in the existing technology.
[0003] After being injected into the oil layer along with the commonly used polymer solution in the oil field, the concentration of polyacrylamide microspheres cannot be accurately measured using methods such as starch-cadmium iodide method, chemiluminescence nitrogen determination method, and organic carbon content method because polyacrylamide contains the same amide functional group as the polymer solution. Fluorescent substances can be used as tracers for fast, simple, and highly sensitive fluorescence analysis, which makes it possible to accurately detect and automatically control the concentration of production water injection systems.
[0004] However, if seawater is used to prepare polymers, salt-resistant polyacrylamide must be used. However, ordinary polyacrylamide has poor temperature and salt resistance. Therefore, it is necessary to develop a fluorescent tracer displacement agent for oil fields with good salt resistance and good profile control and oil recovery effects. While achieving excellent profile control and oil recovery effects, it can also achieve the purpose of being able to detect and adjust the concentration of the displacement agent online. Summary of the invention
[0005] The embodiment of the present application provides a method for preparing high-resolution and high-viscosity fluorescent polyacrylamide to solve the problems in the related art of poor anti-salt performance of polyacrylamide profile control and oil recovery, poor crude oil recovery rate, and inability to measure profile control agents.
[0006] The present application provides a method for preparing high-resolution and high-viscosity fluorescent polyacrylamide, which comprises the following steps:
[0007] S1. Preparation of fluorescent monomers:
[0008] S2, prepare a polymerization monomer aqueous solution: according to mass parts, dissolve 1-5 parts of fluorescent monomer, 20-50 parts of acrylamide, 5-10 parts of acrylic acid, 1-5 parts of 2-acrylamide-2-methylpropanesulfonic acid in 30-70 parts of deionized water, add sodium hydroxide solution, adjust the pH to 6.8-7.2, add 0.1-0.5 parts of complexing agent, 0.1-0.5 parts of chain transfer agent, to obtain a polymerization monomer aqueous solution;
[0009] S3, polymerization reaction: transferring the polymerization monomer aqueous solution to a reactor, adding isophthaloyl chloride accounting for 10% of the mass of the acrylamide, and N,N-dimethylformamide or triethylamine accounting for 1% of the mass of the acrylamide, continuously passing nitrogen into the reactor for 0.5 to 1 hour, adding a composite initiator system, reacting for 4 to 6 hours, and obtaining a polymer block;
[0010] The composite initiator system comprises:
[0011] The invention comprises, by weight, 30 to 40 parts of an azo compound, 30 to 50 parts of an oxidant, and 30 to 40 parts of a reducing agent, wherein the oxidant is selected from diisopropyl peroxydicarbonate;
[0012] S4, loading and compounding: stirring the polymer block at 25-45° C., adding a loading agent accounting for 10-20% of the mass of the polymer block, stirring and mixing for 2-4 hours, and continuously introducing nitrogen into the reactor for 0.5-1 hour to obtain a loaded polymer block, wherein the loading agent includes 70-80% by mass of poly 3-hydroxyalkanoate (PHA) and 20-30% by mass of a composite catalyst;
[0013] S5. Hydrolyze to obtain the finished product: Cut the loaded polymer block obtained in S4 into pieces, add caustic soda and mix, and hydrolyze for 2 to 3 hours. Dry and crush the obtained product to obtain high-score and high-viscosity fluorescent polyacrylamide.
[0014] Preferably, the step S1 comprises the following steps:
[0015] S101, fully stirring 4-bromo-1,8-naphthalene dicarboxylic anhydride, n-propylamine and anhydrous ethanol and refluxing them at an oil bath temperature of 80° C. for 6 hours, freezing the product for 5 hours, filtering and washing, and drying the filtrate to obtain a first intermediate product;
[0016] S102, the first intermediate product, N-methylpiperazine and ethylene glycol methyl ether are fully stirred and refluxed at an oil bath temperature of 150° C. for 12 hours, and the solvent is evaporated off by reduced pressure distillation after the reaction is completed. The product is placed in a refrigerator for 5 hours, filtered and washed, and the filtrate is dried to obtain a second intermediate product;
[0017] S103. The second intermediate product, allyl chloride and an appropriate amount of dimethylformamide are fully stirred and refluxed at a water bath temperature of 50°C for 10 hours. After the reaction is completed, the solvent is evaporated off by reduced pressure distillation. An appropriate amount of acetone is added to the product to dissolve it and the product is placed in a refrigerator for 5 hours. After filtration and washing, the filtrate is dried to obtain a fluorescent monomer.
[0018] Preferably, the mass ratio of the 4-bromo-1,8-naphthalene dicarboxylic anhydride to n-propylamine is 1.5:1 to 2:1; the mass ratio of the first intermediate product to N-methylpiperazine is 1:1 to 1:1.5; and the mass ratio of the second intermediate product to allyl chloride is 1.5:1 to 1:1.
[0019] Preferably, the composite catalyst comprises organosilane and Karstedt's catalyst, and the ratio of the organosilane to the Karstedt's catalyst is 6:1 to 3:1.
[0020] Preferably, the azo compound is selected from azobisisobutyronitrile or dimethyl azobisisobutyrate, and the added amount of the azo compound is 0.05-0.1% of the mass of the acrylamide.
[0021] Preferably, the oxidant is selected from one or more of ammonium persulfate, potassium persulfate or diisopropyl peroxydicarbonate, and the amount of the oxidant added is 0.05-0.1% of the mass of acrylamide.
[0022] Preferably, the reducing agent is one or more of sodium sulfite, sodium hypophosphite or sodium thiosulfate, and the amount of the reducing agent added is 0.04-0.1% of the mass of acrylamide.
[0023] Preferably, the complexing agent is selected from one or more of 2,2-bipyridine, sodium ethylenediaminetetramethylenephosphate or tris(2-dimethylaminoethyl)amine.
[0024] Preferably, the chain transfer agent is selected from one or more of isopropanol, isobutanol or pentaerythritol.
[0025] Preferably, the purity of the nitrogen introduced in step S3 is ≥ 99.99% and the flow rate is 60m 3 / h.
[0026] The beneficial effects of the technical solution provided by this application include:
[0027] The embodiment of the present application provides a method for preparing a high-resolution and high-viscosity fluorescent polyacrylamide, by adding a functional monomer 2-acrylamide-2-methylpropanesulfonic acid to improve the heat and salt resistance of the polymer, and by using a post-hydrolysis process to increase the molecular weight of the polymer, the oil recovery rate is increased by increasing the molecular weight and heat and salt resistance of the polyacrylamide, and the oil displacement effect of the polyacrylamide is enhanced; and a fluorescent monomer 4-(N'-methyl-1-piperazinyl)-N-propyl-1,8-naphthalene dicarboxylic acid allyl ammonium chloride is added to the polymerization system, assisted by a chain transfer agent, which is helpful for synthesizing a high molecular weight, high viscosity tracer;
[0028] Isophthaloyl chloride is introduced into the polymerization reaction, and N,N-dimethylformamide (DMF) or triethylamine is added at the same time. DMF / triethylamine is used as a solvent to promote the reaction between the amino group in acrylamide and the acyl chloride group of isophthaloyl chloride to increase the viscosity of the polymer block; then, by loading and compounding the polymer block, a three-dimensional network structure is formed between the molecular chains of poly 3-hydroxyalkanoate (PHA) and the polymer, and the stability and performance of the product are improved, thereby preparing a high-resolution and high-viscosity polyacrylamide with fluorescent properties, promoting oil-water separation, and improving oil recovery efficiency. During the injection process, the concentration of the oil displacement agent can be detected and adjusted online, and the distribution of the oil displacement agent in the formation can be accurately understood during the oil recovery process. The concentration of the oil displacement agent in the produced fluid can be timely and accurately identified and detected in the produced fluid. Therefore, the problems of poor salt resistance of polyacrylamide profile control and oil recovery, poor crude oil recovery, and inability to measure the profile control agent in the related technology can be solved. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0030] Figure 1 This is a flow chart of the method for preparing high-resolution and high-viscosity fluorescent polyacrylamide provided in an embodiment of the present application. DETAILED DESCRIPTION
[0031] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0032] The present application provides a method for preparing high-resolution and high-viscosity fluorescent polyacrylamide, which comprises the following steps:
[0033] S1. preparing fluorescent monomers.
[0034] In some embodiments, it includes the following steps:
[0035] S101. Fully stir 4-bromo-1,8-naphthalene dicarboxylic anhydride, n-propylamine and anhydrous ethanol and reflux them at an oil bath temperature of 80°C for 6 hours, freeze the product for 5 hours, filter and wash the product, and then dry the filtrate to obtain a first intermediate product; wherein the mass ratio of 4-bromo-1,8-naphthalene dicarboxylic anhydride to n-propylamine is 1.5:1 to 2:1.
[0036] S102. The first intermediate product, N-methylpiperazine and ethylene glycol methyl ether are fully stirred and refluxed at an oil bath temperature of 150°C for 12 hours. After the reaction is completed, the solvent is evaporated by reduced pressure distillation. The product is placed in a refrigerator for 5 hours. After filtration and washing, the filtrate is dried to obtain a second intermediate product; wherein the mass ratio of the first intermediate product to N-methylpiperazine is 1:1 to 1:1.5.
[0037] S103. The second intermediate product, allyl chloride and an appropriate amount of dimethylformamide are fully stirred and refluxed at a water bath temperature of 50°C for 10 hours. After the reaction is completed, the solvent is evaporated by reduced pressure distillation. An appropriate amount of acetone is added to the product to dissolve it and the product is placed in a refrigerator for 5 hours. After filtering and washing, the filtrate is dried to obtain a fluorescent monomer; wherein the mass ratio of the second intermediate product to allyl chloride is 1.5:1 to 1:1.
[0038] S2. Prepare a polymerization monomer aqueous solution: dissolve 1 to 5 parts of fluorescent monomer, 20 to 50 parts of acrylamide, 5 to 10 parts of acrylic acid, and 1 to 5 parts of 2-acrylamide-2-methylpropane sulfonic acid in 30 to 70 parts of deionized water according to mass parts, add sodium hydroxide solution, adjust the pH to 6.8 to 7.2, add 0.1 to 0.5 parts of complexing agent and 0.1 to 0.5 parts of chain transfer agent to obtain a polymerization monomer aqueous solution.
[0039] In some embodiments, the complexing agent is selected from one or more of 2,2-bipyridine, sodium ethylenediaminetetramethylenephosphate or tris(2-dimethylaminoethyl)amine.
[0040] In some embodiments, the chain transfer agent is selected from one or more of isopropanol, isobutanol, or pentaerythritol.
[0041] S3, polymerization reaction: the polymerization monomer aqueous solution is transferred to a reactor, isophthaloyl chloride accounting for 10% of the mass of the acrylamide and N,N-dimethylformamide (DMF) or triethylamine accounting for 1% of the mass of the acrylamide are added, nitrogen is continuously introduced into the reactor for 0.5 to 1 hour, a composite initiator system is added, and the reaction is carried out for 4 to 6 hours to obtain a polymer block.
[0042] In some embodiments, the composite initiator system includes, by weight, 30 to 40 parts of an azo compound, 30 to 50 parts of an oxidant, and 30 to 40 parts of a reducing agent.
[0043] In some embodiments, the azo compound is selected from azobisisobutyronitrile or dimethyl azobisisobutyrate, and the amount of the azo compound added is 0.05-0.1% of the mass of the acrylamide.
[0044] In some embodiments, the oxidant is selected from one or more of ammonium persulfate, potassium persulfate or diisopropyl peroxydicarbonate, and the amount of the oxidant added is 0.05-0.1% of the mass of acrylamide.
[0045] In some embodiments, the reducing agent is one or more of sodium sulfite, sodium hypophosphite or sodium thiosulfate, and the amount of the reducing agent added is 0.04-0.1% of the mass of acrylamide.
[0046] In some embodiments, the purity of the nitrogen introduced in step S3 is ≥ 99.99%, and the flow rate is 60m 3 / h.
[0047] S4, loading and compounding: stir the polymer block at 25-45°C, add a loading agent accounting for 10-20% of the mass of the polymer block, stir and mix for 2-4 hours, and continuously introduce nitrogen into the reactor for 0.5-1 hour to obtain a loaded polymer block, wherein the loading agent includes 70-80% by mass of poly 3-hydroxyalkanoate (PHA) and 20-30% by mass of a composite catalyst.
[0048] In some embodiments, the composite catalyst includes organosilane and Karstedt's catalyst, and the ratio of the organosilane to the Karstedt's catalyst is 6:1 to 3:1. The organosilane can be KH570 silane coupling agent or KH550 silane coupling agent.
[0049] Specifically, the composite catalyst is used to connect the polymer obtained in step S3 with PHA by forming a chemical bond to achieve complexation / polymerization of the two; specifically, to form a three-dimensional network structure between molecular chains, improve the stability and performance of the product, and thereby obtain a product with better viscosity performance.
[0050] S5. Hydrolyze to obtain the finished product: Cut the loaded polymer block obtained in S4 into pieces, add caustic soda and mix, and hydrolyze for 2 to 3 hours. Dry and crush the obtained product to obtain high-score and high-viscosity fluorescent polyacrylamide.
[0051] Example 1
[0052] S1. Preparation of fluorescent monomers:
[0053] S101, adding 10.28 g of 4-bromo-1,8-naphthalene dicarboxylic anhydride, 7.52 g of n-propylamine and 150 ml of anhydrous ethanol into a three-necked flask, stirring thoroughly and refluxing at an oil bath temperature of 80° C. for 6 hours, then freezing the product for 5 hours, filtering and washing, and drying the filtrate to obtain a first intermediate product;
[0054] S102, add 7.76g of the first intermediate product, 8.59g of N-methylpiperazine and 100ml of ethylene glycol methyl ether into a three-necked flask, stir well and reflux at an oil bath temperature of 150°C for 12 hours, and after the reaction, distill under reduced pressure to evaporate the solvent, place the product in a refrigerator for 5 hours, filter and wash, and dry the filtrate to obtain a second intermediate product;
[0055] S103. Add 5.84 g of the second intermediate product, 5.26 g of allyl chloride and 100 ml of dimethylformamide into a three-necked flask, stir well and reflux in a water bath at 50°C for 10 hours. After the reaction is completed, evaporate the solvent by vacuum distillation. Add appropriate amount of acetone to the product to dissolve it and freeze it in a refrigerator for 5 hours. After filtering and washing, dry the filtrate to obtain the fluorescent monomer 4-(N'-methyl-1-piperazinyl)-N-propyl-1,8-naphthalene dicarboxylate allyl ammonium chloride.
[0056] S2, preparing polymerization monomer aqueous solution:
[0057] Weigh 45 g of acrylamide, 5 g of acrylic acid, 1.25 g of 4-(N'-methyl-1-piperazinyl)-N-propyl-1,8-naphthalene dicarboxylic acid allyl ammonium chloride, and 1.5 g of 2-acrylamide-2-methylpropane sulfonic acid and dissolve them in 70 g of deionized water. Fully dissolve them to prepare an aqueous solution. Add an appropriate amount of 50% sodium hydroxide solution dropwise to adjust the pH value of the aqueous solution to 7. Subsequently, add 0.2 g of sodium ethylenediaminetetramethylenephosphate and 0.2 g of pentaerythritol. After fully dissolving, obtain an aqueous solution of polymerization monomers.
[0058] S3, polymerization reaction:
[0059] The polymerization monomer aqueous solution was transferred into a reaction container, 4.5 g of isophthaloyl chloride and 0.45 g of N,N-dimethylformamide (DMF) were added, nitrogen was continuously introduced into the reactor for 40 minutes, 0.03 g of azobisisobutyronitrile was added, nitrogen was continued to be introduced for 30 minutes, 0.025 g of ammonium persulfate was added, nitrogen was continued to be introduced for 2 minutes, and then 0.025 g of sodium thiosulfate was added to initiate the polymerization reaction, and a polymer block was obtained after 4 hours.
[0060] S4. Loading compound:
[0061] The polymer gel block obtained in step S3 was stirred at 30° C., and 7 g of poly 3-hydroxyalkanoate (PHA) and 3 g of a composite catalyst were added, wherein the composite catalyst included 2.5 g of KH570 silane coupling agent and 0.5 g of Karstedt's catalyst. The mixture was stirred for 3 h, and nitrogen was continuously introduced into the reactor for 1 h to obtain a loaded polymer gel block.
[0062] S5, hydrolyze to obtain the finished product:
[0063] The loaded polymer block obtained in step S4 is cut into pieces and 15 g of caustic soda is added. After kneading evenly, the mixture is hydrolyzed for 2.5 hours. The mixture is then taken out and placed in a 75°C vacuum drying oven for drying. After drying, the mixture is crushed with a pulverizer and sieved through a 60-mesh sieve to obtain a high-score and high-viscosity fluorescent polyacrylamide product.
[0064] Example 2
[0065] S1. Preparation of fluorescent monomers:
[0066] S101, adding 10.28 g of 4-bromo-1,8-naphthalene dicarboxylic anhydride, 7.52 g of n-propylamine and 150 ml of anhydrous ethanol into a three-necked flask, stirring thoroughly and refluxing at an oil bath temperature of 80° C. for 6 hours, then freezing the product for 5 hours, filtering and washing, and drying the filtrate to obtain a first intermediate product;
[0067] S102, add 7.76g of the first intermediate product, 8.59g of N-methylpiperazine and 100ml of ethylene glycol methyl ether into a three-necked flask, stir well and reflux at an oil bath temperature of 150°C for 12 hours, and after the reaction, distill under reduced pressure to evaporate the solvent, place the product in a refrigerator for 5 hours, filter and wash, and dry the filtrate to obtain a second intermediate product;
[0068] S103. Add 5.84 g of the second intermediate product, 5.26 g of allyl chloride and 100 ml of dimethylformamide into a three-necked flask, stir well and reflux in a water bath at 50°C for 10 hours. After the reaction is completed, evaporate the solvent by vacuum distillation. Add appropriate amount of acetone to the product to dissolve it and freeze it in a refrigerator for 5 hours. After filtering and washing, dry the filtrate to obtain the fluorescent monomer 4-(N'-methyl-1-piperazinyl)-N-propyl-1,8-naphthalene dicarboxylate allyl ammonium chloride.
[0069] S2, preparing polymerization monomer aqueous solution:
[0070] Weigh 45 g of acrylamide, 5 g of acrylic acid, 1.25 g of 4-(N'-methyl-1-piperazinyl)-N-propyl-1,8-naphthalene dicarboxylic acid allyl ammonium chloride, and 1.5 g of 2-acrylamide-2-methylpropane sulfonic acid and dissolve them in 70 g of deionized water. Fully dissolve them to prepare an aqueous solution. Add an appropriate amount of 50% sodium hydroxide solution dropwise to adjust the pH value of the aqueous solution to 7. Subsequently, add 0.2 g of sodium ethylenediaminetetramethylenephosphate and 0.2 g of pentaerythritol. After fully dissolving, obtain an aqueous solution of polymerization monomers.
[0071] S3, polymerization reaction:
[0072] The polymerization monomer aqueous solution was transferred into a reaction container, 4.5 g of isophthaloyl chloride and 0.45 g of triethylamine were added, nitrogen was continuously introduced into the reactor for 40 minutes, 0.03 g of azobisisobutyronitrile was added, nitrogen was continued to be introduced for 30 minutes, 0.025 g of ammonium persulfate was added, nitrogen was continued to be introduced for 2 minutes, and then 0.025 g of sodium thiosulfate was added to initiate the polymerization reaction, and a polymer block was obtained after 4 hours.
[0073] S4. Loading compound:
[0074] The polymer gel block obtained in step S3 was stirred at 30° C., and 7 g of poly 3-hydroxyalkanoate (PHA) and 3 g of a composite catalyst were added, wherein the composite catalyst included 2.5 g of KH570 silane coupling agent and 0.5 g of Karstedt's catalyst. The mixture was stirred for 3 h, and nitrogen was continuously introduced into the reactor for 1 h to obtain a loaded polymer gel block.
[0075] S5, hydrolyze to obtain the finished product:
[0076] The loaded polymer block obtained in step S4 is cut into pieces and 15 g of caustic soda is added. After kneading evenly, the mixture is hydrolyzed for 2.5 hours. The mixture is then taken out and placed in a 75°C vacuum drying oven for drying. After drying, the mixture is crushed with a pulverizer and sieved through a 60-mesh sieve to obtain a high-score and high-viscosity fluorescent polyacrylamide product.
[0077] Example 3
[0078] S1. Preparation of fluorescent monomers:
[0079] S101, adding 10.28 g of 4-bromo-1,8-naphthalene dicarboxylic anhydride, 7.52 g of n-propylamine and 150 ml of anhydrous ethanol into a three-necked flask, stirring thoroughly and refluxing at an oil bath temperature of 80° C. for 6 hours, then freezing the product for 5 hours, filtering and washing, and drying the filtrate to obtain a first intermediate product;
[0080] S102, add 7.76g of the first intermediate product, 8.59g of N-methylpiperazine and 100ml of ethylene glycol methyl ether into a three-necked flask, stir well and reflux at an oil bath temperature of 150°C for 12 hours, and after the reaction, distill under reduced pressure to evaporate the solvent, place the product in a refrigerator for 5 hours, filter and wash, and dry the filtrate to obtain a second intermediate product;
[0081] S103. Add 5.84 g of the second intermediate product, 5.26 g of allyl chloride and 100 ml of dimethylformamide into a three-necked flask, stir well and reflux in a water bath at 50°C for 10 hours. After the reaction is completed, evaporate the solvent by vacuum distillation. Add appropriate amount of acetone to the product to dissolve it and freeze it in a refrigerator for 5 hours. After filtering and washing, dry the filtrate to obtain the fluorescent monomer 4-(N'-methyl-1-piperazinyl)-N-propyl-1,8-naphthalene dicarboxylate allyl ammonium chloride.
[0082] S2, preparing polymerization monomer aqueous solution:
[0083] Weigh 45 g of acrylamide, 5 g of acrylic acid, 1.25 g of 4-(N'-methyl-1-piperazinyl)-N-propyl-1,8-naphthalene dicarboxylic acid allyl ammonium chloride, and 1.5 g of 2-acrylamide-2-methylpropane sulfonic acid and dissolve them in 60 g of deionized water. Fully dissolve them to prepare an aqueous solution. Add an appropriate amount of 50% sodium hydroxide solution dropwise to adjust the pH value of the aqueous solution to 7. Subsequently, add 0.2 g of sodium ethylenediaminetetramethylenephosphate and 0.2 g of pentaerythritol. After fully dissolving, obtain an aqueous solution of polymerization monomers.
[0084] S3, polymerization reaction:
[0085] The polymerization monomer aqueous solution was transferred into a reaction container, 4.5 g of isophthaloyl chloride and 0.45 g of triethylamine were added, nitrogen was continuously introduced into the reactor for 40 minutes, 0.03 g of azobisisobutyronitrile was added, nitrogen was continued to be introduced for 30 minutes, 0.025 g of ammonium persulfate was added, nitrogen was continued to be introduced for 2 minutes, and then 0.025 g of sodium thiosulfate was added to initiate the polymerization reaction, and a polymer block was obtained after 4 hours.
[0086] S4. Loading compound:
[0087] The polymer gel block obtained in step S3 was stirred at 30° C., and 8 g of poly 3-hydroxyalkanoate (PHA) and 2 g of a composite catalyst were added, wherein the composite catalyst included 1.5 g of KH570 silane coupling agent and 0.5 g of Karstedt's catalyst. The mixture was stirred for 3 h, and nitrogen was continuously introduced into the reactor for 1 h to obtain a loaded polymer gel block.
[0088] S5, hydrolyze to obtain the finished product:
[0089] After cutting the polymer block into pieces, add 15g of caustic soda, knead it evenly and then carry out hydrolysis reaction for 2.5 hours. Then take it out and put it into a 75℃ vacuum drying oven for drying. After drying, crush it with a grinder and sieve it with a 60-mesh screen to obtain a high-score and high-viscosity fluorescent polyacrylamide finished product.
[0090] Example 4
[0091] S1. Preparation of fluorescent monomers:
[0092] S101, adding 10.28 g of 4-bromo-1,8-naphthalene dicarboxylic anhydride, 7.52 g of n-propylamine and 150 ml of anhydrous ethanol into a three-necked flask, stirring thoroughly and refluxing at an oil bath temperature of 80° C. for 6 hours, then freezing the product for 5 hours, filtering and washing, and drying the filtrate to obtain a first intermediate product;
[0093] S102, add 7.76g of the first intermediate product, 8.59g of N-methylpiperazine and 100ml of ethylene glycol methyl ether into a three-necked flask, stir well and reflux at an oil bath temperature of 150°C for 12 hours, and after the reaction, distill under reduced pressure to evaporate the solvent, place the product in a refrigerator for 5 hours, filter and wash, and dry the filtrate to obtain a second intermediate product;
[0094] S103. Add 5.84 g of the second intermediate product, 5.26 g of allyl chloride and 100 ml of dimethylformamide into a three-necked flask, stir well and reflux in a water bath at 50°C for 10 hours. After the reaction is completed, evaporate the solvent by vacuum distillation. Add appropriate amount of acetone to the product to dissolve it and freeze it in a refrigerator for 5 hours. After filtering and washing, dry the filtrate to obtain the fluorescent monomer 4-(N'-methyl-1-piperazinyl)-N-propyl-1,8-naphthalene dicarboxylate allyl ammonium chloride.
[0095] S2, preparing polymerization monomer aqueous solution:
[0096] Weigh 20 g of acrylamide, 5 g of acrylic acid, 1.25 g of 4-(N'-methyl-1-piperazinyl)-N-propyl-1,8-naphthalene dicarboxylic acid allyl ammonium chloride, and 1.5 g of 2-acrylamide-2-methylpropane sulfonic acid and dissolve them in 70 g of deionized water. Fully dissolve them to prepare an aqueous solution. Add an appropriate amount of 50% sodium hydroxide solution to adjust the pH value of the aqueous solution to 7. Then add 0.2 g of sodium ethylenediaminetetramethylenephosphate and 0.2 g of pentaerythritol. After fully dissolving, obtain an aqueous solution of polymerization monomers.
[0097] S3, polymerization reaction:
[0098] The polymerization monomer aqueous solution was transferred into a reactor, 4.5 g of isophthaloyl chloride and 0.45 g of triethylamine were added, nitrogen was continuously passed into the reactor for 40 minutes, 0.03 g of azobisisobutyronitrile was added, nitrogen was continued to be passed for 30 minutes, 0.025 g of ammonium persulfate was added, nitrogen was continued to be passed for 2 minutes, and 0.025 g of sodium thiosulfate was added to initiate the polymerization reaction. A polymer block was obtained after 4 hours.
[0099] S4. Loading compound:
[0100] The polymer gel block obtained in step S3 was stirred at 30° C., and 12 g of poly 3-hydroxyalkanoate (PHA) and 3 g of a composite catalyst were added, wherein the composite catalyst included 2.5 g of KH570 silane coupling agent and 0.5 g of Karstedt's catalyst. The mixture was stirred for 3 h, and nitrogen was continuously introduced into the reactor for 1 h to obtain a loaded polymer gel block.
[0101] S5, hydrolyze to obtain the finished product:
[0102] After the reaction is completed, cut the rubber block into pieces and add 16.5g of flake caustic soda. Knead it evenly and then carry out hydrolysis reaction for 2.5 hours. Then take it out and put it into a 75℃ vacuum drying oven for drying. After drying, crush it with a grinder and sieve it with a 60-mesh sieve to obtain a high-score and high-viscosity fluorescent polyacrylamide finished product.
[0103] Example 5
[0104] S1. Preparation of fluorescent monomers:
[0105] S101, adding 10.28 g of 4-bromo-1,8-naphthalene dicarboxylic anhydride, 7.52 g of n-propylamine and 150 ml of anhydrous ethanol into a three-necked flask, stirring thoroughly and refluxing at an oil bath temperature of 80° C. for 6 hours, then freezing the product for 5 hours, filtering and washing, and drying the filtrate to obtain a first intermediate product;
[0106] S102, add 7.76g of the first intermediate product, 8.59g of N-methylpiperazine and 100ml of ethylene glycol methyl ether into a three-necked flask, stir well and reflux at an oil bath temperature of 150°C for 12 hours, and after the reaction, distill under reduced pressure to evaporate the solvent, place the product in a refrigerator for 5 hours, filter and wash, and dry the filtrate to obtain a second intermediate product;
[0107] S103. Add 5.84 g of the second intermediate product, 5.26 g of allyl chloride and 100 ml of dimethylformamide into a three-necked flask, stir well and reflux in a water bath at 50°C for 10 hours. After the reaction is completed, evaporate the solvent by vacuum distillation. Add appropriate amount of acetone to the product to dissolve it and freeze it in a refrigerator for 5 hours. After filtering and washing, dry the filtrate to obtain the fluorescent monomer 4-(N'-methyl-1-piperazinyl)-N-propyl-1,8-naphthalene dicarboxylate allyl ammonium chloride.
[0108] S2, preparing polymerization monomer aqueous solution:
[0109] Weigh 50 g of acrylamide, 5 g of acrylic acid, 1.25 g of 4-(N'-methyl-1-piperazinyl)-N-propyl-1,8-naphthalene dicarboxylic acid allyl ammonium chloride, and 1.25 g of 2-acrylamide-2-methylpropanesulfonic acid and dissolve them in 30 g of deionized water. Fully dissolve them to prepare an aqueous solution. Add an appropriate amount of 50% sodium hydroxide solution to adjust the pH value of the aqueous solution to 7.05, then add 0.215 g of 2,2-bipyridine and 0.215 g of isobutyl alcohol. After fully dissolving, obtain an aqueous solution of polymerization monomers.
[0110] S3, polymerization reaction:
[0111] The polymerization monomer aqueous solution was transferred into a reactor, 4.5 g of isophthaloyl chloride and 0.45 g of triethylamine were added, nitrogen was continuously introduced into the reactor for 40 minutes, 0.025 g of dimethyl azobisisobutyrate was added, nitrogen was continuously introduced for 30 minutes, 0.0315 g of diisopropyl peroxydicarbonate was added, nitrogen was continuously introduced for 2 minutes, 0.0315 g of sodium sulfite was added to initiate the polymerization reaction, and a polymer block was obtained after 4 hours.
[0112] S4. Loading compound:
[0113] The polymer gel block obtained in step S3 was stirred at 30° C., and 7 g of poly 3-hydroxyalkanoate (PHA) and 3 g of a composite catalyst were added, wherein the composite catalyst included 2.5 g of KH570 silane coupling agent and 0.5 g of Karstedt's catalyst. The mixture was stirred for 3 h, and nitrogen was continuously introduced into the reactor for 1 h to obtain a loaded polymer gel block.
[0114] S5, hydrolyze to obtain the finished product:
[0115] After the reaction is completed, cut the rubber block into pieces and add 16.5g of flake caustic soda. Knead it evenly and then carry out hydrolysis reaction for 2.5 hours. Then take it out and put it into a 75℃ vacuum drying oven for drying. After drying, crush it with a grinder and sieve it with a 60-mesh sieve to obtain a high-score and high-viscosity fluorescent polyacrylamide finished product.
[0116] Comparative Example 1
[0117] S1. Preparation of polymerization monomer aqueous solution:
[0118] Weigh 45 g of acrylamide, 5 g of acrylic acid, and 1.5 g of 2-acrylamide-2-methylpropanesulfonic acid and dissolve them in 70 g of deionized water. Fully dissolve them to prepare an aqueous solution. Add an appropriate amount of 50% sodium hydroxide solution and adjust the pH value of the aqueous solution to 7. Then add 0.2 g of sodium ethylenediaminetetramethylenephosphate and 0.2 g of pentaerythritol. After fully dissolving, obtain an aqueous solution of polymerization monomers.
[0119] S2. Polymerization reaction:
[0120] The polymerization monomer aqueous solution was transferred into a reaction container, 4.5 g of isophthaloyl chloride and 0.45 g of triethylamine were added, nitrogen was continuously introduced into the reactor for 40 minutes, 0.03 g of azobisisobutyronitrile was added, nitrogen was continued to be introduced for 30 minutes, 0.025 g of ammonium persulfate was added, nitrogen was continued to be introduced for 2 minutes, and then 0.025 g of sodium thiosulfate was added to initiate the polymerization reaction, and a polymer block was obtained after 4 hours.
[0121] S3, at 30°C, the polymer gel block obtained in step S2 was stirred evenly, and 7g of poly 3-hydroxyalkanoate (PHA) and 3g of a composite catalyst were added, wherein the composite catalyst includes 2.5g of KH570 silane coupling agent and 0.5g of Karstedt's catalyst. The mixture was stirred and mixed for 3h, and nitrogen was continuously introduced into the reactor for 1h to obtain a loaded polymer gel block.
[0122] S4, hydrolysis to obtain the finished product:
[0123] The loaded polymer block obtained in step S3 is cut into pieces and 15 g of caustic soda is added. After kneading evenly, the mixture is hydrolyzed for 2.5 hours. The mixture is then taken out and placed in a 75°C vacuum drying oven for drying. After drying, the mixture is crushed with a pulverizer and sieved through a 60-mesh sieve to obtain a high-score and high-viscosity fluorescent polyacrylamide product.
[0124] Comparative Example 2
[0125] S1. Preparation of fluorescent monomers:
[0126] S101, adding 10.28 g of 4-bromo-1,8-naphthalene dicarboxylic anhydride, 7.52 g of n-propylamine and 150 ml of anhydrous ethanol into a three-necked flask, stirring thoroughly and refluxing at an oil bath temperature of 80° C. for 6 hours, then freezing the product for 5 hours, filtering and washing, and drying the filtrate to obtain a first intermediate product;
[0127] S102, add 7.76g of the first intermediate product, 8.59g of N-methylpiperazine and 100ml of ethylene glycol methyl ether into a three-necked flask, stir well and reflux at an oil bath temperature of 150°C for 12 hours, and after the reaction, distill under reduced pressure to evaporate the solvent, place the product in a refrigerator for 5 hours, filter and wash, and dry the filtrate to obtain a second intermediate product;
[0128] S103. Add 5.84 g of the second intermediate product, 5.26 g of allyl chloride and 100 ml of dimethylformamide into a three-necked flask, stir well and reflux in a water bath at 50°C for 10 hours. After the reaction is completed, evaporate the solvent by vacuum distillation. Add appropriate amount of acetone to the product to dissolve it and freeze it in a refrigerator for 5 hours. After filtering and washing, dry the filtrate to obtain the fluorescent monomer 4-(N'-methyl-1-piperazinyl)-N-propyl-1,8-naphthalene dicarboxylate allyl ammonium chloride.
[0129] S2, preparing polymerization monomer aqueous solution:
[0130] Weigh 45 g of acrylamide, 5 g of acrylic acid, 1.25 g of 4-(N'-methyl-1-piperazinyl)-N-propyl-1,8-naphthalene dicarboxylic acid allyl ammonium chloride, and 1.5 g of 2-acrylamide-2-methylpropane sulfonic acid and dissolve them in 70 g of deionized water. Fully dissolve them to prepare an aqueous solution. Add an appropriate amount of 50% sodium hydroxide solution dropwise to adjust the pH value of the aqueous solution to 7. Subsequently, add 0.2 g of sodium ethylenediaminetetramethylenephosphate and 0.2 g of pentaerythritol. After fully dissolving, obtain an aqueous solution of polymerization monomers.
[0131] S3, polymerization reaction:
[0132] The polymerization monomer aqueous solution was transferred into a reaction container, 4.5 g of isophthaloyl chloride and 0.45 g of triethylamine were added, nitrogen was continuously introduced into the reactor for 40 minutes, 0.03 g of azobisisobutyronitrile was added, nitrogen was continued to be introduced for 30 minutes, 0.025 g of ammonium persulfate was added, nitrogen was continued to be introduced for 2 minutes, and then 0.025 g of sodium thiosulfate was added to initiate the polymerization reaction, and a polymer block was obtained after 4 hours.
[0133] S4, hydrolysis to obtain the finished product:
[0134] The polymer block obtained in step S3 is cut into pieces, 15 g of caustic soda is added, the mixture is kneaded evenly and subjected to hydrolysis reaction for 2.5 hours, and then taken out and placed in a 75° C. vacuum drying oven for drying. After drying, the mixture is crushed with a pulverizer and sieved through a 60-mesh sieve to obtain a high-score and high-viscosity fluorescent polyacrylamide product.
[0135] Comparative Example 3
[0136] S1. Preparation of fluorescent monomer: the same as the preparation method in Example 1.
[0137] S2, preparing polymerization monomer aqueous solution:
[0138] Weigh 45 g of acrylamide, 5 g of acrylic acid, 1.25 g of 4-(N'-methyl-1-piperazinyl)-N-propyl-1,8-naphthalene dicarboxylic acid allyl ammonium chloride, and 1.5 g of 2-acrylamide-2-methylpropane sulfonic acid and dissolve them in 70 g of deionized water. Fully dissolve them to prepare an aqueous solution. Add an appropriate amount of 50% sodium hydroxide solution dropwise to adjust the pH value of the aqueous solution to 7. Subsequently, add 0.2 g of sodium ethylenediaminetetramethylenephosphate and 0.2 g of pentaerythritol. After fully dissolving, obtain an aqueous solution of polymerization monomers.
[0139] S3, polymerization reaction:
[0140] The polymerization monomer aqueous solution was transferred into a reaction container. After nitrogen was continuously introduced into the reactor for 40 minutes, 0.03 g of azobisisobutyronitrile was added, and nitrogen was continued to be introduced for 30 minutes. 0.025 g of ammonium persulfate was added, and nitrogen was continued to be introduced for 2 minutes. After that, 0.025 g of sodium thiosulfate was added to initiate the polymerization reaction. A polymer block was obtained after 4 hours.
[0141] S4. Loading compound:
[0142] The polymer gel block obtained in step S3 was stirred at 30° C., and 7 g of poly 3-hydroxyalkanoate (PHA) and 3 g of a composite catalyst were added, wherein the composite catalyst included 2.5 g of KH570 silane coupling agent and 0.5 g of Karstedt's catalyst. The mixture was stirred for 3 h, and nitrogen was continuously introduced into the reactor for 1 h to obtain a loaded polymer gel block.
[0143] S5, hydrolyze to obtain the finished product:
[0144] The loaded polymer block obtained in step S4 is cut into pieces and 15 g of caustic soda is added. After kneading evenly, the mixture is hydrolyzed for 2.5 hours. The mixture is then taken out and placed in a 75°C vacuum drying oven for drying. After drying, the mixture is crushed with a pulverizer and sieved through a 60-mesh sieve to obtain a high-score and high-viscosity fluorescent polyacrylamide product.
[0145] Comparative Example 4
[0146] S1. Preparation of fluorescent monomer: the same as the preparation method in Example 1.
[0147] S2, preparing polymerization monomer aqueous solution:
[0148] Weigh 45 g of acrylamide, 5 g of acrylic acid, 1.25 g of 4-(N'-methyl-1-piperazinyl)-N-propyl-1,8-naphthalene dicarboxylic acid allyl ammonium chloride, and 1.5 g of 2-acrylamide-2-methylpropane sulfonic acid and dissolve them in 70 g of deionized water. Fully dissolve them to prepare an aqueous solution. Add an appropriate amount of 50% sodium hydroxide solution dropwise to adjust the pH value of the aqueous solution to 7. Subsequently, add 0.2 g of sodium ethylenediaminetetramethylenephosphate and 0.2 g of pentaerythritol. After fully dissolving, obtain an aqueous solution of polymerization monomers.
[0149] S3, polymerization reaction:
[0150] The polymerization monomer aqueous solution was transferred into a reaction container. After nitrogen was continuously introduced into the reactor for 40 minutes, 0.03 g of azobisisobutyronitrile was added, and nitrogen was continued to be introduced for 30 minutes. 0.025 g of ammonium persulfate was added, and nitrogen was continued to be introduced for 2 minutes. After that, 0.025 g of sodium thiosulfate was added to initiate the polymerization reaction. A polymer block was obtained after 4 hours.
[0151] S4, hydrolysis to obtain the finished product:
[0152] The polymer rubber block obtained in step S3 is cut into pieces and 15g of caustic soda is added. After kneading evenly, the mixture is hydrolyzed for 2.5 hours. The mixture is then taken out and placed in a 75°C vacuum drying oven for drying. After drying, the mixture is crushed with a pulverizer and sieved through a 60-mesh sieve to obtain a high-score and high-viscosity fluorescent polyacrylamide product.
[0153] Specifically, the types of reagents added in Examples 1 to 5 and Comparative Examples 1 to 4 are shown in Tables 1 and 2.
[0154] Table 1 Types of reagents added in Examples 1 to 5
[0155]
[0156] Table 2 Types of reagents added in Comparative Examples 1 to 4
[0157]
[0158]
[0159] In Examples 1 to 5 and Comparative Examples 1 to 4, the amounts of poly 3-hydroxyalkanoate (PHA) and composite catalyst added in the loading and composite step are shown in Table 3.
[0160] Table 3 Addition amount of PHA and composite catalyst in Examples 1 to 5 and Comparative Examples 1 to 4
[0161]
[0162]
[0163] The molecular weight and apparent viscosity of the polyacrylamide products prepared in the above Examples 1 to 5 and Comparative Examples 1 to 4 were tested, and the shear resistance, high temperature resistance and salt resistance of the polyacrylamide were also tested.
[0164] 1) Shear resistance test: The polyacrylamide product was prepared into a 2000 mg / L polymer aqueous solution, and its apparent viscosity W1 was measured using a Brookfield viscometer at a temperature of 25°C. Then, the product was sheared at a speed of 1000 r / min for 12 hours, and the apparent viscosity W2 after shearing was measured. The viscosity retention rate was calculated according to the formula 100%×W2 / W1.
[0165] 2) High temperature resistance test: The polyacrylamide finished product was prepared into a 2000 mg / L polymer aqueous solution, and its apparent viscosity W3 was measured with a Brookfield viscometer at a temperature of 25°C. Then, it was heated in a 95°C water bath for 12 hours, and the apparent viscosity W4 after heating was measured. The viscosity retention rate was calculated according to the formula 100%×W4 / W3.
[0166] 3) Salt resistance test: The polyacrylamide product was prepared into a 2000 mg / L polymer aqueous solution, and its apparent viscosity W5 was measured with a Brookfield viscometer at a temperature of 25°C. Then, 1.5 g of anhydrous calcium chloride and 1.0 g of anhydrous magnesium chloride were added to 500 mL of the polymer aqueous solution, and after stirring and dissolving, it was treated in a 5000 mg / L calcium and magnesium solution for 12 hours, and the apparent viscosity W6 after treatment was measured, and the viscosity retention rate was calculated according to the formula 100%×W6 / W5.
[0167] The test results are shown in Table 4:
[0168] Table 4 Properties of polyacrylamide obtained in Examples 1 to 5 and Comparative Examples 1 to 4
[0169]
[0170]
[0171] Compared with Example 2, Comparative Example 1 does not add fluorescent monomers, and its molecular weight is much lower than that of Example 1, and its apparent viscosity is lower; Compared with Example 2, Comparative Example 2 does not perform the loading and compounding step, and the molecular weight of the obtained product is relatively small, and the surface viscosity is larger than that of other embodiments, but the viscosity retention rate after shearing and water bath is not good; Comparative Example 3 does not add isophthaloyl chloride and triethylamine during polymerization, the molecular weight is small, and the viscosity performance is poor.
[0172] For Examples 1 to 5, by changing the type of reagents added during the polymerization reaction, the type of composite initiator system, and the amount of PHA and composite catalyst in the loading and compounding step, anionic polyacrylamide emulsions with different particle sizes and viscosities were obtained. For Examples 2 to 4, by changing the amount of PHA and composite catalyst added in the loading and compounding step, anionic polyacrylamide emulsions with different particle sizes and viscosities were obtained, wherein the anionic polyacrylamide emulsion obtained in Example 2 had a larger molecular weight and excellent viscosity retention.
[0173] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.
Claims
1. A method for preparing high-resolution and high-viscosity fluorescent polyacrylamide, characterized in that: It includes the following steps: S1, preparing fluorescent monomers; S2, prepare a polymerization monomer aqueous solution: according to mass parts, dissolve 1-5 parts of fluorescent monomer, 20-50 parts of acrylamide, 5-10 parts of acrylic acid, 1-5 parts of 2-acrylamide-2-methylpropanesulfonic acid in 30-70 parts of deionized water, add sodium hydroxide solution, adjust the pH to 6.8-7.2, add 0.1-0.5 parts of complexing agent, 0.1-0.5 parts of chain transfer agent, to obtain a polymerization monomer aqueous solution; S3, polymerization reaction: transferring the polymerization monomer aqueous solution to a reactor, adding isophthaloyl chloride accounting for 10% of the mass of the acrylamide, and N,N-dimethylformamide or triethylamine accounting for 1% of the mass of the acrylamide, continuously passing nitrogen into the reactor for 0.5 to 1 hour, adding a composite initiator system, reacting for 4 to 6 hours, and obtaining a polymer block; The composite initiator system comprises: The invention comprises, by weight, 30 to 40 parts of an azo compound, 30 to 50 parts of an oxidant, and 30 to 40 parts of a reducing agent, wherein the oxidant is selected from diisopropyl peroxydicarbonate; S4, loading and compounding: stirring the polymer block at 25-45° C., adding a loading agent accounting for 10-20% of the mass of the polymer block, stirring and mixing for 2-4 hours, and continuously introducing nitrogen into the reactor for 0.5-1 hour to obtain a loaded polymer block, wherein the loading agent includes 70-80% by mass of poly 3-hydroxyalkanoate and 20-30% by mass of a composite catalyst; S5. Hydrolyze to obtain the finished product: Cut the loaded polymer block obtained in S4 into pieces, add caustic soda and mix, and hydrolyze for 2 to 3 hours. Dry and crush the obtained product to obtain high-score and high-viscosity fluorescent polyacrylamide.
2. The method for preparing high-resolution and high-viscosity fluorescent polyacrylamide according to claim 1, characterized in that: The step S1 comprises the following steps: S101, fully stirring 4-bromo-1,8-naphthalene dicarboxylic anhydride, n-propylamine and anhydrous ethanol and refluxing them at an oil bath temperature of 80° C. for 6 hours, freezing the product for 5 hours, filtering and washing, and drying the filtrate to obtain a first intermediate product; S102, the first intermediate product, N-methylpiperazine and ethylene glycol methyl ether are fully stirred and refluxed at an oil bath temperature of 150° C. for 12 hours, and the solvent is evaporated off by reduced pressure distillation after the reaction is completed. The product is placed in a refrigerator for 5 hours, filtered and washed, and the filtrate is dried to obtain a second intermediate product; S103. The second intermediate product, allyl chloride and an appropriate amount of dimethylformamide are fully stirred and refluxed at a water bath temperature of 50°C for 10 hours. After the reaction is completed, the solvent is evaporated off by reduced pressure distillation. An appropriate amount of acetone is added to the product to dissolve it and the product is placed in a refrigerator for 5 hours. After filtration and washing, the filtrate is dried to obtain a fluorescent monomer.
3. The method for preparing the high-resolution and high-viscosity fluorescent polyacrylamide according to claim 2, characterized in that: The mass ratio of the 4-bromo-1,8-naphthalene dicarboxylic anhydride to n-propylamine is 1.5:1 to 2:1; the mass ratio of the first intermediate product to N-methylpiperazine is 1:1 to 1:1.5; and the mass ratio of the second intermediate product to allyl chloride is 1.5:1 to 1:
1.
4. The method for preparing the high-resolution and high-viscosity fluorescent polyacrylamide according to claim 1, characterized in that: The composite catalyst comprises organosilane and Karstedt's catalyst, and the ratio of the organosilane to the Karstedt's catalyst is 6:1 to 3:
1.
5. The method for preparing the high-resolution and high-viscosity fluorescent polyacrylamide according to claim 1, characterized in that: The azo compound is selected from azobisisobutyronitrile or dimethyl azobisisobutyrate, and the added amount of the azo compound is 0.05-0.1% of the mass of the acrylamide.
6. The method for preparing the high-resolution and high-viscosity fluorescent polyacrylamide according to claim 1, characterized in that: The reducing agent is one or more of sodium sulfite, sodium hypophosphite or sodium thiosulfate, and the amount of the reducing agent added is 0.04-0.1% of the mass of acrylamide.
7. The method for preparing high-resolution and high-viscosity fluorescent polyacrylamide according to claim 1, characterized in that: The complexing agent is selected from one or more of 2,2-bipyridine, sodium ethylenediaminetetramethylenephosphate or tris(2-dimethylaminoethyl)amine.
8. The method for preparing high-resolution and high-viscosity fluorescent polyacrylamide according to claim 1, characterized in that: The chain transfer agent is selected from one or more of isopropanol, isobutanol or pentaerythritol.
9. The method for preparing high-resolution and high-viscosity fluorescent polyacrylamide according to claim 1, characterized in that: The nitrogen introduced in step S3 has a purity of ≥99.99% and a flow rate of 60 m 3 / h.
Citation Information
Cited By
Terpolymer compositions, methods for their preparation, and their use for separating minerals
WO2026099320A1